Photosensitive resin composition and photosensitive dry film
By using a photosensitive resin composition of phenolic hydroxyl resin and epoxy additives in electronic devices, the problem of insufficient bonding force between copper wiring and dielectric films is solved, and efficient bonding force improvement and device reliability are achieved.
Patent Information
- Application Number
- CN201911050756.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-10-31
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-10-31
AI Technical Summary
It is difficult to achieve efficient bonding between copper wiring and dielectric films in electronic devices with existing technology, which affects device performance. In particular, because copper does not contain functional groups, commonly used coupling agents cannot effectively enhance the bonding force.
A photosensitive resin composition containing phenolic hydroxyl resin and epoxy additive is used. The epoxy additive contains 1 to 8 epoxy groups and nitrogen, sulfur, and phosphorus elements. It is used to form a coating that improves the bonding force of the copper interface and passes light Curing techniques form patterns.
It improves the bonding force between copper wiring and dielectric film, enhances the reliability and performance of the device, while maintaining the photosensitivity of the photosensitive resin, and is suitable for electronic devices such as chips.
Smart Images

Figure BDA0002255275570000031 
Figure BDA0002255275570000041 
Figure BDA0002255275570000042
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This nonprovisional application claims priority under 35 U.S.C. 119(a) to Patent Application No. 2018-206503 filed in Japan on November 1, 2018, the entire contents of which are incorporated herein by reference. Technical Field
[0003] The invention relates to a photosensitive resin composition, a photosensitive dry film and a pattern forming method. Background Art
[0004] In order to meet the recent demand for compact and high-performance electronic tools, the pattern size of the memory and CPU installed in such tools has been reduced. As pattern miniaturization technology approaches its limit, the structure of a multi-layer wiring layer is essential to achieve a higher level of computing. The structure of the multi-layer wiring layer is obtained by forming a first wiring layer, forming an interlayer dielectric film thereon, forming a second wiring layer thereon, and further forming an interlayer dielectric film. These steps are repeated until a structure with two or more layers of wiring layers stacked is obtained. In this process, a process of intentionally corroding copper wiring to make the copper wiring have ultra-fine concave-convex to enhance the bonding force between the interlayer dielectric film and the copper wiring is adopted, so as to give the device sufficient reliability. However, as a result of the progress of electronic devices to higher performance, there has been a situation where the concave-convex on the copper wiring may adversely affect the performance of the device. It is necessary to establish a material that can be satisfactorily combined with copper wiring that is substantially free of concave-convex.
[0005] Many efforts have been made to obtain satisfactory bonding strength. For example, Patent Documents 1 and 2 disclose the use of silane coupling agents and titanate coupling agents. Since copper generally does not have a functional group for coupling, coupling agents sometimes cannot fully enhance the bonding strength.
[0006] Citation List
[0007] Patent Document 1: JP 4918313
[0008] Patent Document 2: JP 4183459 Summary of the invention
[0009] An object of the present invention is to provide a photosensitive resin composition having improved bonding strength to metal wiring, particularly copper wiring.
[0010] Since the copper used for wiring does not contain functional groups, the bonding strength enhancement method based on the reaction of coupling agents with functional groups on the object is invalid. It is estimated that the coordination of elements such as nitrogen, sulfur and phosphorus will be effective. These elements often have nucleophilicity or alkalinity, which may adversely affect the photosensitivity mechanism. Moreover, most of these compounds are incompatible with resin compositions, resulting in a loss of reliability.
[0011] The inventors have discovered a photosensitive resin composition comprising a phenolic hydroxyl group-containing resin and an epoxy additive in the form of a compound having 1 to 8 epoxy groups per molecule, containing nitrogen, sulfur and / or phosphorus and having a molecular weight of 50 to 6,000, which forms a coating that exhibits improved bonding to copper and good reliability without sacrificing photosensitivity.
[0012] In one aspect, the present invention provides a photosensitive resin composition comprising (A) a resin having a phenolic hydroxyl group and (B) an epoxy additive in the form of a compound having 1 to 8 epoxy groups per molecule, containing at least one element selected from nitrogen, sulfur and phosphorus, and having a molecular weight of 50 to 6000, wherein the epoxy additive (B) is present in an amount of 0.1 to 18 parts by weight relative to 100 parts by weight of the resin (A).
[0013] In a preferred embodiment, the resin (A) is at least one selected from polybenzoxazole, polyimide, epoxy resin, and silicone-modified resins thereof.
[0014] In a preferred embodiment, the composition may further include (C) a crosslinking agent, (D) a photoacid generator, and / or (E) an organic solvent.
[0015] In another aspect, the present invention provides a photosensitive resin coating obtained from the photosensitive resin composition defined above.
[0016] In another aspect, the present invention provides a photosensitive dry film comprising the photosensitive resin coating defined above.
[0017] In another aspect, the present invention provides a pattern forming method comprising the steps of:
[0018] (i) forming a photosensitive resin coating on a substrate using the photosensitive resin composition defined above,
[0019] (ii) exposing the photosensitive resin coating to radiation, and
[0020] (iii) The exposed photosensitive resin coating is developed using a developer.
[0021] Alternatively, the pattern forming method may include the following steps:
[0022] (i) forming a photosensitive resin coating on a substrate using the photosensitive dry film defined above,
[0023] (ii) exposing the photosensitive resin coating to radiation, and
[0024] (iii) The exposed photosensitive resin coating is developed using a developer.
[0025] Advantageous Effects of the Invention
[0026] Since the epoxy additive contains nitrogen, sulfur or phosphorus atoms that can interact with copper, it helps to improve the bonding force at the copper interface. At the same time, since the epoxy additive has an epoxy group that reacts with the phenolic hydroxyl group in the composition, it is fixed in the cured product, eliminating the risk of precipitation or separation. Since the amount of epoxy additive added is limited, the composition can be used without reducing the photosensitivity. As a result, the composition is effectively applicable to device chips. DETAILED DESCRIPTION
[0027] The symbols used in this paper (C n -C m ) refers to a group containing n to m carbon atoms per group. In the chemical formula, the dotted line represents a valence bond.
[0028] (A) Resins containing phenolic hydroxyl groups
[0029] The resin used as component (A) in the photosensitive resin composition of the present invention is not particularly limited as long as it has a phenolic hydroxyl group. The resin (A) is preferably selected from polybenzoxazole, polyimide, epoxy resin and their silicone-modified resins, because when combined with such a resin, the epoxy additive (B) exerts its effect to a greater extent.
[0030] The polybenzoxazole and silicone-modified polybenzoxazole may be selected from a wide range of those conventionally used, and preferably have the following formula (1).
[0031]
[0032] In formula (1), L 1 is a single bond or C1-C 10 R and R' are each independently a C1-C6 monovalent organic group, L 2 is a divalent organic group that may contain an organic silicon skeleton, n 1 and n 2 Each independently represents an integer from 0 to 2.
[0033] The polyimide and silicone-modified polyimide should preferably have formula (2), but are not limited thereto.
[0034]
[0035] In formula (2), X 1 is a tetravalent group having the formula (3).
[0036]
[0037] In formula (3), R 1 To R 6 Each independently is a C1-C8 monovalent hydrocarbon group. The monovalent hydrocarbon group may be linear, branched or cyclic. Examples thereof include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; aryl groups such as phenyl; aralkyl groups such as benzyl and phenethyl; and alkenyl groups such as vinyl, 1-propenyl, 2-propenyl, isopropenyl and butenyl. Methyl, ethyl, phenyl and vinyl are particularly preferred because of the availability of reactants.
[0038] In formula (3), R 7 and R 8 Each is independently a single bond or C1-C 12 Divalent hydrocarbon group. The divalent hydrocarbon group may be linear, branched or cyclic. Examples thereof include methylene, ethane-1,1-diyl, ethane-1,2-diyl, propane-1,3-diyl, butane-1,4-diyl, benzene-1,4-diyl and biphenyl-4,4'-diyl. Preferably, R 7 and R 8 Each is a single bond, a methylene group, an ethane-1,1-diyl group, a propane-1,3-diyl group or a benzene-1,4-diyl group.
[0039] In formula (3), R 9 and R 10 Each independently is a trivalent organic group. The trivalent organic group preferably has 2 to 10 carbon atoms. Examples of the trivalent organic group are shown below, but are not limited thereto.
[0040]
[0041] In formula (3), r is an integer of 0 to 120, preferably an integer of 3 to 80, and more preferably an integer of 5 to 50. When r ≥ 2, that is, when two or more siloxane units are included, the siloxane units may be of the same type or of two or more different types. When two or more different types of siloxane units are included, they may be randomly or alternately bonded, or may include multiple blocks of the same type of siloxane units.
[0042] Quaternary Group X 1 Examples are shown below, but are not limited thereto.
[0043]
[0044] Here, r is defined as above, r 1 and r 2 For 0≤r 1 ≤119、0≤r 2 ≤120, and 1≤r 1 +r 2 An integer in the range ≤120.
[0045]
[0046] Here, r is defined as above, r 3 and r 4 are each independently 0 or an integer of at least 1, r 3 +r 4 = r, r 5 and r 6 are each independently 0 or an integer of at least 1, r 5 +r 6 =r.
[0047] Quaternary Group X 1 Preferred examples are shown below.
[0048]
[0049] Group X 1 It can be derived from a modified silicone obtained by reacting an organohydrogenpolysiloxane with an acid anhydride having an unsaturated group, such as succinic anhydride, norbornene dicarboxylic anhydride, propyl nadic anhydride or phthalic anhydride. The number of siloxane units in the anhydride-modified polysiloxane is distributed according to the distribution of the number of siloxane units in the organohydrogenpolysiloxane. Therefore, r in formula (3) represents the average number of siloxane units.
[0050] In formula (2), X 2 is a tetravalent organic group other than the group having the formula (3). Although the tetravalent organic group is not particularly limited, preferred examples thereof are shown below.
[0051]
[0052] In formula (2), Y 1 It is a divalent group represented by formula (4) having at least one phenolic hydroxyl group.
[0053]
[0054] In formula (4), A 1 To A 3Each is independently a single bond, a methylene group, an ether bond, a sulfonyl group, an amide bond, a propane-2,2-diyl group, a 1,1,1,3,3,3-hexafluoropropane-2,2-diyl group and a fluorene-9,9-diyl group.
[0055] In formula (4), a is an integer of 1 to 10, b is 0 or 1, and c is 0 or 1.
[0056] In formula (4), R 11 To R 12 Each independently represents a hydroxyl group or a group containing an alcoholic hydroxyl group, R 11 To R 12 At least one of the groups is a hydroxyl group. Examples of the group containing an alcoholic hydroxyl group include -OCH2CH(OH)CH2OH and -OCH(CH2OH)CH2OH.
[0057] In formula (4), R 13 To R 16 Each is independently a C1-C4 alkyl group. Suitable alkyl groups include methyl, ethyl, propyl and butyl, of which methyl is preferred. In the case where each of d to g is 2, R 13 To R 16 Each of can be the same or different.
[0058] In formula (4), d to g are each independently 0, 1 or 2, preferably 0 or 1.
[0059] Examples of the group having the formula (4) are shown below, but are not limited thereto.
[0060]
[0061] In formula (2), it means that X 1 The number of repeating units p is 0 or a positive integer, preferably 1 to 500, more preferably 3 to 300; 2 The number q of repeating units is a positive integer, preferably 1 to 500, more preferably 3 to 300.
[0062] Additionally, p and q are in the range of 0≤p / (p+q)<1. For silicone-modified polyimide, p is in the range of 0.1≤p / (p+q)<1, more preferably 0.2≤p / (p+q)≤0.95, even more preferably 0.5≤p / (p+q)≤0.9.
[0063] The polyimide and the silicone-modified polyimide may include at least one type of repeating unit selected from the repeating unit having the formula (2-1) and the repeating unit having the formula (2-2).
[0064]
[0065] In formulas (2-1) and (2-2), X 1 and X 2 As defined above. 2 is a divalent group other than a group having formula (4). Suitable divalent groups include those having 11 and R 12 Those groups of formula (4) are eliminated, as well as the divalent organic groups containing the organosilicon skeleton.
[0066] In the case where the polyimide contains a repeating unit having the formula (2-1) and / or a repeating unit having the formula (2-2), the content of these repeating units is arbitrary as long as the advantages of the present invention are not impaired.
[0067] The polyimide and silicone-modified polyimide preferably have a weight average molecular weight (Mw) of 2,000 to 200,000, more preferably 4,000 to 100,000. As long as the Mw is within this range, easy handling is ensured and a cured product with sufficient strength is obtained. It should be noted that throughout the specification, Mw is measured relative to polystyrene standards by gel permeation chromatography (GPC) using tetrahydrofuran (THF) solvent.
[0068] Examples of the epoxy resin and the silicone-modified epoxy resin include those having the following formula (5), but are not limited thereto.
[0069]
[0070] In formula (5), R 21 To R 26 Each independently is C1-C 20 Suitable monovalent hydrocarbon groups include linear, branched or cyclic alkyl, alkenyl and alkynyl groups, but are not limited thereto. Preferably, R 21 To R 26 Selected from C1-C 12 A monovalent hydrocarbon group or an alkoxy group, preferably a C1-C 10 R is a monovalent hydrocarbon group and an alkoxy group, and even more preferably a C1-C6 monovalent hydrocarbon group and an alkoxy group. 21 To R 26 Preferred illustrative examples of include methyl, ethyl, propyl, hexyl, cyclohexyl and phenyl, with methyl and phenyl being more preferred due to the availability of reactants.
[0071] In formula (5), Z 1 is a divalent group having the formula (6).
[0072]
[0073] In formula (6), Z 11R is a single bond, methylene, propane-2,2-diyl, 1,1,1,3,3,3-hexafluoropropane-2,2-diyl or fluorene-9,9-diyl. 31 and R 32 may be the same or different, and are independently C1-C 20 A monovalent hydrocarbon group or an alkoxy group. 31 and R 32 Preferably, it is a C1-C4 alkyl or alkoxy group, more preferably a C1-C2 alkyl or alkoxy group. Preferred illustrative examples include methyl, ethyl, propyl, tert-butyl, methoxy and ethoxy. Subscripts w and x are each independently an integer from 0 to 2.
[0074] In formula (5), Z 2 is a divalent group having formula (7):
[0075] Wherein v is an integer from 0 to 300.
[0076] In formula (5), Z 3 is a divalent group having the formula (8).
[0077]
[0078] In formula (8), Z 12 R is a single bond, methylene, propane-2,2-diyl, 1,1,1,3,3,3-hexafluoropropane-2,2-diyl or fluorene-9,9-diyl. 33 and R 34 may be the same or different, and are independently C1-C 20 A monovalent hydrocarbon group or an alkoxy group. 33 and R 34 Preferably, it is a C1-C4 alkyl or alkoxy group, more preferably a C1-C2 alkyl or alkoxy group. Preferred illustrative examples include methyl, ethyl, propyl, tert-butyl, methoxy and ethoxy. Subscripts y and z are each independently an integer from 0 to 2.
[0079] In formula (5), k represents the composition ratio of the corresponding repeating units. 1 , k 2 , k 3 , k 4 and k 5 is a positive number in the following range: 0 <k 1 <1,0 <k 2 <1, 0≤k 3 <1, 0≤k 4 <1,0 <k 5 <1, 0.67≤(k 2 +k 4 ) / (k 1 +k3 +k 5 )≤1.67 and k 1 +k 2 +k 3 +k 4 +k 5 =1; h is an integer from 0 to 300.
[0080] (B) Epoxy Additives
[0081] The epoxy additive as component (B) is a compound containing 1 to 8 epoxy groups per molecule, containing at least one selected from nitrogen, sulfur and phosphorus and having a molecular weight of 50 to 6,000. Since the epoxy additive has an epoxy group that reacts with the phenolic hydroxyl group in the composition, it is fixed as a cured product. In addition, the epoxy additive contains nitrogen, sulfur and / or phosphorus atoms, which interact with copper to enhance the bonding force at the copper interface.
[0082] Preferred examples of the epoxy additive include the following compounds.
[0083]
[0084] Also preferably, the compound having the formula (9) can be used as the epoxy additive.
[0085] X A m -X B (9)
[0086] In formula (9), m is an integer from 1 to 3. A X is a monovalent organic group having at least one epoxy group. B is a group containing at least one element selected from nitrogen, sulfur and phosphorus. A and X B The structure of the epoxy additive is not critical, but it is necessary that the epoxy additive has a molecular weight of 50 to 6,000. If the molecular weight is less than this range, the compound will evaporate before curing, and the effect of improving the bonding strength cannot be obtained. If the molecular weight is greater than this range, the compound may become incompatible, and the effect of improving the bonding strength cannot be obtained or the curing strength may be reduced.
[0087] X A An example of is shown below.
[0088]
[0089] Here, the dotted line indicates the B Bonded valence bond. a To R e Each is independently a C1-C6 monovalent hydrocarbon group. 1 and E 2Each independently is C1-C 12 Divalent hydrocarbon group. 1 、m 2 and m 3 are each independently an integer from 0 to 3, j 1 is an integer from 0 to 7, j 2 is an integer from 1 to 8, j 3 An integer from 1 to 3.
[0090] X B An example of is shown below.
[0091]
[0092] In formula (9), when m is 2 or 3, the group X A Can be the same or different.
[0093] The compound of formula (9) can be easily prepared by reacting a compound having at least two epoxy groups with nitric acid, sulfuric acid or phosphoric acid. For example, the desired compound can be obtained by dissolving the compound having at least two epoxy groups in a solvent in a reactor, adding the acid dropwise thereto, stirring the mixture for 2 hours and distilling the reaction mixture.
[0094] The epoxy additive is preferably added in an amount of 0.1 to 18 parts by weight, more preferably 0.5 to 15 parts by weight, and even more preferably 1.0 to 10 parts by weight per 100 parts by weight of the resin as component (A). Outside this range, a smaller amount of the epoxy additive may be insufficient in the effect of improving the bonding force, while a larger amount may result in reduced photosensitivity, inhibited curing, and reduced device reliability.
[0095] Other components
[0096] If necessary, the composition of the present invention may further include (C) a crosslinking agent, (D) a photoacid generator, (E) an organic solvent, (F) a polyfunctional epoxy compound other than the compound as component (B), and the like.
[0097] (C) Cross-linking agent
[0098] The crosslinking agent undergoes a crosslinking reaction with component (A) to promote pattern formation and increase the strength of the resin coating.
[0099] The crosslinking agent is preferably selected from nitrogen-containing compounds containing at least two hydroxymethyl and / or alkoxymethyl groups per molecule (such as melamine, guanamine, glycoluril and urea compounds), and condensates thereof, and phenol compounds having at least two hydroxymethyl or alkoxymethyl groups per molecule, but is not limited thereto.
[0100] Suitable melamine compounds include those having formula (10).
[0101]
[0102] In formula (10), R 41 To R 46 are each independently hydroxymethyl, C2-C5 alkoxymethyl or hydrogen, and R 41 To R 46 At least two of the methyl groups are hydroxymethyl or alkoxymethyl. Suitable alkoxymethyl groups include methoxymethyl and ethoxymethyl.
[0103] Suitable melamine compounds include trimethoxymethylmonomethylolmelamine, dimethoxymethylmonomethylolmelamine, trimethylolmelamine, hexamethylolmelamine, hexamethoxymethylmelamine and hexaethoxymethylmelamine.
[0104] Suitable guanamine compounds include tetramethylolguanamine, tetramethoxymethylguanamine and tetramethoxyethylguanamine.
[0105] Suitable glycoluril compounds include tetrakishydroxymethyl glycoluril and tetrakis(methoxymethyl) glycoluril.
[0106] Suitable urea compounds include tetramethylol urea, tetramethoxymethyl urea, tetramethoxyethyl urea, tetraethoxymethyl urea and tetrapropoxymethyl urea.
[0107] The condensate of the nitrogen-containing compound includes a condensate of the nitrogen-containing compound and formaldehyde, preferably a condensate of a melamine compound or a urea compound. The condensate of the nitrogen-containing compound can be prepared by any method known in the art.
[0108] Examples of the phenol compound having an average of at least two hydroxymethyl groups or alkoxymethyl groups per molecule include (2-hydroxy-5-methyl)-1,3-benzenedimethanol and 2,2′,6,6′-tetramethoxymethylbisphenol A.
[0109] The crosslinking agent (C) is preferably used in an amount of 0.5 to 50 parts by weight, more preferably 1 to 30 parts by weight per 100 parts by weight of component (A). The amount of the crosslinking agent within this range ensures that the composition can be effectively photocured and is advantageously used as a resist material. The crosslinking agent can be used alone or in combination.
[0110] (D) Photoacid generator
[0111] There is no particular limitation on the photoacid generator (PAG), as long as it decomposes to generate acid when exposed to light, preferably light with a wavelength of 240 to 500 nm. The generated acid is used as a curing catalyst. Typical PAGs include onium salts, diazomethane derivatives, oxadioxime derivatives, β-ketosulfone derivatives, disulfone derivatives, sulfonic acid nitrobenzyl ester derivatives, sulfonic acid ester derivatives, imidosulfonic acid ester derivatives, sulfonic acid oxime ester derivatives, imidosulfonic acid ester derivatives and triazine derivatives.
[0112] Suitable onium salts include sulfonium salts having the following formula (11) and iodonium salts having the following formula (12).
[0113]
[0114] In equations (11) and (12), R 51 To R 55 Each independently is C1-C 12 Alkyl, C6-C 12 Aryl or C7-C 12 An aralkyl group which may have a substituent. - It is a non-nucleophilic counter ion.
[0115] The alkyl group may be straight chain, branched or cyclic. Examples include methyl, ethyl, n-propyl, isopropyl, cyclopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, cyclobutyl, n-pentyl, cyclopentyl, cyclohexyl, norbornyl and adamantyl. Exemplary aryl groups include phenyl, naphthyl and biphenyl. Exemplary aralkyl groups include benzyl and phenethyl. Examples of substituents include oxo, straight chain, branched or cyclic C1-C 12 Alkoxy, linear, branched or cyclic C1-C 12 Alkyl, C6-C 24 Aryl, C7-C 25 Arylalkyl, C6-C 24 Aryloxy and C6-C 24 Arylthio.
[0116] Preferably, R 51 To R 55 Selected from optionally substituted alkyl, such as methyl, ethyl, propyl, butyl, cyclohexyl, norbornyl, adamantyl, 2-oxocyclohexyl; optionally substituted aryl, such as phenyl, naphthyl, biphenyl, 2-, 3- or 4-methoxyphenyl, ethoxyphenyl, 3- or 4-tert-butoxyphenyl, 2-, 3- or 4-methylphenyl, ethylphenyl, 4-tert-butylphenyl, 4-butylphenyl, dimethylphenyl, terphenyl, biphenyloxyphenyl and biphenylylthiophenyl; and optionally substituted aralkyl, such as benzyl and phenethyl. In particular, optionally substituted aryl and optionally substituted aralkyl are more preferred.
[0117] By A - Examples of non-nucleophilic counterions represented by include halides such as chloride and bromide; fluoroalkanesulfonate ions such as trifluoromethanesulfonate, 1,1,1-trifluoroethanesulfonate and nonafluorobutanesulfonate; arylsulfonate ions such as toluenesulfonate, benzenesulfonate, 4-fluorobenzenesulfonate and 1,2,3,4,5-pentafluorobenzenesulfonate; alkanesulfonate ions such as methanesulfonate and butanesulfonate; hexafluorophosphate ions and fluoroalkylfluorophosphate ions.
[0118] Examples of the diazomethane derivative are compounds of the following formula (13).
[0119]
[0120] In formula (13), R 61 and R 62 Each independently is C1-C 12 alkyl or haloalkyl, optionally substituted C6-C 12 Aryl or optionally substituted C7-C 12 Aralkyl.
[0121] Examples of alkyl groups are as follows for R 51 To R 55 Exemplary haloalkyl groups include trifluoromethyl, 1,1,1-trifluoroethyl, 1,1,1-trichloroethyl and nonafluorobutyl.
[0122] Examples of optionally substituted aryl groups include phenyl; and alkoxyphenyl groups such as 2-, 3- or 4-methoxyphenyl, 2-, 3- or 4-ethoxyphenyl, 3- or 4-tert-butoxyphenyl; alkylphenyl groups such as 2-, 3- or 4-methylphenyl, ethylphenyl, 4-tert-butylphenyl, 4-butylphenyl and dimethylphenyl; halogenated aryl groups such as fluorophenyl, chlorophenyl and 1,2,3,4,5-pentafluorophenyl. Examples of optionally substituted aralkyl groups include benzyl and phenethyl.
[0123] An exemplary glyoxime derivative is a compound of the following formula (14).
[0124]
[0125] In formula (14), R 71 To R 74 Each independently is C1-C 12 alkyl or haloalkyl, optionally substituted C6-C 12 Aryl or optionally substituted C7-C 12 Aralkyl. 73 and R 74can be bonded together to form a ring with the carbon atoms to which they are attached, in which case R 73 and R 74 The combination is C1-C 12 A straight-chain or branched alkane diyl group.
[0126] Examples of alkyl, haloalkyl, optionally substituted aryl and optionally substituted aralkyl are as described above for R 61 and R 62 Suitable straight or branched alkanediyl groups include methylene, ethanediyl, propanediyl, butanediyl and hexanediyl.
[0127] Exemplary onium salts include:
[0128] Diphenyliodonium trifluoromethanesulfonate,
[0129] (p-tert-Butoxyphenyl)phenyliodonium trifluoromethanesulfonate,
[0130] Diphenyliodonium p-toluenesulfonate,
[0131] (p-tert-Butoxyphenyl)phenyliodonium p-toluenesulfonate,
[0132] Triphenylsulfonium trifluoromethanesulfonate,
[0133] (p-tert-Butoxyphenyl)diphenylsulfonium trifluoromethanesulfonate,
[0134] Bis(p-tert-butoxyphenyl)phenylsulfonium trifluoromethanesulfonate,
[0135] Tri(p-tert-butoxyphenyl)sulfonium trifluoromethanesulfonate,
[0136] Triphenylsulfonium p-toluenesulfonate,
[0137] (p-tert-Butoxyphenyl)diphenylsulfonium p-toluenesulfonate,
[0138] Bis(p-tert-butoxyphenyl)phenylsulfonium p-toluenesulfonate,
[0139] Tri(p-tert-butoxyphenyl)sulfonium p-toluenesulfonate,
[0140] Triphenylsulfonium nonafluorobutanesulfonate, triphenylsulfonium butanesulfonate,
[0141] Trimethylsulfonium trifluoromethanesulfonate, trimethylsulfonium p-toluenesulfonate,
[0142] Cyclohexylmethyl (2-oxocyclohexyl)sulfonium trifluoromethanesulfonate,
[0143] Cyclohexylmethyl (2-oxocyclohexyl)sulfonium p-toluenesulfonate,
[0144] Dimethylphenylsulfonium trifluoromethanesulfonate,
[0145] Dimethylphenylsulfonium p-toluenesulfonate,
[0146] Dicyclohexylphenylsulfonium trifluoromethanesulfonate,
[0147] Dicyclohexylphenylsulfonium p-toluenesulfonate,
[0148] Bis(4-tert-butylphenyl)iodonium hexafluorophosphate,
[0149] Diphenyl (4-thiophenoxyphenyl) sulfonium hexafluoroantimonate,
[0150] [4-(4-biphenylthio)phenyl]-4-biphenylphenylsulfonium tris(trifluoromethanesulfonyl)methyl,
[0151] Triphenylsulfonium tetrakis(fluorophenyl)borate,
[0152] tris[4-(4-acetylphenyl)thiophenyl]sulfonium tetrakis(fluorophenyl)borate,
[0153] triphenylsulfonium tetrakis(pentafluorophenyl)borate, and
[0154] Tris[4-(4-acetylphenyl)thiophenyl]sulfonium tetrakis(pentafluorophenyl)borate.
[0155] Examples of diazomethane derivatives include:
[0156] Bis(benzenesulfonyl)diazomethane, Bis(p-toluenesulfonyl)diazomethane,
[0157] Bis(xylenesulfonyl)diazomethane, Bis(cyclohexylsulfonyl)diazomethane,
[0158] Bis(cyclopentylsulfonyl)diazomethane, Bis(n-butylsulfonyl)diazomethane,
[0159] Bis(isobutylsulfonyl)diazomethane, Bis(sec-butylsulfonyl)diazomethane,
[0160] Bis(n-propylsulfonyl)diazomethane, Bis(isopropylsulfonyl)diazomethane,
[0161] Bis(tert-butylsulfonyl)diazomethane, Bis(n-pentylsulfonyl)diazomethane,
[0162] Bis(isopentylsulfonyl)diazomethane, Bis(sec-pentylsulfonyl)diazomethane,
[0163] Bis(tert-amylsulfonyl)diazomethane,
[0164] 1-cyclohexylsulfonyl-1-(tert-butylsulfonyl)diazomethane,
[0165] 1-cyclohexylsulfonyl-1-(tert-amylsulfonyl)diazomethane and
[0166] 1-tert-Amylsulfonyl-1-(tert-butylsulfonyl)diazomethane.
[0167] Exemplary glyoxime derivatives include:
[0168] Bis-O-(p-toluenesulfonyl)-α-dimethylglyoxime,
[0169] Bis-O-(p-toluenesulfonyl)-α-diphenylglyoxime,
[0170] Bis-O-(p-toluenesulfonyl)-α-dicyclohexylglyoxime,
[0171] Bis-O-(p-toluenesulfonyl)-2,3-pentanedione glyoxime,
[0172] Bis-O-(p-toluenesulfonyl)-2-methyl-3,4-pentanedione glyoxime,
[0173] Bis-O-(n-butylsulfonyl)-α-dimethylglyoxime,
[0174] Bis-O-(n-butylsulfonyl)-α-diphenylglyoxime,
[0175] Bis-O-(n-butylsulfonyl)-α-dicyclohexylglyoxime,
[0176] Bis-O-(n-butylsulfonyl)-2,3-pentanedione glyoxime
[0177] Bis-O-(n-butylsulfonyl)-2-methyl-3,4-pentanedione glyoxime
[0178] Bis-O-(methylsulfonyl)-α-dimethylglyoxime,
[0179] Bis-O-(trifluoromethanesulfonyl)-α-dimethylglyoxime,
[0180] Bis-O-(1,1,1-trifluoroethanesulfonyl)-α-dimethylglyoxime,
[0181] Bis-O-(tert-butanesulfonyl)-α-dimethylglyoxime,
[0182] Bis-O-(perfluorooctanesulfonyl)-α-dimethylglyoxime,
[0183] Bis-O-(cyclohexanesulfonyl)-α-dimethylglyoxime,
[0184] Bis-O-(phenylsulfonyl)-α-dimethylglyoxime,
[0185] Bis-O-(p-fluorophenylsulfonyl)-α-dimethylglyoxime,
[0186] Bis-O-(p-tert-butylbenzenesulfonyl)-α-dimethylglyoxime,
[0187] Bis-O-(xylenesulfonyl)-α-dimethylglyoxime, and
[0188] Bis-O-(camphorsulfonyl)-α-dimethylglyoxime.
[0189] Exemplary β-ketosulfone derivatives include:
[0190] 2-cyclohexylcarbonyl-2-(p-toluenesulfonyl)propane and
[0191] 2-isopropylcarbonyl-2-(p-toluenesulfonyl)propane.
[0192] Exemplary disulfone derivatives include diphenyl disulfone and dicyclohexyl disulfone.
[0193] Exemplary nitrobenzyl sulfonate derivatives include:
[0194] 2,6-dinitrobenzyl p-toluenesulfonate and 2,4-dinitrobenzyl p-toluenesulfonate.
[0195] Exemplary sulfonate derivatives include:
[0196] 1,2,3-Tris(methanesulfonyloxy)benzene, 1,2,3-tris(trifluoromethanesulfonyloxy)benzene, and 1,2,3-tris(p-toluenesulfonyloxy)benzene.
[0197] Exemplary imidosulfonate derivatives include:
[0198] Phthalimide trifluoromethanesulfonate, Phthalimide toluenesulfonate, 5-norbornene-2,3-dicarboximido trifluoromethanesulfonate,
[0199] 5-Norbornene-2,3-dicarboximidotoluenesulfonate,
[0200] 5-Norbornene-2,3-dicarboximidobutylsulfonate and
[0201] N-Trifluoromethylsulfonyloxynaphthoimide.
[0202] A typical representative of the sulfonic acid oxime ester derivative is α-(benzenesulfoniumoxyimino)-4-methylphenylacetonitrile.
[0203] Suitable imidosulfonate derivatives include:
[0204] (5-(4-methylphenyl)sulfonyloxyimino-5H-thiophen-2-ylidene)-(2-methylphenyl)-acetonitrile and
[0205] (5-(4-(4-methylphenylsulfonyloxy)phenylsulfonyloxyimino)-5H-thiophen-2-ylidene)-(2-methylphenyl)acetonitrile.
[0206] Examples of triazine derivatives include
[0207] 2-(Methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine,
[0208] 2-[2-(3,4-dimethoxyphenyl)vinyl]-4,6-bis(trichloromethyl)-s-triazine,
[0209] 2-[2-(Furan-2-yl)vinyl]-4,6-bis(trichloromethyl)-s-triazine and
[0210] 2-[2-(5-Methylfuran-2-yl)vinyl]-4,6-bis(trichloromethyl)-s-triazine.
[0211] As the PAG, the onium salts listed above are preferred, and the sulfonium salts listed above are more preferred.
[0212] PAG (B) is preferably used in an amount of 0.05 to 20 parts by weight, more preferably 0.2 to 5 parts by weight, per 100 parts by weight of component (A). As long as the amount of PAG is within this range, sufficient photocuring can be obtained and curing in the form of a thick film is satisfactory. PAG can be used alone or in combination of two or more.
[0213] (E) Organic solvents
[0214] The organic solvent in which the above compounds are soluble or dispersible is preferred. Examples of organic solvents include ketones such as cyclohexanone, cyclopentanone and methyl-2-n-pentyl ketone; and alcohols such as 3-methoxybutanol, 3-methyl-3-methoxybutanol, 1-methoxy-2-propanol and 1-ethoxy-2-propanol; ethers such as propylene glycol monomethyl ether (PGME), ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol dimethyl ether and diethylene glycol dimethyl ether; esters such as propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monoethyl ether acetate, ethyl lactate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, tert-butyl acetate, tert-butyl propionate, propylene glycol monotert-butyl ether acetate and γ-butyrolactone; and amides such as N-methyl-2-pyrrolidone and N,N-dimethylacetamide.
[0215] Among these solvents, PGMEA, PGME, ethyl lactate, cyclohexanone, cyclopentanone, methyl isobutyl ketone, γ-butyrolactone and mixtures thereof are preferred because PAG is most soluble therein.
[0216] Based on the composition, the organic solvent is preferably used in an amount of 20 to 90 wt %, more preferably 30 to 65 wt %. As long as the amount of the organic solvent is within this range, the compound is compatible and the composition can be easily coated. The organic solvent can be used alone or in combination.
[0217] (F) Multifunctional Epoxy Compounds
[0218] The multifunctional epoxy compound (excluding the compound as component (B)) undergoes a crosslinking reaction with component (A) when the resin coating is thermally cured after patterning, thereby contributing to the reliability of the coating and the adhesion of the coating to the substrate.
[0219] Examples of the polyfunctional epoxy compound include glycidyl ether forms of phenols, alicyclic epoxy compounds having a cyclohexene oxide group, and those obtained by introducing an epoxy compound having an unsaturated bond into an organosiloxane having a hydrosilyl group by a hydrosilylation reaction.
[0220] In the glycidyl ether form of phenol, the phenol structure may be of a novolac, bisphenol, biphenyl, phenol aralkyl, dicyclopentadiene, naphthalene or amino-containing type. Suitable glycidyl ether forms of phenol include glycidyl ethers of bisphenol A type, bisphenol AD type and bisphenol F type, glycidyl ethers of hydrogenated bisphenol A, glycidyl ethers of ethylene oxide adduct bisphenol A, glycidyl ethers of propylene oxide adduct bisphenol A, glycidyl ethers of novolac resins, glycidyl ethers of cresol novolac resins, glycidyl ethers of naphthalene resins, glycidyl ethers of dicyclopentadiene phenol type resins and trifunctional epoxy forms of aminophenol.
[0221] The alicyclic epoxy compounds having a cyclohexene oxide group include tetrakis(3,4-epoxycyclohexylmethyl)-modified ε-caprolactone butane tetracarboxylic acid ester and the compounds shown below.
[0222]
[0223] Compounds obtained by introducing an epoxy compound having an unsaturated bond into an organosiloxane having a hydrosilyl group through a hydrosilylation reaction include reaction products obtained by reacting an epoxy compound having an unsaturated bond such as allyl glycidyl ether or vinylcyclohexyl epoxide with an organosiloxane having a hydrosilyl group.
[0224] Illustrative examples of such compounds include epoxy-containing organopolysiloxanes having formula (15), epoxy-containing cyclosiloxanes having formula (16), and bis-silyl-substituted compounds having formula (17).
[0225]
[0226] In equations (15) to (17), R A To R D Each independently is an organic group containing an epoxy group. Preferred examples of the organic group containing an epoxy group include, but are not limited to, an alkyl group containing an epoxy group, such as glycidyloxypropyl and cyclohexyloxyethyl. Among them, glycidyloxypropyl is most preferred as R A To R D .
[0227] In equations (15) to (17), R 81 To R 90 , R 101 To R 103 , R 112 and R 113 Each is independently a C1-C8 monovalent hydrocarbon group. Suitable monovalent hydrocarbon groups are as described above for R in formula (2): 1 To R 6 exemplified.
[0228] In formula (15), R 91 is hydrogen or a C1-C8 alkyl group. Suitable alkyl groups include methyl, ethyl, propyl, butyl, pentyl, hexyl and octyl.
[0229] In formula (15), z 1 To z 6 is at 0≤z 1 ≤10、0≤z 2 ≤10、0≤z 3 ≤30, 0≤z 4 ≤100、0≤z 5 ≤10、0≤z6 ≤20, z 1 +z 3 ≥2, 0.1≤(z 1 +z 3 ) / (z 1 +z 2 +z 3 +z 4 )≤1, and 0≤(z 5 +z 6 ) / (z 1 +z 2 +z 3 +z 4 +z 5 +z 6 ) is an integer in the range of )≤0.05.
[0230] In formula (16), z 11 and z 12 For 2≤z 11 ≤10、0≤z 12 ≤20 and 0.2≤z 11 / (z 11 +z 12 )≤1.
[0231] In formula (17), R 111 C2-C 24 The divalent organic group may be linear, branched or cyclic. Examples include alkane diyls such as ethane diyl, propane diyl and hexane diyl, cycloalkane diyls such as cyclopentane diyl and cyclohexane diyl, divalent aromatic groups such as phenylene and biphenyl diyl, and groups obtained by combining a plurality of such groups.
[0232] In formula (17), z 21 and z 22 Each independently represents an integer from 1 to 3.
[0233] Examples of the epoxy-containing organopolysiloxane having the formula (15) are shown below, but are not limited thereto.
[0234]
[0235] Here, s is preferably an integer of 1-10, and t is preferably an integer of 1-5.
[0236] Examples of the epoxy-containing cyclosiloxane having the formula (16) are shown below, but are not limited thereto.
[0237]
[0238] Examples of the bis-silyl-substituted compound having the formula (17) are shown below, but are not limited thereto.
[0239]
[0240] Here, u is an integer from 2 to 24.
[0241] The polyfunctional epoxy compound is suitably used in an amount of 0.05 to 100 parts by weight, more preferably 0.1 to 50 parts by weight, and even more preferably 1 to 30 parts by weight per 100 parts by weight of component (A). As long as the amount of the polyfunctional epoxy compound is within this range, the composition cures into a film having improved toughness and substrate adhesion. The polyfunctional epoxy compound may be used alone or in combination.
[0242] The photosensitive resin composition of the present invention is advantageously used as, for example, a wiring protection film and an interlayer dielectric film in a semiconductor device, and a photoresist material for micro-processing.
[0243] Photosensitive dry film
[0244] Another embodiment of the present invention is a photosensitive dry film comprising a photosensitive resin coating obtained by processing the photosensitive resin composition into a film form. Since the film form of the photosensitive resin composition is used, a pattern can be obtained without a solvent, which is advantageous from the viewpoint of the working environment. Even when the photosensitive dry film is used, a pattern of the same quality as that of the solution form of the photosensitive resin composition can be obtained.
[0245] The photosensitive dry film may further include a protective film stacked on the photosensitive resin coating layer of the photosensitive resin composition. Described below is an exemplary method of manufacturing the photosensitive dry film in this embodiment.
[0246] The dry film is manufactured by mixing the necessary components to form a photosensitive resin composition solution and applying the solution to the protective film to a desired thickness by a reverse roll coater, a notch wheel coater, etc. The protective film coated with the resin composition solution is passed through an online dryer, where it is dried by heating at 30 to 160° C. for 2 to 20 minutes to remove the organic solvent. Next, the coated protective film is press-bonded or laminated to another protective film by a roll laminator to obtain a laminate having a resin film between the protective films.
[0247] When the photosensitive resin composition is preformed into a film form, the thickness is not particularly limited. The thickness of the resin film is preferably 1 to 120 μm, more preferably 2 to 100 μm, and even more preferably 3 to 85 μm. Within this range, a resin film with minimal thickness variation and easy patterning can be obtained.
[0248] There is no particular restriction on the protective film, as long as it can be peeled off or peeled off from the resin film of the resin composition of the present invention without deforming its shape. The protective film is generally used as a protective film or a demoulding film of a wafer, and includes a plastic film that has undergone a demoulding process, such as a polyethylene (PE) film, a polypropylene (PP) film, a polymethylpentene (TPX) film, and a polyester film. Preferably, the stripping force or peeling force of 50 to 300 mN / min. The protective film preferably has a thickness of 25 to 150 μm, more preferably 38 to 125 μm.
[0249] By using a photosensitive dry film, the wafer can be packaged or sealed. The packaging method is not particularly limited, and includes the following steps: peeling a protective layer from a resin film; setting a vacuum chamber of a vacuum laminator (e.g., TEAM-300 of Takatori Corp.) to a vacuum degree of 50 to 1,000 Pa, preferably 50 to 500 Pa, and typically 100 Pa, tightly bonding the resin film having an additional protective layer to the wafer at a temperature of 30 to 130° C., preferably 50 to 120° C., and typically 100° C., restoring atmospheric pressure, cooling the wafer to room temperature, taking the wafer out of the laminator, and then peeling off the additional protective layer.
[0250] Patterning method
[0251] Another embodiment of the present invention is a method for forming a pattern using the photosensitive resin composition defined above, the method comprising the steps of: (i) forming a photosensitive resin coating of the photosensitive resin composition on a substrate, (ii) exposing the photosensitive resin coating to radiation; and (iii) developing the exposed resin coating with a developer.
[0252] In step (i), a photosensitive resin coating is formed on a substrate using a photosensitive resin composition. Examples of substrates used herein include silicon, glass and quartz wafers, silicon nitride substrates, silicon oxide substrates, plastic substrates such as paper phenol, glass-reinforced epoxy and polyimide substrates, ceramic-based circuit boards, and substrates having a resin film on their surfaces. On these substrates, a metal film may be deposited, a wiring pattern may be printed, or a photosensitive resin coating of the same or different type may be formed.
[0253] One method of forming the photosensitive resin coating is to apply a solution of the photosensitive resin composition in an organic solvent by any technique such as dip coating, spin coating or roller coating. The coating weight can be appropriately selected for a particular purpose, preferably to form a photosensitive resin coating having a thickness of 0.1 to 300 μm.
[0254] Another method of forming a photosensitive resin coating is to adhere a photosensitive dry film to a substrate. To this end, a vacuum diaphragm laminator (Nikko Material Co., Ltd. trade name V-130) can be used under the following conditions: a lamination temperature of 30 to 130° C., a vacuum of 50 to 500 Pa, a pressure of 0.1 to 0.9 MPa, and a lamination time of 15 to 300 seconds.
[0255] Once the photosensitive resin coating is formed on the substrate, the coating may be prebaked to volatilize the solvent, etc., if necessary, to allow for an effective photocuring reaction. The prebaking may be performed, for example, at 40 to 140° C. for 1 minute to about 1 hour.
[0256] Next, in step (ii), the photosensitive resin coating is exposed to radiation preferably having a wavelength of 240 to 500 nm to cure. Exposure can be performed through a photomask. The photomask can be, for example, a photomask perforated with a desired pattern. Although there is no particular restriction on the material of the photomask, it is preferred that the material be capable of shielding radiation within the above-mentioned wavelength range. Although not limited thereto, a mask having a chromium light shielding film is generally used.
[0257] Examples of radiation having a wavelength of 240 to 500 nm include radiation of various wavelengths from a radiation emitting unit, particularly UV radiation such as g-line or i-line and deep UV (248 nm). Suitable exposure doses are 10 to 5,000 mJ / cm 2 The next step may be a post-exposure bake (PEB) to effectively increase the developing sensitivity. PEB may be performed at 40 to 150° C. for 0.5 to 10 minutes, for example.
[0258] Exposure or PEB is followed by a step (iii) of developing the exposed resin coating with a developer. Preferred examples of the developer include organic solvents used as solvents, such as dimethylacetamide and cyclohexanone, and alkaline aqueous solutions, such as aqueous solutions of tetramethylammonium hydroxide (TMAH) and sodium carbonate. Development is carried out in a conventional manner, for example, by immersing the exposed coating in a developer. After development, washing, rinsing and drying are performed as necessary. In this way, a resin coating having a desired pattern is obtained. Although the pattern forming method has been described, it is sometimes not necessary to form a pattern. For example, when only a uniform film needs to be formed, the same process as above can be carried out except that a photomask is not used.
[0259] After the development step, the patterned coating may be heated in an oven or hot plate at a temperature of 70 to 380° C., preferably 80 to 300° C., for about 10 minutes to about 10 hours to increase the crosslinking density and remove any remaining volatile materials. As a result, a cured resin coating having improved adhesion to the substrate, heat resistance, mechanical strength, and good electrical properties is obtained.
[0260] The cured coating thus obtained has enhanced adhesion to substrates, copper wiring and resist films. The cured coating passes migration tests because the hygroscopicity remains unchanged, and the risk of precipitation is eliminated because it is introduced into the curing system. Due to these characteristics, the cured coating is most suitable for use as a material for electronic devices.
[0261] Example
[0262] Examples of the present invention are given below by way of illustration and not limitation. It is worth noting that the weight average molecular weight (Mw) was measured relative to polystyrene standards by GPC using tetrahydrofuran (THF) solvent. 1 The composition of the resin was analyzed by H-NMR spectroscopy.
[0263] Compounds (S-1) to (S-6) and (R-1) to (R-7) used in Examples are shown below.
[0264]
[0265]
[0266] Examples 1 to 6
[0267] A 5-liter separable flask equipped with a reflux condenser, a thermometer, and a dropping funnel was charged with 2,000 g of toluene and each of the compounds (S-1) to (S-6) as reactants in the amounts shown in Table 1. Then, nitric acid, sulfuric acid, or phosphoric acid in the amounts shown in Table 1 was added dropwise from the dropping funnel to the flask over 2 hours. After the addition, the solution was heated at 80° C. and maintained for 2 hours. Finally, the solvent and unreacted compounds were removed from the reaction solution by vacuum distillation to obtain compounds (G-1) to (G-6) as epoxy additives.
[0268] Table 1
[0269]
[0270] Compounds (G-1) to (G-6) have the following structures.
[0271]
[0272] Here, the dotted line represents the valence bond to the oxygen atom.
[0273]
[0274] Here, the dotted line represents the valence bond to the oxygen atom.
[0275]
[0276] Here, N A As defined above, the dashed lines represent valence bonds to the oxygen atoms.
[0277]
[0278] Here, N B As defined above, the dashed lines represent valence bonds to the oxygen atoms.
[0279] Resin Synthesis Example 1
[0280] A 3-L flask equipped with a stirrer, a thermometer, a nitrogen purge line and a reflux condenser was charged with 271.1 g (0.50 mol) of compound (R-1), 215.1 g (0.50 mol) of compound (R-3) and 1,500 g of toluene and heated at 70°C. Thereafter, 1.0 g of a toluene solution of chloroplatinic acid (platinum concentration of 0.5 wt%) was added, and 194.1 g (1.00 mol) of compound (R-2) was added dropwise over 1 hour. At the end of the addition, the reaction solution was heated at 100°C and aged for 6 hours. Toluene was distilled off from the reaction solution in a vacuum to obtain 590 g of resin 1. Resin 1 had an Mw of 38,800.
[0281]
[0282] Resin Synthesis Example 2
[0283] A 3-L flask equipped with a stirrer, a thermometer, a nitrogen purge line and a reflux condenser was charged with 81.3 g (0.15 mol) of compound (R-1), 64.5 g (0.15 mol) of compound (R-3) and 1,500 g of toluene and heated at 70°C. Thereafter, 1.0 g of a toluene solution of chloroplatinic acid (platinum concentration of 0.5 wt%) was added, and 29.1 g (0.15 mol) of compound (R-2) and 442.0 g (0.15 mol) of compound (R-4) were added dropwise over 1 hour. At the end of the addition, the reaction solution was heated at 100°C and aged for 6 hours. Toluene was distilled off from the reaction solution under vacuum to obtain 2570 g of resin 2. Resin 2 has an Mw of 40400.
[0284]
[0285] Resin Synthesis Example 3
[0286] A flask equipped with a stirrer, a thermometer and a nitrogen purge line was charged with 264.0 g (0.25 mol) of compound (R-5), 183.1 g (0.50 mol) of compound (R-6) and 1,400 g of γ-butyrolactone. Then 111.1 g (0.25 mol) of compound (R-7) was added to the flask, and the temperature of the reaction system was controlled not to exceed 50 ° C. After that, 2.2 g (0.02 mol) of p-aminophenol was added to the solution, which was stirred at room temperature for 10 hours. The flask was equipped with a reflux condenser with a water pipe joint, and 250 g of xylene was added. The solution was heated at 170 ° C and maintained at this temperature for 6 hours to obtain a brown solution. Then 60.2 g (0.80 mol) of glycidol was added to the solution, and the solution was heated at 110 ° C for 3 hours. At the end of the reaction, the reaction solution was cooled to room temperature and poured into methanol. The resulting precipitate was filtered and dried to obtain Resin 3. Resin 3 had an Mw of 36,700.
[0287]
[0288] Patterning assay
[0289] A resin solution was prepared by combining the components according to the formulations shown in Tables 2, 3 and 4, stirring and mixing them. The resin solution was spin-coated on a silicon wafer to form a 10 μm thick resin layer.
[0290] In Examples 1 to 9, 13 to 20 and Comparative Examples 1 to 11, the resin layer was heated on a hot plate at 90° C. for 2 minutes to volatilize the solvent, exposed to radiation with a wavelength of 365 nm through a mask having a 20-μm through-hole pattern, baked (PEB) on a hot plate at 90° C. for 4 minutes, developed 4 times for 60 seconds in a 2.38 wt % TMAH aqueous solution as a developer, and then heated at 200° C. for 2 hours to cure.
[0291] In Examples 10 to 12 using polyimide PIMEL, the resin layer was exposed to radiation with a wavelength of 365 nm through a mask having a 20-μm through-hole pattern, developed 4 times for 60 seconds in a 2.38 wt % TMAH aqueous solution as a developer, and heated at 350° C. for 2 hours for curing.
[0292] The cross section of the pattern was observed under SEM. The sample was rated as "OK" when the resin was removed up to the bottom, and "NG" when any resin residue was found at the bottom.
[0293] Wafer shear test
[0294] The resin solution prepared as described above was spin-coated onto the silicon wafer on which copper was evaporated to form a 10 μm-thick resin layer.
[0295] In Examples 1 to 9, 13 to 20 and Comparative Examples 1 to 11, the resin layer was heated on a hot plate at 90° C. for 2 minutes to volatilize the solvent, exposed to radiation of a wavelength of 365 nm through a mask having a 100 μm square column pattern, baked (PEB) on a hot plate at 90° C. for 4 minutes, developed 4 times for 60 seconds in a 2.38 wt % TMAH aqueous solution as a developer, and then heated at 200° C. for 2 hours to cure.
[0296] In Examples 10 to 12 using polyimide PIMEL, the resin layer was exposed to radiation with a wavelength of 365 nm through a mask having a 100 μm square columnar pattern, developed 4 times for 60 seconds in a 2.38 wt % TMAH aqueous solution as a developer, and heated at 350° C. for 2 hours for curing.
[0297] The resulting 100-μm square columnar pattern was examined by a wafer shear test using a bonding force measurement system (Multi-function Adhesion Tester 4000 Series, DS-100 from Nordson Advanced Technology) The bonding force when the columnar pattern was flipped laterally was measured.
[0298] Migration assay
[0299] The resin solution prepared as described above was spin-coated onto the SiN wafer having the comb-shaped copper wiring thereon to form a 10 μm-thick resin layer.
[0300] In Examples 1 to 9, 13 to 20 and Comparative Examples 1 to 11, the resin layer was heated on a hot plate at 90° C. for 2 minutes to volatilize the solvent, the entire sheet was exposed to radiation with a wavelength of 365 nm without using a mask, baked (PEB) on a hot plate at 90° C. for 4 minutes, developed 4 times for 60 seconds in a 2.38 wt % TMAH aqueous solution as a developer, and then heated at 200° C. for 2 hours to cure.
[0301] In Examples 10 to 12 using polyimide PIMEL, the resin layer was exposed to radiation having a wavelength of 365 nm without using a mask, developed 4 times for 60 seconds in a 2.38 wt % TMAH aqueous solution as a developer, and heated at 350° C. for 2 hours for curing.
[0302] The cured product was subjected to a migration test by applying a voltage of 20 V for 1,000 hours in an environment of 85°C and 85% humidity. The sample was rated "OK" when no conduction occurred until the end of the test, and "NG" when conduction occurred during the test.
[0303] The components in Tables 2, 3 and 4 are shown below.
[0304] PIMEL: Photosensitive polyimide manufactured by Asahi Kasei Microdevices Corp. 18320.
[0305] Crosslinker: Tetrakis(methoxymethyl)glycoluril ( MX-270, manufactured by Sanwa Chemical Co., Ltd.)
[0306]
[0307] PAG: (p-Toluenesulfonyloxyimino)-p-methoxyphenylacetonitrile
[0308]
[0309] Solvent: Cyclopentanone
[0310] Table 2
[0311]
[0312] Table 3
[0313]
[0314] Table 4
[0315]
[0316] It has been demonstrated that the resin composition within the scope of the present invention exhibits better bonding than the comparative composition and gives satisfactory results in the pattern forming test and the migration test. The resin composition of the present invention has satisfactory characteristics as a photosensitive material.
[0317] Japanese Patent Application No. 2018-206503 is incorporated herein by reference.
[0318] Although some preferred embodiments have been described, many modifications and variations are possible in light of the above teachings. It is therefore to be understood that the invention may be practiced other than as specifically described without departing from the scope of the appended claims.
Claims
1. A photosensitive resin composition comprising (A) a resin having a phenolic hydroxyl group, and (B) an epoxy additive in the form of a compound having 1 to 8 epoxy groups per molecule, containing at least one element selected from nitrogen, sulfur and phosphorus and having a molecular weight of 50 to 6,000, The epoxy additive (B) is present in an amount of 0.1 to 18 parts by weight per 100 parts by weight of the resin (A), The epoxy additive (B) is a compound having the formula (9), X A m -X B (9) X A is a group selected from the following formulae, in, The dotted line represents the B Bonded valence bond, R a To R e Each is independently a C1-C6 monovalent hydrocarbon group, E 1 and E 2 Each independently is C1-C 12 Divalent hydrocarbon group, subscript m 1 、m 2 and m 3 are each independently an integer from 0 to 3, j 1 is an integer from 0 to 7, j 2 is an integer from 1 to 8, j 3 is an integer from 1 to 3, X B Selected from the group represented by the following formula:
2. The composition according to claim 1, wherein The resin (A) is at least one selected from the group consisting of polybenzoxazole, polyimide, epoxy resin, silicone-modified polybenzoxazole, silicone-modified polyimide, and silicone-modified epoxy resin. The composition according to claim 1 , further comprising (C) a cross-linking agent. The composition according to claim 1 , further comprising (D) a photoacid generator. The composition according to claim 1 , further comprising (E) an organic solvent. 6 . A photosensitive resin coating obtained from the photosensitive resin composition according to claim 1 .
7. A photosensitive dry film comprising the photosensitive resin coating according to claim 6.
8. A pattern forming method comprising the following steps: (i) forming a photosensitive resin coating on a substrate using the photosensitive resin composition according to claim 1, (ii) exposing the photosensitive resin coating to radiation, and (iii) The exposed photosensitive resin coating is developed using a developer.
9. A pattern forming method comprising the following steps: (i) forming a photosensitive resin coating on a substrate using the photosensitive dry film according to claim 7, (ii) exposing the photosensitive resin coating to radiation, and (iii) The exposed photosensitive resin coating is developed using a developer.
Citation Information
Patent Citations
Illumination structure
JP2018206503A
Positive photosensitive resin composition, photo-curable dry film and method for producing the same, patterning process, and laminate
EP3214497A1
Photo-curable resin composition, pattern forming method and substrate protecting film, and film-shaped adhesive and adhesive sheet using said composition
TW201136997A
Chemically amplified negative resist composition, photo-curable dry film, making method, pattern forming process, and electric / electronic part protecting film
TW201337462A