A combined turbulence controller for continuous casting of profiled blanks and a preparation method thereof

By designing a combined special-shaped blank continuous cast tundra turbulence controller, adopting a conical raised structure and a round table cavity, combined with seam optimization, the problem of poor performance of the tundra turbulence controller in the existing technology is solved, and better performance is achieved The liquid steel flow characteristics and lower production costs extend the service life and reduce the oxygen content in the liquid steel.

CN111113637BActive Publication Date: 2024-11-12LAIWU STEEL YINSHAN SECTION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010067179.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-01-20
Publication Date
2024-11-12
Estimated Expiration
2040-01-20

AI Technical Summary

Technical Problem

The existing tundra turbulence controller performs poorly in metallurgical functionalization, longevity and low cost. The inner cavity is cylindrical in shape to suppress the turbulence energy of the ladle flow injection, and the core is made of arc-shaped magnesium carbon brick annular building. Poor construction performance and high production cost.

Method used

Using a combined special-shaped blank continuous casting tundra turbulence controller, the conical convex structure and the round table-shaped inner cavity are designed through the overall design of the upper and lower parts of the sleeve core, combined with the split joints and different materials. Optimize, use isostatic molding and sintered magnesium sand filling, and apply regenerated magnesium carbonaceous material to improve performance.

Benefits of technology

It significantly improves the effect of suppressing the turbulent kinetic energy of steel flow, extends the service life, reduces production costs, improves the flow characteristics and overall performance of the liquid steel in the tundra, solves the problem of flow and slag in the impact area, and the steel in the crystallizer The total oxygen content of liquid is reduced by more than 15%, the service life is increased by more than 4 hours, and the production cost is reduced by more than 16%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111113637B_ABST
    Figure CN111113637B_ABST
Patent Text Reader

Abstract

The invention discloses a combined turbulence controller for a shaped billet continuous casting ladle and a preparation method thereof. The turbulence controller comprises an outer shell, an upper sleeve core, a lower sleeve core and a conical protrusion structure arranged on the bottom surface of the lower sleeve core. The method comprises positioning the components, filling the joint seams, applying a regenerated magnesium carbonaceous coating material and performing natural curing, thereby improving the effect of suppressing the turbulent kinetic energy of the ladle injection turbulence and effectively improving the flow characteristics of the molten steel in the ladle. The combined structural design of the main body outer shell, the upper sleeve core and the lower sleeve core is adopted. The upper sleeve core and the lower sleeve core are designed as a whole, made of different materials and prepared separately. The shape design of the inner cavity of the combined sleeve core is based on the numerical simulation research and application test of the shaped billet continuous casting ladle, and at the same time meets the performance requirements of metallurgical functionalization, long life and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of continuous casting refractory materials, and in particular to a combined special-shaped blank continuous casting tundish turbulence controller and a preparation method thereof. Background Art

[0002] Setting a turbulence controller in the tundish of a continuous casting machine can change the route of molten steel in the tundish, prolong the residence time, and promote the floating and removal of inclusions, which plays an important role in improving the quality of the ingot. At the same time, it can slow down the scouring of the impact zone of the tundish working lining by the ladle injection and increase the continuous casting time of the tundish. In recent years, the production technology of turbulence controllers has developed towards metallurgical functionalization, longevity, and low cost, but the tundish turbulence controllers produced by existing technologies cannot meet the performance requirements of metallurgical functionalization, longevity, and low cost at the same time.

[0003] The patent document with the publication number CN104707956B discloses a turbulence controller for a continuous casting tundish of a special-shaped blank and its installation method, which includes a shell, a bottom plate, a sleeve core and a pressure ring. The shell is a cavity structure with an upper end opening, the bottom plate is located on the bottom of the shell cavity, the bottom end of the sleeve core is located above the bottom plate, the pressure ring is arranged at the upper end of the sleeve core and is located in the shell cavity, and an expansion joint is arranged between the bottom of the shell cavity and the bottom plate, and between the inner wall of the shell and the sleeve core. The invention solves the problem of the upper layer of magnesium carbon bricks falling off the side wall of the sleeve core by arranging a pressure ring above the sleeve core, and improves the quality stability of the turbulence controller. The shortcomings of the invention are: the inner cavity shape is "cylindrical", the effect of suppressing the turbulent kinetic energy of the ladle injection turbulence is poor, which is not conducive to improving the flow characteristics of the molten steel in the tundish, and the sleeve core is built with arc-shaped magnesium carbon bricks in an annular shape, which has poor overall performance and is prone to brick falling, and the production cost is high, which increases the cost of continuous casting refractory materials. Summary of the invention

[0004] In view of the above problems, the present invention provides a combined turbulence controller for a shaped billet continuous casting tundish and a preparation method thereof, which improves the effect of suppressing the turbulent kinetic energy of the ladle injection turbulence and effectively improves the flow characteristics of the molten steel in the tundish. The invention adopts a combined structural design of a main body shell, an upper sleeve core and a lower sleeve core. The upper sleeve core and the lower sleeve core are designed as an integral whole, made of different materials, and prepared separately. The shape design of the inner cavity of the combined sleeve core is based on the numerical simulation research and application test of the shaped billet continuous casting tundish, and at the same time meets the performance requirements of metallurgical functionality, long life and low cost.

[0005] The technical solution of the present invention to solve the technical problem is:

[0006] A combined turbulence controller for a continuous casting tundish of a profiled blank comprises an outer shell and a sleeve core, wherein the sleeve core is arranged in the inner cavity of the outer shell, and the sleeve core comprises an upper sleeve core portion and a lower sleeve core portion which are arranged up and down, and the lower sleeve core portion is arranged on the bottom surface of the inner cavity of the outer shell, and the longitudinal center lines of the upper sleeve core portion and the lower sleeve core portion coincide with the longitudinal center line of the inner cavity of the outer shell, a joint seam is provided between the side walls of the outer shell and the sleeve core, and a plurality of conical protrusion structures are provided at the bottom of the inner cavity of the sleeve core, and the protrusion structures are distributed in an array on a circle with the longitudinal center line of the lower sleeve core portion as the axis. The present invention provides a plurality of conical protrusion structures at the bottom of the inner cavity of the sleeve core, and the protrusion structures are distributed in an array on a circle with the longitudinal center line of the lower part of the sleeve core as the axis. Compared with designing the protrusion structure as a circular, semicircular or truncated cone shape, the conical protrusion structure has a higher height under the condition of the same volume, and has a better effect of suppressing the turbulent kinetic energy of the steel flow. Moreover, through the joint action of multiple protrusion structures distributed in a circular array, the present invention has a better effect of suppressing the turbulent kinetic energy of the steel flow.

[0007] Furthermore, the inner cavity of the upper part of the sleeve core is in the shape of a truncated cone with a small inner diameter at the upper part and a large inner cavity at the lower part, the inner cavity bottom surface of the lower part of the sleeve core is an arc curved surface, and the inner cavity side wall and the bottom surface of the lower part of the sleeve core are transitioned by an arc chamfer. The upper part of the sleeve core is designed to have a small upper opening and a large inner diameter at the lower part, thereby solving the problem of molten steel splashing.

[0008] Furthermore, the outer shape of the upper part of the sleeve core is a truncated cone with a large upper bottom surface and a small lower bottom surface, and the outer shape of the lower part of the sleeve core is a truncated cone with a large upper bottom surface and a small lower bottom surface. According to this design, the side wall of the sleeve core is a structure with a thick upper end and a thin lower end. Since the steel flow scours the upper part more heavily than the lower part during the pouring process, this design overcomes the technical problem that the erosion rate of the upper part is greater than that of the lower part, and prolongs the service life of the turbulence controller.

[0009] Furthermore, the width of the joint is larger at the top and smaller at the bottom. The upper width m is 10-15 mm, and the lower width n is 5-10 mm. By designing the joint to be wider at the top and narrower at the bottom, the density of the filler at the bottom of the joint can be naturally increased, effectively preventing the problem of steel penetration from top to bottom of the joint.

[0010] Furthermore, the number of the protruding structures is four.

[0011] Further, the height a of the upper part of the core is 258-288 mm, the outer diameter D1 of the upper bottom surface of the upper part of the core is 650-700 mm, the inner diameter d1 of the upper bottom surface of the upper part of the core is 350-400 mm, the outer diameter D2 of the lower bottom surface of the upper part of the core is 550-600 mm, the inner diameter d2 of the lower bottom surface of the upper part of the core is 420-470 mm, the height b of the lower part of the core is 172-202 mm, the outer diameter D2 of the upper bottom surface of the lower part of the core is 550-600 mm, the outer diameter D3 of the lower bottom surface of the lower part of the core is 475-525 mm, the arc chamfer radius R of the lower part of the core is 82-102 mm, the thickness c of the bottom of the lower part of the core is 90-100 mm, the inner diameter of the upper bottom surface of the lower part of the core is the same as the inner diameter of the lower bottom surface of the upper part of the core, and the outer diameter of the upper bottom surface of the lower part of the core is the same as the outer diameter of the lower bottom surface of the upper part of the core.

[0012] Furthermore, the protruding structures are evenly distributed on a circle with a diameter of ¢130-150 mm on the bottom surface of the inner cavity, and the bottom circle diameter d of the conical protruding structures is 70-80 mm, and the height h is 70-80 mm.

[0013] A method for preparing a combined profiled blank continuous casting tundish turbulence controller comprises the following steps:

[0014] S1: From bottom to top, sequentially place the lower part of the core sleeve and the upper part of the core sleeve in the housing of the turbulence controller, ensuring that the longitudinal center lines of the lower part of the core sleeve and the upper part of the core sleeve coincide with the longitudinal center line of the inner cavity of the housing;

[0015] S2: The joint between the shell and the core is filled with sintered magnesia with a particle size of ≤1mm;

[0016] S3: Apply a layer of recycled magnesium carbon coating material with a thickness of 25 to 35 mm on the outer surface of the sintered magnesia sand filled in the joint, that is, the upper surface of the sintered magnesia sand; the coating material is used to prevent the sintered magnesia sand in the joint from falling off and the resulting loosening of the sleeve core and other quality problems;

[0017] S4: After natural curing for 1 to 2 days, the preparation of the turbulence controller for the combined profiled blank continuous casting tundish is completed;

[0018] The shape and size of the shell are designed according to the shape and size of the impact zone of the working lining of the tundish for continuous casting of special-shaped blanks, and are cast by using magnesium castables produced by existing technology, and are prepared by natural curing and baking in a heating furnace.

[0019] The magnesium castable is produced by existing technology, with MgO content ≥ 80wt%, and volume density ≥ 2.8g / cm 3 , flexural strength (1500℃)≥12Mpa.

[0020] Furthermore, the upper part of the core sleeve is prepared by isostatic pressing. Isostatic pressing uses the incompressible property of the liquid medium and the property of uniformly transmitting pressure to uniformly pressurize the sample from all directions. The pressure on the powder in all directions is uniform and consistent, so the powder molding is denser and more uniform. The isostatic pressing method includes the following steps:

[0021] 1) Ingredients:

[0022] Preparation of sintered magnesia fine powder: The recycled granular material of waste magnesia carbon brick with a particle size of 0.074mm < 1mm is hydrated and ground into sintered magnesia fine powder with a particle size of ≤0.074 by a ball mill. During the high-temperature use of magnesia carbon bricks, the metal aluminum powder in the magnesia carbon bricks will undergo an oxidation-reduction reaction with carbon to generate Al4C3. The Al4C3 in the used waste magnesia carbon bricks is easy to react with water: Al4C3+12H2O=4Al(OH)3+3CH4↑. The solid volume generated by this reaction alone increases by 1.65 times, which will cause the pulverization and cracking of the waste magnesia carbon bricks. After further research and analysis, we found that Al4C3 mainly exists in granular materials with a particle size of 0.074mm < 1mm. To this end, the present invention sprays hydration and natural drying treatment on the recycled granular materials of waste magnesia carbon bricks with a particle size of 0.074mm<particle size<1mm, grinds them into materials with a particle size of ≤0.074 using a ball mill, and uses sintered magnesia sand particles for the materials with a particle size of 0.074mm<particle size<1mm in the above material composition.

[0023] The materials are weighed according to the proportion, with waste magnesia carbon brick recycled particles as the main raw material, and composed of the following materials by weight percentage: 20-24% of waste magnesia carbon brick recycled particles with a particle size of 3mm≦<5mm, 28-32% of waste magnesia carbon brick recycled particles with a particle size of 1mm≦<3mm, 10-14% of waste magnesia carbon brick recycled fine powder with a particle size of ≦0.074mm, 10-15% of sintered magnesia sand with a particle size of 0.074mm<<1mm, 5-9% of sintered magnesia sand with a particle size of ≦0.074mm, 7-10% of flake graphite, 4-5% of antioxidant, and 3.5-4.5% of phenolic resin.

[0024] The antioxidant is selected from the group consisting of aluminum powder, silicon powder, and silicon carbide powder, or a mixture of the two or more of the two.

[0025] The sintered magnesia is produced by using light-burned magnesia with a MgO content of 95wt% as raw material through processes such as ball pressing and high-temperature vertical kiln calcination, and the MgO content percentage is 94-95wt%.

[0026] The flake graphite has a purity C content of ≥98wt% and a particle size of 100 meshes.

[0027] The aluminum powder has a purity AI content of ≥99wt% and a particle size of 100 meshes.

[0028] The silicon powder has a purity Si content of ≥97wt% and a particle size of 100 meshes.

[0029] The silicon carbide powder has a purity SiC content of ≥94wt% and a particle size of 100 meshes.

[0030] The phenolic resin has a solid content of ≥72wt%, a residual carbon content of ≥42wt%, and a moisture content of ≤5wt%.

[0031] The recycled granular material of waste magnesia carbon bricks refers to granular materials with four particle sizes of 3mm≦<5mm, 1mm≦<3mm, 0.074mm<<1mm and <0.074mm obtained after the waste magnesia carbon bricks are processed and graded by removing the slag layer, sorting, magnetic separation, crushing, wheel rolling and the like.

[0032] In order to solve the problem that the recycled granular materials of waste magnesium carbon bricks contain flake graphite and are easily oxidized, the material composition of the sleeve core of the present invention, which uses the recycled granular materials of waste magnesium carbon bricks as the main raw material, appropriately reduces the weight percentage of flake graphite and increases the weight percentage of antioxidants, thereby solving the problem of reduced oxidation resistance and corrosion resistance of recycled magnesium carbon bricks developed with recycled granular materials of waste magnesium carbon bricks as the main raw material in the prior art.

[0033] 2) Mixing:

[0034] Preheat the mixer to 40-50°C.

[0035] When the mixer is running at low speed, add sintered magnesia with a particle size of 3mm≦<5mm, 1mm≦≤3mm and 0.074mm<<1mm.

[0036] After dry mixing for 1 to 2 minutes, add phenolic resin.

[0037] After 2-3 minutes of wet mixing, add flake graphite.

[0038] After 2-3 minutes of wet mixing, add antioxidant and sintered magnesia fine powder with a particle size of ≤0.074mm.

[0039] Wet mix for 2 to 3 minutes, high speed mix for 10 to 15 minutes,

[0040] Discharging;

[0041] The temperature of the clay during mixing is less than 70°C;

[0042] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 200-250MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;

[0043] 4) After the green body is stored at room temperature for 4 to 8 hours, it is put into the kiln for baking:

[0044] The temperature is raised evenly and continuously from room temperature to 80±10℃, and the heating and heat preservation time are 8 to 16 hours respectively.

[0045] Raise the temperature evenly and continuously from 80±10℃ to 150±10℃, and keep warm for 4 to 8 hours respectively.

[0046] Raise the temperature evenly and continuously from 150±10℃ to 200±10℃, with each heating and heat preservation taking 8 to 16 hours.

[0047] Stop the fire, cool naturally and then take out of the kiln. The preparation of the upper part of the core sleeve is completed and its compressive strength is ≥40MPa.

[0048] Furthermore, the lower part of the sleeve core is prepared by isostatic pressing. Isostatic pressing uses the incompressible property of the liquid medium and the property of uniformly transmitting pressure to uniformly pressurize the sample from all directions. The pressure on the powder in all directions is uniform and consistent, so the powder molding is denser and more uniform. The isostatic pressing method includes the following steps:

[0049] 1) Ingredients: The recycled granular materials of waste magnesia carbon bricks with a particle size of 0.074 mm < 1 mm are sprayed for hydration and naturally dried, and then ground into sintered magnesia fine powder with a particle size of ≤0.074 by a ball mill. The materials are weighed according to the proportion. The main ingredient is 76-84wt% of sintered magnesia mixed with 1mm ≤ particle size ≤3mm, 0.074mm < particle size <1mm, and particle size ≤0.074mm.

[0050] Auxiliary materials: flake graphite 11.5~16wt%

[0051] Antioxidant: 2-5wt% of one or a mixture of aluminum powder, silicon powder, silicon carbide powder

[0052] Binder: 3.5-4.0wt% phenolic resin.

[0053] 2) Mixing: Preheat the mixer to 40-50°C.

[0054] When the mixer is running at low speed, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.074mm<particle size<1mm.

[0055] After dry mixing for 1 to 2 minutes, add phenolic resin.

[0056] After 2-3 minutes of wet mixing, add flake graphite.

[0057] After 2-3 minutes of wet mixing, add antioxidant and sintered magnesia with a particle size of ≤0.074mm.

[0058] Wet mix for 2 to 3 minutes, high speed mix for 10 to 15 minutes,

[0059] Discharging;

[0060] The temperature of the clay during mixing is less than 70°C;

[0061] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 200-250MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;

[0062] 4) Natural drying and baking:

[0063] After the green body is naturally dried for 8 to 16 hours, it is put into the kiln for baking.

[0064] Raise the temperature from room temperature to 140-160°C at a rate of 10°C / h and keep warm for 4-8 hours;

[0065] Then, the temperature is raised to 200-220°C at a rate of 10°C / h and kept at this temperature for 16-24 hours;

[0066] Stop the fire, cool naturally to room temperature and then take out of the kiln. The lower part of the core sleeve is ready and its compressive strength is ≥40MPa.

[0067] The regenerated magnesium carbon coating material of the present invention refers to a coating material prepared by treating and processing waste magnesium carbon bricks with a particle size of 1mm≦≤3mm and a particle size of 0.074mm<<1mm and sintered magnesium sand fine powder with a particle size of ≤0.074mm, soft clay, silicon powder, sodium tripolyphosphate, etc. according to a certain ratio, wherein the weight percentage of the regenerated magnesium carbon particle material is 60-70%, the MgO content is ≥65wt%, and the volume density is ≥1.87g / cm 3 .

[0068] The effects provided in the content of the invention are only the effects of the embodiments, not all the effects of the invention. One of the above technical solutions has the following advantages or beneficial effects:

[0069] 1. The upper and lower parts of the sleeve core of the combined special-shaped blank continuous casting tundish turbulence controller of the present invention are integrally designed and separately formed. The inner cavity of the upper part of the sleeve core is in the shape of a truncated cone with a small upper bottom surface and a large lower bottom surface. The upper bottom surface circle diameter d1 of the outer truncated cone is 350-400 mm, and the lower bottom surface circle diameter d2 of the outer truncated cone is 420-470 mm; the inner cavity bottom of the lower part of the sleeve core is an arc surface, and the arc radius R of the circumference is 82-102 mm. Four conical protrusion structures are evenly distributed on the circumference of a circle with a plane diameter of ¢130-150 mm at the inner cavity bottom, and the bottom surface circle diameter d is 70-80 mm, and the height h is 70-80 mm. The design is a research object of the technicians in this field. The results of numerical simulation research and application test verification show that the above design has a direct impact on the flow state of the molten steel in the tundish. The bottom of the inner cavity of the sleeve core of the turbulence controller of the profiled blank continuous casting tundish designed by the present invention is an arc curved surface, a conical convex structure and a truncated cone curved surface structure of the inner cavity side wall are provided, so that the large ladle injection flow is splashed in different directions in the sleeve core inner cavity of the turbulence controller, collides with each other, dissipates most of the kinetic energy, weakens the degree of turbulence formed by the molten steel, and suppresses the liquid level fluctuation caused by strong turbulence and the slag roll caused by the liquid surface vortex. The numerical simulation calculation results show that the turbulent kinetic energy of the steel flow in the center section of the tundish of the profiled blank continuous casting tundish stabilizer with a straight inner cavity described in the present invention and CN104707956B is 1.46m 2 s 2 , 1.87m 2 s 2 , which is a year-on-year decrease of 21.9%. By applying the present invention, the total oxygen content in the molten steel in the crystallizer is reduced by more than 15% year-on-year, and the problem of slag entrapment in the impact zone is effectively solved.

[0070] 2. The core sleeve of the present invention adopts the material composition of waste magnesium carbon brick recycled granular material as the main raw material, which is obtained through a large number of research experiments and performance test verification, and has achieved beneficial effects: under the premise of ensuring that the performance is not reduced, the amount of magnesium sand replaced by waste magnesium carbon brick recycled granular material reaches 60-66%, making the raw material cost of the production of the turbulence controller of the special-shaped billet continuous casting ladle of the present invention lower by more than 50% year-on-year than the special-shaped billet continuous casting ladle stabilizer described in CN104707956B. The upper part of the sleeve core of the combined special-shaped blank continuous casting tundish turbulence controller of the present invention is composed of materials with waste magnesium carbon brick recycled granular materials as the main raw material. The amount of magnesium sand replaced by waste magnesium carbon brick recycled granular materials reaches 60-66%. It is prepared by isostatic pressing method, and has achieved beneficial effects: high molding quality, good overall performance, and low production cost. It effectively solves the problems of poor overall performance, high production cost, and service life not being synchronized with the service life of the tundish working lining in the sleeve core of the special-shaped blank continuous casting tundish described in CN104707956B, which adopts arc-shaped magnesium carbon brick annular masonry. The service life is increased from 31-35 hours to 35-38 hours year-on-year, and the production cost is reduced by more than 16% year-on-year.

[0071] 3. The lower part of the sleeve core of the combined special-shaped billet continuous casting ladle turbulence controller of the present invention is prepared by isostatic pressing method with sintered magnesia as the main raw material, which improves the molding quality and overall performance of the arc surface and conical protrusion structure of the inner cavity bottom of the lower part of the sleeve core, and meets the requirements of metallurgical functionalization and longevity. BRIEF DESCRIPTION OF THE DRAWINGS

[0072] Figure 1 This is a front view of the structure of the combined slab continuous casting tundish turbulence controller of the present invention;

[0073] Figure 2 It is a top view of the sleeve-core structure of the combined slab continuous casting tundish of the present invention;

[0074] In the figure, there is a shell 1, an upper part of the core 2, a lower part of the core 3, a joint seam 4, and a protruding structure 5. DETAILED DESCRIPTION

[0075] In order to clearly illustrate the technical features of the present solution, the present invention is described in detail below through specific implementation methods and in conjunction with the accompanying drawings. The disclosure below provides many different embodiments or examples for realizing different structures of the present invention. In order to simplify the disclosure of the present invention, the components and settings of specific examples are described below. In addition, the present invention may repeat reference numbers and / or letters in different examples. This repetition is for the purpose of simplification and clarity, and does not itself indicate the relationship between the various embodiments and / or settings discussed. It should be noted that the components illustrated in the accompanying drawings are not necessarily drawn to scale. The present invention omits the description of known components and processing techniques and processes to avoid unnecessary limitations on the present invention.

[0076] Waste magnesium carbon bricks, the waste magnesium carbon bricks mentioned in the present invention, refer to waste magnesium carbon bricks used for the working lining of refining ladles, steelmaking converters and electric furnaces, with a MgO content of ≥76wt%.

[0077] Isostatic pressing is a molding method that subjects the clay to equal liquid static pressure in all directions. Liquid is used as the pressure transmission medium. The clay is loaded into an elastic mold and pressed into shape in a high-pressure cylinder. The isostatic press consists of a high-pressure container and a high-pressure oil pump. The high-pressure container is made of high-grade alloy steel and has a certain thickness to withstand huge pressure. The size of the container is selected according to the size of the molded product. The liquid medium in the high-pressure container can be oil, water or glycerin, etc. Brake oil or anhydrous glycerin is generally used. The compressibility of these two liquids is very small, and almost all the pressure can be transmitted to the elastic mold.

[0078] The following examples further illustrate the invention, but the invention is not limited thereto. The magnesium castable and recycled magnesium carbonaceous coating used in the examples are produced using existing technology, and the waste magnesium carbon brick recycled granular material used refers to waste magnesium carbon bricks that have been processed and graded after removing the slag layer, sorting, magnetic separation, crushing, wheel rolling, etc. to obtain granular materials with four particle sizes of 3mm≦particle size<5mm, 1mm≦particle size<3mm, 0.074mm<particle size<1mm and particle size≤0.074mm. The recycled granular materials of waste magnesium carbon bricks with a particle size of 0.074mm<particle size<1mm are then sprayed for hydration and naturally dried, and ground into recycled fine powder of waste magnesium carbon bricks with a particle size of ≤0.074 using a ball mill. Other raw materials are commercially available products:

[0079] The sintered magnesia is produced by using light-burned magnesia with a MgO content of 95wt% as raw material through processes such as ball pressing and high-temperature vertical kiln calcination, and the MgO content percentage is 94-95wt%.

[0080] The flake graphite has a purity C content of ≥98wt% and a particle size of 100 meshes.

[0081] The aluminum powder has a purity AI content of ≥99wt% and a particle size of 100 meshes.

[0082] The silicon powder has a purity Si content of ≥97wt% and a particle size of 100 meshes.

[0083] The silicon carbide powder has a purity SiC content of ≥94wt% and a particle size of 100 meshes.

[0084] The phenolic resin has a solid content of ≥72wt%, a residual carbon content of ≥42wt%, and a moisture content of ≤5wt%.

[0085] Embodiment 1:

[0086] like Figure 1 , Figure 2As shown, a combined turbulence controller for a continuous casting tundish of a special-shaped billet is composed of an outer shell 1, an upper core part 2, and a lower core part 3. The upper core part 2 and the lower core part 3 are designed as a whole and formed separately, and are positioned on the bottom surface of the inner cavity of the outer shell 1 from top to bottom, and the longitudinal center lines of the upper core part 2 and the lower core part 3 coincide with the longitudinal center line of the inner cavity of the outer shell 1. A joint seam 4 is provided between the outer shell 1 and the upper core part 2 and the lower core part 3. The shape of the inner cavity formed by the combination of the upper core part 2 and the lower core part 3 is designed based on numerical simulation research and application test verification. Four conical protrusion structures 5 are provided at the bottom of the inner cavity of the lower core part 3. The upper core part 2 is prepared by isostatic pressing using recycled granular waste magnesium-carbon bricks as the main raw material, and the lower core part 3 is a magnesium-carbon preform prepared by isostatic pressing.

[0087] The outer shape of the core upper part 2 of the turbulence controller is a truncated cone with a large upper bottom surface and a small lower bottom surface, the height a of the outer truncated cone is 288 mm, the circular diameter D1 of the upper bottom surface of the outer truncated cone is 700 mm, and the diameter D2 of the lower bottom surface of the outer truncated cone is 600 mm. The inner cavity of the core upper part 2 is a truncated cone with a small upper bottom surface and a large lower bottom surface, the circular diameter d1 of the upper bottom surface of the inner truncated cone is 400 mm, and the circular diameter d2 of the lower bottom surface of the inner truncated cone is 470 mm.

[0088] The outer shape of the lower part 3 of the core of the turbulence controller is a truncated cone with a large upper bottom surface and a small lower bottom surface, and the height b of the truncated cone is 202mm, the upper bottom surface circle diameter D2 of the outer truncated cone is 600mm, and the lower bottom surface circle diameter D3 of the outer truncated cone is 525mm. The inner cavity bottom of the lower part 3 of the core is a circular arc surface, and the arc radius R of the circumference is 102mm. Four convex structures 5 are evenly distributed on the circumference of the circle with a plane diameter of ¢150mm at the inner cavity bottom, and the thickness c of the circular plane part is 100mm. The bottom surface circle diameter d of the conical convex structure is 80mm, and the height h is 80mm.

[0089] The width of the joint seam 4 is larger at the top and smaller at the bottom, with the upper width m being 15 mm and the lower width n being 10 mm.

[0090] The shape and size of the shell 1 are designed according to the shape and size of the impact zone of the working lining of the tundish for continuous casting of special-shaped blanks, and are cast by using magnesium spinel castable produced by existing technology, and are prepared by natural curing and baking in a heating furnace.

[0091] The upper part 2 of the sleeve core is prepared by isostatic pressing, with waste magnesium carbon brick recycled granular material as the main raw material, and is composed of the following materials by weight percentage: 24% of waste magnesium carbon brick recycled granular material with a particle size of 3mm≦<5mm, 32% of waste magnesium carbon brick recycled granular material with a particle size of 1mm≦<3mm, 10% of waste magnesium carbon brick recycled fine powder with a particle size of ≦0.074mm, 15% of sintered magnesia sand with a particle size of 0.074mm<<1mm, 5% of sintered magnesia sand with a particle size of ≦0.074mm, 7% of flake graphite, 4% of aluminum powder, and 4% of phenolic resin.

[0092] The core upper part 2 is prepared by isostatic pressing, which includes the following steps:

[0093] 1) Ingredients: weigh the above raw materials according to the above ratio;

[0094] 2) Mixing: preheat the mixer to 40°C, add 3mm≦particle size<5mm, 1mm≦particle size≤3mm and 0.074mm<particle size<1mm sintered magnesia at low speed, add phenolic resin after dry mixing for 1 minute, add flake graphite after wet mixing for 3 minutes, add fine powder with particle size ≤0.074mm and antioxidant after wet mixing for 2 minutes, wet mix for 3 minutes, mix at high speed for 10 minutes, and discharge. The temperature of the mud during mixing is less than 70°C;

[0095] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 200MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;

[0096] 4) The green body is placed in a kiln for baking after being stored at room temperature for 4 hours: ① the temperature is raised uniformly and continuously from room temperature to 70°C, and kept warm for 16 hours after 8 hours of heating; ② the temperature is raised uniformly and continuously from 70°C to 140°C, and kept warm for 8 hours after 4 hours of heating; ② the temperature is raised uniformly and continuously from 140°C to 190°C, and kept warm for 16 hours after 8 hours of heating. After natural cooling, the green body is taken out of the kiln. The preparation of the core sleeve 2 is completed, and its compressive strength is ≥40MPa.

[0097] The core lower part 3 is prepared by isostatic pressing and is made of the following raw materials in percentage by weight:

[0098] Main material: 84wt% sintered magnesia mixed with 1mm≦particle size≤3mm, 0.074mm<particle size<1mm, and particle size≦0.074mm

[0099] Auxiliary materials: flake graphite 10.5wt%

[0100] Antioxidant: Aluminum powder 2.0wt%

[0101] Binder: 3.5wt% phenolic resin.

[0102] The core lower part 3 is prepared by isostatic pressing, which includes the following steps:

[0103] 1) Ingredients: weigh the above raw materials according to the above ratio;

[0104] 2) Mixing: preheat the mixer to 40°C, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.074mm<particle size<1mm at low speed, add phenolic resin after dry mixing for 1 minute, add flake graphite after wet mixing for 3 minutes, add sintered magnesia with a particle size of ≤0.074mm and antioxidant after wet mixing for 2 minutes, wet mix for 3 minutes, mix at high speed for 10 minutes, and discharge. During the mixing process, the temperature of the mud material is less than 70°C;

[0105] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 200MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;

[0106] 4) Natural drying and baking: After the green body is naturally dried for 8 hours, it is put into the kiln for baking: ① heat up from room temperature to 140℃ at a heating rate of 10℃ / h and keep warm for 4 hours; ② heat up from 10℃ / h to 200℃ and keep warm for 16 hours; ③ stop the fire, cool naturally to room temperature and then take out of the kiln. The preparation of the lower part 3 of the core sleeve is completed, and its compressive strength is ≥40MPa.

[0107] A preparation method for a combined special-shaped blank continuous casting tundish turbulence controller comprises the following steps: sequentially inserting a sleeve core lower part 3 and a sleeve core upper part 2 into a shell 1 of the turbulence controller from bottom to top, ensuring that the longitudinal center lines of the sleeve core lower part 3 and the sleeve core upper part 2 coincide with the longitudinal center line of the inner cavity of the shell 1, filling a joint seam 4 between the shell 1 and the sleeve core lower part 3 and the sleeve core upper part 2 with sintered magnesia sand with a particle size of ≤1 mm, and applying a layer of recycled magnesia carbonaceous coating material with a thickness of 35 mm on the outer surface thereof, and naturally curing for 2 days, thereby completing the preparation of the combined special-shaped blank continuous casting tundish turbulence controller.

[0108] Embodiment 2:

[0109] As described in Example 1, except that:

[0110] The height a of the truncated cone of the upper core part 2 of the turbulence controller is 258 mm, the upper bottom circular diameter D1 of the outer truncated cone is 650 mm, the lower bottom circular diameter D2 of the outer truncated cone is 550 mm, the upper bottom circular diameter d1 of the inner truncated cone in the inner cavity of the upper core part 2 is 350 mm, and the lower bottom circular diameter d2 of the inner truncated cone is 420 mm.

[0111] The outer cone height b of the lower core part 3 of the turbulence controller is 172mm, the upper bottom diameter D2 of the outer cone is 550mm, the lower bottom diameter D3 of the outer cone is 475mm, the arc radius R of the inner cavity bottom circumference of the lower core part 3 is 82mm, four protrusion structures 5 are evenly distributed on the circumference of the inner cavity bottom circular plane diameter ¢ of 130mm, and the thickness c of the circular plane part is 90mm. The bottom circle diameter d of the conical protrusion structure is 70mm, and the height h is 70mm.

[0112] The upper width m of the joint seam 4 is 10 mm, and the lower width n is 5 mm.

[0113] The upper part 2 of the sleeve core is prepared by isostatic pressing, with waste magnesium carbon brick recycled granular material as the main raw material, and is composed of the following materials by weight percentage: 20% of waste magnesium carbon brick recycled granular material with a particle size of 3mm≦<5mm, 28% of waste magnesium carbon brick recycled granular material with a particle size of 1mm≦<3mm, 12% of waste magnesium carbon brick recycled fine powder with a particle size of ≦0.074mm, 12% of sintered magnesia sand with a particle size of 0.074mm<<1mm, 9% of sintered magnesia sand with a particle size of ≦0.074mm, 10% of flake graphite, 4.5% of silicon powder, and 4.5% of phenolic resin.

[0114] The core upper part 2 is prepared by isostatic pressing, which includes the following steps:

[0115] 1) Ingredients: weigh the above raw materials according to the above ratio;

[0116] 2) Mixing: preheat the mixer to 50°C, add 3mm≦particle size<5mm, 1mm≦particle size≤3mm and 0.074mm<particle size<1mm sintered magnesia at low speed, add phenolic resin after dry mixing for 2 minutes, add flake graphite after wet mixing for 2 minutes, add fine powder with particle size ≤0.074mm and antioxidant after wet mixing for 3 minutes, wet mix for 2 minutes, mix at high speed for 15 minutes, and discharge. The temperature of the mud during mixing is less than 70°C;

[0117] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 250MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;

[0118] 4) The green body is placed in a kiln for baking after being stored at room temperature for 8 hours: ① the temperature is uniformly and continuously raised from room temperature to 90°C, and kept warm for 8 hours after 16 hours; ② the temperature is uniformly and continuously raised from 90°C to 160°C, and kept warm for 4 hours after 8 hours; ② the temperature is uniformly and continuously raised from 160°C to 210°C, and kept warm for 8 hours after 16 hours. After natural cooling, the green body is taken out of the kiln. The preparation of the core sleeve 2 is completed, and its compressive strength is ≥40MPa.

[0119] 4) Natural drying and baking: After the green body is naturally dried for 16 hours, it is put into the kiln for baking: ① heat up from room temperature to 160℃ at a heating rate of 10℃ / h and keep warm for 4 hours; ② heat up from room temperature to 220℃ at a heating rate of 10℃ / h and keep warm for 16 hours; ③ stop the fire, cool naturally to room temperature and then take out of the kiln. The preparation of the lower part 3 of the core sleeve is completed, and its compressive strength is ≥40MPa.

[0120] The core lower part 3 is prepared by isostatic pressing and is made of the following raw materials in percentage by weight:

[0121] Main material: 76wt% sintered magnesia mixed with 1mm≦particle size≤3mm, 0.074mm<particle size<1mm, and particle size≦0.074mm

[0122] Auxiliary materials: flake graphite 16wt%

[0123] Antioxidant: Silicon powder 2wt%, Silicon carbide powder 2wt%

[0124] Binder: 4.0wt% phenolic resin.

[0125] The core lower part 3 is prepared by isostatic pressing, which includes the following steps:

[0126] 1) Ingredients: weigh the above raw materials according to the above ratio;

[0127] 2) Mixing: preheat the mixer to 50°C, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.074mm<particle size<1mm at low speed, add phenolic resin after dry mixing for 2 minutes, add flake graphite after wet mixing for 2 minutes, add sintered magnesia with a particle size of ≤0.074mm and antioxidant after wet mixing for 3 minutes, wet mix for 2 minutes, mix at high speed for 15 minutes, and discharge. During the mixing process, the temperature of the mud is less than 70°C;

[0128] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 250MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;

[0129] 4) Natural drying and baking: After the green body is naturally dried for 16 hours, it is put into the kiln for baking: ① heat up from room temperature to 160℃ at a heating rate of 10℃ / h and keep warm for 8 hours; ② heat up from 10℃ / h to 220℃ and keep warm for 24 hours; ③ stop the fire, cool naturally to room temperature and then take out of the kiln. The preparation of the lower part 3 of the core sleeve is completed, and its compressive strength is ≥40MPa.

[0130] A preparation method for a combined special-shaped blank continuous casting tundish turbulence controller comprises the following steps: sequentially inserting a sleeve core lower part 3 and a sleeve core upper part 2 into a shell 1 of the turbulence controller from bottom to top, ensuring that the longitudinal center lines of the sleeve core lower part 3 and the sleeve core upper part 2 coincide with the longitudinal center line of the inner cavity of the shell 1, filling a joint seam 4 between the shell 1 and the sleeve core lower part 3 and the sleeve core upper part 2 with sintered magnesia sand with a particle size of ≤1 mm, and applying a layer of recycled magnesia carbonaceous coating material with a thickness of 25 mm on the outer surface thereof, and naturally curing for 1 day, thereby completing the preparation of the combined special-shaped blank continuous casting tundish turbulence controller.

[0131] Embodiment 3:

[0132] As described in Example 1, except that:

[0133] The height a of the outer cone of the upper core part 2 of the turbulence controller is 270 mm, the upper bottom circular diameter D1 of the outer cone is 670 mm, the lower bottom circular diameter D2 of the outer cone is 570 mm, the upper bottom circular diameter d1 of the inner cone of the inner cavity of the upper core part 2 is 370 mm, and the lower bottom circular diameter d2 of the inner cone is 450 mm.

[0134] The height b of the truncated cone of the core lower part 3 of the turbulence controller is 192 mm, the upper bottom diameter D2 of the outer truncated cone is 570 mm, the lower bottom diameter D3 of the outer truncated cone is 550 mm, the arc radius R of the inner cavity bottom circumference of the core lower part 3 is 92 mm, four protrusion structures 5 are evenly distributed on the circumference of the inner cavity bottom circular plane diameter ¢ of 140 mm, and the thickness c of the circular plane part is 95 mm. The bottom circle diameter d of the conical protrusion structure is 75 mm, and the height h is 75 mm.

[0135] The upper width m of the joint seam 4 is 10 mm, and the lower width n is 5 mm.

[0136] The upper part 2 of the sleeve core is prepared by isostatic pressing, with waste magnesium carbon brick recycled granular material as the main raw material, and is composed of the following materials by weight percentage: 21% of waste magnesium carbon brick recycled granular material with a particle size of 3mm≦<5mm, 30% of waste magnesium carbon brick recycled granular material with a particle size of 1mm≦<3mm, 14% of waste magnesium carbon brick recycled fine powder with a particle size of ≦0.074mm, 10% of sintered magnesia sand with a particle size of 0.074mm<<1mm, 7% of sintered magnesia sand with a particle size of ≦0.074mm, 8.5% of flake graphite, 3% of silicon powder, 3% of silicon carbide powder, and 4% of phenolic resin.

[0137] The core upper part 2 is prepared by isostatic pressing, which includes the following steps:

[0138] 1) Ingredients: weigh the above raw materials according to the above ratio;

[0139] 2) Mixing: preheat the mixer to 45°C, add 3mm≦particle size<5mm, 1mm≦particle size≤3mm and 0.074mm<particle size<1mm sintered magnesia at low speed, add phenolic resin after dry mixing for 2 minutes, add flake graphite after wet mixing for 3 minutes, add fine powder with particle size ≤0.074mm and antioxidant after wet mixing for 2 minutes, wet mix for 3 minutes, mix at high speed for 12 minutes, and discharge. The temperature of the mud during mixing is less than 70°C;

[0140] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 200MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;

[0141] 4) After the green body is stored at room temperature for 6 hours, it is put into the kiln for baking: ① uniformly and continuously heated from room temperature to 80°C, heating and keeping warm for 12 hours each; ② uniformly and continuously heated from 80°C to 150°C, heating and keeping warm for 6 hours each; ② uniformly and continuously heated from 150°C to 200°C, heating and keeping warm for 12 hours each, and then naturally cooled and taken out of the kiln. The preparation of the sleeve core 2 is completed, and its compressive strength is ≥40MPa.

[0142] 4) Natural drying and baking: After the green body is naturally dried for 12 hours, it is put into the kiln for baking: ① heat up from room temperature to 150℃ at a heating rate of 10℃ / h and keep warm for 6 hours; ② heat up from room temperature to 210℃ at a heating rate of 10℃ / h and keep warm for 20 hours; ③ stop the fire, cool naturally to room temperature and then take out of the kiln. The preparation of the lower part 3 of the core sleeve is completed, and its compressive strength is ≥40MPa.

[0143] The core lower part 3 is prepared by isostatic pressing and is made of the following raw materials in percentage by weight:

[0144] Main material: 79wt% sintered magnesia mixed with 1mm≦particle size≤3mm, 0.074mm<particle size<1mm, and particle size≦0.074mm

[0145] Auxiliary materials: flake graphite 14wt%

[0146] Antioxidant: Aluminum-magnesium alloy powder 3.3wt%

[0147] Binder: 3.7wt% phenolic resin.

[0148] The core lower part 3 is prepared by isostatic pressing, which includes the following steps:

[0149] 1) Ingredients: weigh the above raw materials according to the above ratio;

[0150] 2) Mixing: preheat the mixer to 45°C, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.074mm<particle size<1mm at low speed, add phenolic resin after dry mixing for 1 minute, add flake graphite after wet mixing for 3 minutes, add sintered magnesia with a particle size of ≤0.074mm and antioxidant after wet mixing for 3 minutes, wet mix for 2 minutes, mix at high speed for 10 minutes, and discharge. During the mixing process, the temperature of the mud material is less than 70°C;

[0151] 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 220MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed;

[0152] 4) Natural drying and baking: After the green body is naturally dried for 12 hours, it is put into the kiln for baking: ① heat up from room temperature to 150℃ at a heating rate of 10℃ / h and keep warm for 6 hours; ② heat up from room temperature to 210℃ at a heating rate of 10℃ / h and keep warm for 20 hours; ③ stop the fire, cool naturally to room temperature and then take out of the kiln. The preparation of the lower part 3 of the core sleeve is completed, and its compressive strength is ≥40MPa.

[0153] A preparation method for a combined special-shaped blank continuous casting tundish turbulence controller comprises the following steps: sequentially inserting a sleeve core lower part 3 and a sleeve core upper part 2 into a shell 1 of the turbulence controller from bottom to top, ensuring that the longitudinal center lines of the sleeve core lower part 3 and the sleeve core upper part 2 coincide with the longitudinal center line of the inner cavity of the shell 1, filling a joint seam 4 between the shell 1 and the sleeve core lower part 3 and the sleeve core upper part 2 with sintered magnesia sand with a particle size of ≤1 mm, and applying a layer of recycled magnesia carbonaceous coating material with a thickness of 30 mm on the outer surface thereof, and naturally curing for 2 days, thereby completing the preparation of the combined special-shaped blank continuous casting tundish turbulence controller.

[0154] Comparative Example 1: CN104707956B discloses a turbulence controller for a continuous casting tundish of a special-shaped billet and an installation method thereof, comprising an outer shell, a bottom plate, a sleeve core and a pressure ring. The outer shell is a cavity structure with an upper end opening, the bottom plate is located on the bottom of the outer shell cavity, the bottom end of the sleeve core is located above the bottom plate, the pressure ring is arranged at the upper end of the sleeve core and is located in the outer shell cavity, and expansion joints are arranged between the bottom of the inner cavity of the outer shell and the bottom plate, and between the inner wall of the outer shell and the sleeve core. The invention solves the problem of falling off of the upper layer of magnesium-carbon bricks on the side wall of the sleeve core by arranging a pressure ring above the sleeve core; when installing the turbulence controller, a plurality of pressure bricks are arranged on the same circumference in the same plane above the pressure ring to solve the problem of overall floating of the turbulence controller.

[0155] The structural materials, service life, slag rolling condition in the impact zone of the tundish injection flow, and total oxygen content in the molten steel in the crystallizer of a turbulence controller for a shaped billet continuous casting tundish are disclosed in Examples 1-3 of the present invention and the comparative document CN104707956B (comparison test steel grade Q355B, gas samples are taken from the crystallizer, and the oxygen content is detected. The oxygen content in steel is the sum of dissolved oxygen and non-metallic oxide inclusion combined oxygen. Since the dissolved oxygen content is not much, it is generally believed that the non-metallic oxide inclusion oxygen content in steel is the total oxygen content, that is, the total oxygen content in steel represents the control level of oxide inclusions in steel) are compared in the application of the tundish for shaped billet continuous casting of Laiwu Iron and Steel Group Yinshan Steel Co., Ltd., as shown in Table 1 below:

[0156] The comparison of the application of tundish for continuous casting of special-shaped billets in Laiwu Iron and Steel Group Yinshan Steel Co., Ltd. is shown in the following table:

[0157]

[0158]

[0159]

[0160] By comparing the data in the above table, the service life of the combined special-shaped billet continuous casting tundish turbulence controller prepared by the present invention is increased by more than 4 hours year-on-year compared with the special-shaped billet continuous casting tundish turbulence controller described in the existing patent technology CN104707956B, the total oxygen content in the molten steel in the crystallizer is reduced by more than 15% year-on-year, the production cost is reduced by more than 16% year-on-year, and the problem of slag rolling in the impact zone of the tundish is effectively solved.

[0161] Although the above describes the specific implementation mode of the invention in conjunction with the drawings, it is not intended to limit the scope of protection of the invention. Based on the technical solution of the present invention, various modifications or variations that can be made by those skilled in the art without creative work are still within the scope of protection of the present invention.

Claims

1. A combined profiled blank continuous casting tundish turbulence controller, comprising a housing (1) and a sleeve core, wherein the sleeve core is arranged in an inner cavity of the housing, It is characterized in that The core comprises an upper core portion (2) and a lower core portion (3) arranged in a vertical direction, wherein the lower core portion (3) is arranged on the bottom surface of the inner cavity of the outer shell (1), and the longitudinal centerline of the upper core portion (2) and the lower core portion (3) coincides with the longitudinal centerline of the inner cavity of the outer shell (1), a joint seam (4) is arranged between the side walls of the outer shell (1) and the core, and a plurality of conical protrusion structures (5) are arranged at the bottom of the inner cavity of the core, wherein the protrusion structures (5) are arranged in an array on a circle with the longitudinal centerline of the lower core portion (3) as the axis. The upper part of the sleeve core (2) is composed of the following materials by weight percentage: 20-24% of recycled granular materials of waste magnesia carbon bricks with a particle size of 3mm≦<5mm, 28-32% of recycled granular materials of waste magnesia carbon bricks with a particle size of 1mm≦<3mm, 10-14% of recycled fine powder of waste magnesia carbon bricks with a particle size of 0.074mm≦, 10-15% of sintered magnesia sand with a particle size of 0.074mm<<1mm, 5-9% of sintered magnesia sand with a particle size of 0.074mm≦, 7-10% of flake graphite, 4-5% of antioxidant, and 3.5-4.5% of phenolic resin; The main material of the lower part of the core sleeve (3) is 76-84wt% of sintered magnesia mixed with 1mm≤particle size≤3mm, 0.074mm<particle size<1mm, and particle size≤0.074mm.

2. A combined turbulence controller for continuous casting of profiled blanks as claimed in claim 1, It is characterized in that The inner cavity of the upper core part (2) is in the shape of a truncated cone with a small inner diameter at the upper part and a large inner cavity at the lower part. The inner cavity bottom surface of the lower core part (3) is an arc curved surface. The inner cavity side wall and the bottom surface of the lower core part (3) are transitioned by an arc chamfer.

3. A combined turbulence controller for continuous casting of profiled blanks as claimed in claim 2, It is characterized in that The outer shape of the upper part (2) of the sleeve core is a truncated cone with a large upper bottom surface and a small lower bottom surface, and the outer shape of the lower part (3) of the sleeve core is a truncated cone with a large upper bottom surface and a small lower bottom surface.

4. A combined turbulence controller for continuous casting of profiled blanks as claimed in claim 1, 2 or 3, It is characterized in that The number of the protruding structures (5) is four.

5. A combined turbulence controller for continuous casting of profiled blanks as claimed in claim 3, It is characterized in that The height a of the core upper part (2) is 258-288 mm, the outer diameter D1 of the upper bottom surface of the core upper part (2) is 650-700 mm, the inner diameter d1 of the upper bottom surface of the core upper part (2) is 350-400 mm, the outer diameter D2 of the lower bottom surface of the core upper part (2) is 550-600 mm, the inner diameter d2 of the lower bottom surface of the core upper part (2) is 420-470 mm, the height b of the core lower part (3) is 172-202 mm, and the core lower part (4) is 172-202 mm. The outer diameter D2 of the upper bottom surface of the sleeve core (3) is 550-600 mm, the outer diameter D3 of the lower bottom surface of the sleeve core lower part (3) is 475-525 mm, the arc chamfer radius R of the sleeve core lower part (3) is 82-102 mm, the thickness c of the bottom of the sleeve core lower part (3) is 90-100 mm, the inner diameter of the upper bottom surface of the sleeve core lower part (3) is the same as the inner diameter of the lower bottom surface of the sleeve core upper part (2), and the outer diameter of the upper bottom surface of the sleeve core lower part (3) is the same as the outer diameter of the lower bottom surface of the sleeve core upper part (2).

6. A combined turbulence controller for continuous casting of profiled blanks as claimed in claim 5, It is characterized in that The protruding structures (5) are evenly distributed on a circle with a diameter of ¢130-150 mm on the bottom surface of the inner cavity. The bottom circle diameter d of the conical protruding structures is 70-80 mm, and the height h is 70-80 mm.

7. A method for preparing a combined turbulence controller for continuous casting of profiled blanks. It is characterized in that The following steps are involved: S1: sequentially inserting the core lower part (3) and the core upper part (2) into the housing (1) of the turbulence controller from bottom to top, ensuring that the longitudinal center lines of the core lower part (3) and the core upper part (2) coincide with the longitudinal center line of the inner cavity of the housing (1); S2: The joint (4) between the outer shell (1) and the sleeve core is filled with sintered magnesia sand with a particle size of ≤1 mm; S3: Apply a layer of recycled magnesium carbon coating material with a thickness of 25-35mm on the outer surface of the sintered magnesia sand filled in the joint. The recycled magnesium carbon coating material is a coating material prepared by treating and processing waste magnesium carbon bricks with a particle size of 1mm≦≤3mm and 0.074mm<particle size<1mm, and sintered magnesia sand fine powder with a particle size of ≤0.074mm, soft clay, silicon powder, and sodium tripolyphosphate. The weight percentage of the recycled magnesium carbon coating material is 60-70%, the MgO content is ≥65wt%, and the volume density is ≥1.87g / cm 3 ; S4: After natural curing for 1 to 2 days, the preparation of the turbulence controller for the combined special-shaped billet continuous casting tundish is completed.

8. A method for preparing a combined profiled blank continuous casting tundish turbulence controller as claimed in claim 7, It is characterized in that The core upper part (2) is prepared by isostatic pressing, which comprises the following steps: 1) Ingredients: Preparation of sintered magnesia fine powder: The recycled granular materials of waste magnesia carbon bricks with a particle size of 0.074 mm < 1 mm are sprayed for hydration and naturally dried, and then ground into sintered magnesia fine powder with a particle size of ≦0.074 by a ball mill. Weigh the materials according to the proportion; 2) Mixing: Preheat the mixer to 40-50°C. When the mixer is running at low speed, add sintered magnesia with a particle size of 3mm≦<5mm, 1mm≦≤3mm and 0.074mm<<1mm. After dry mixing for 1 to 2 minutes, add phenolic resin. After 2-3 minutes of wet mixing, add flake graphite. After 2-3 minutes of wet mixing, add antioxidant and sintered magnesia fine powder with a particle size of ≤0.074mm. Wet mix for 2 to 3 minutes, high speed mix for 10 to 15 minutes, Discharging; The temperature of the clay during mixing is less than 70°C; 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 200-250MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed; 4) After the green body is stored at room temperature for 4 to 8 hours, it is put into the kiln for baking: The temperature is raised evenly and continuously from room temperature to 80±10℃, and the heating and heat preservation time are 8 to 16 hours respectively. Raise the temperature evenly and continuously from 80±10℃ to 150±10℃, and keep warm for 4 to 8 hours respectively. Raise the temperature evenly and continuously from 150±10℃ to 200±10℃, with each heating and heat preservation taking 8 to 16 hours. The firing is stopped, and the product is taken out of the kiln after natural cooling, and the preparation of the upper part of the core sleeve (2) is completed.

9. A method for preparing a combined profiled blank continuous casting tundish turbulence controller as claimed in claim 7 or 8, It is characterized in that The core lower part (3) is prepared by isostatic pressing, which comprises the following steps: 1) Batching: weigh the materials according to the proportion; 2) Mixing: Preheat the mixer to 40-50°C. When the mixer is running at low speed, add sintered magnesia with a particle size of 1mm≦≤3mm and 0.074mm<particle size<1mm. After dry mixing for 1 to 2 minutes, add phenolic resin. After 2-3 minutes of wet mixing, add flake graphite. After 2-3 minutes of wet mixing, add antioxidant and sintered magnesia with a particle size of ≤0.074mm. Wet mix for 2 to 3 minutes, high speed mix for 10 to 15 minutes, Discharging; The temperature of the clay during mixing is less than 70°C; 3) Green body molding: fill the clay into the mold, then remove the air in the mold, press it under 200-250MPa with isostatic pressure and then take it out of the mold, and the green body molding is completed; 4) Natural drying and baking: After the green body is naturally dried for 8 to 16 hours, it is put into the kiln for baking. Raise the temperature from room temperature to 140-160°C at a rate of 10°C / h and keep warm for 4-8 hours; Then, the temperature is raised to 200-220°C at a rate of 10°C / h and kept at this temperature for 16-24 hours; The firing is stopped, and the product is naturally cooled to room temperature before being taken out of the kiln. The preparation of the lower part of the core sleeve (3) is completed.