Metal-clad laminate for flexible circuit substrate and flexible circuit substrate

By controlling the storage elastic coefficient and introducing specific functional groups in the polyimide layer, the foaming problem caused by high-temperature heat treatment in the casting method is solved, and the quality and reliability of the metal-clad laminated plate and the circuit substrate are improved.

CN111385967BActive Publication Date: 2024-11-05NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201911189866.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-12-26
Filing Date
2019-11-28
Publication Date
2024-11-05
Estimated Expiration
2039-11-28

AI Technical Summary

Technical Problem

When forming a polyimide layer by casting, the foaming phenomenon caused by high-temperature heat treatment reduces the yield and reliability of the metal-clad laminated plate and circuit substrate. It is difficult for the prior art to simultaneously improve the polyimide layer and the metal layer. and elastic coefficients to suppress foaming.

Method used

By controlling the storage elastic coefficient in the polyimide layer and including specific functional groups, the resin component interaction between the polyimide layer is used to improve the adhesion and interface of the polyimide layer and the metal layer, ensuring that Internal pressure stability at high temperature.

Benefits of technology

The damage to the polyimide layer caused by the rise of internal pressure at high temperature is effectively suppressed, and the manufacturing yield and reliability of the metal-clad laminated plate and circuit substrate are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0005049125840000011
    Figure FDA0005049125840000011
  • Figure FDA0005049125840000021
    Figure FDA0005049125840000021
  • Figure FDA0005049125840000022
    Figure FDA0005049125840000022
Patent Text Reader

Abstract

The present invention provides a metal-clad laminate and a circuit board, which suppress foaming caused by heat treatment at high temperature by controlling the elastic coefficient of a polyimide layer in contact with a metal layer to be high and ensuring the close contact of the interface with the adjacent polyimide layer. The metal-clad laminate comprises an insulating resin layer, a metal layer laminated on one or both sides of the insulating resin layer, and a polyimide layer (A) in contact with the metal layer having a storage elastic coefficient E' at 300°C measured by a dynamic viscoelasticity measuring device (DMA) of 1.0×10 8 Pa or more, and the storage elastic coefficient E' at 350°C is 1.0×10 7 Pa or more, the polyimide constituting the polyimide layer (A) contains 40 mol parts or more of acid anhydride residues derived from tetracarboxylic dianhydride having a keto group (-CO-) in the molecule, relative to a total of 100 mol parts of acid anhydride residues.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a metal-clad laminate used in the field of electronic materials, for example, to form a circuit substrate, and a circuit substrate obtained by processing the metal-clad laminate. Background Art

[0002] In recent years, with the progress of miniaturization, lightness and space saving of electronic devices, the demand for flexible printed circuits (FPC) that are thin, light, flexible and have excellent durability even after repeated bending has increased. Since FPC can be installed three-dimensionally and at a high density even in a limited space, its use is expanding in wiring, cables, connectors and other parts of electronic devices such as hard disk drives (HDD), digital versatile discs (DVD), mobile phones and smartphones. As an insulating resin used in FPC, polyimide with excellent heat resistance or adhesion has attracted much attention.

[0003] The metal-clad laminate used in the manufacture of FPC is a laminate of a metal layer and an insulating resin. It can be processed into a fine circuit and can be bent in a narrow space. Therefore, its application is increasing with the miniaturization and weight reduction of electronic devices.

[0004] As a method for manufacturing a metal-clad laminate, the following manufacturing method (casting method) is known, i.e., a laminate prepared by repeatedly applying a polyamic acid solution to a metal foil and drying it is heat-treated at a high temperature and imidized to form a polyimide layer. In the casting method, since the heat treatment is performed at a temperature exceeding the boiling point of the solvent, depending on the dry state of the polyamic acid layer or the amount of residual solvent, between the metal foil and the polyimide layer in contact with it, or between the polyimide layer in contact with the metal foil and the adjacent polyimide layer, sometimes there is a phenomenon such as bulge or peeling, foaming caused by the volume expansion of the vaporized solvent or the water (imidized water) produced by imidization (hereinafter, these phenomena are sometimes collectively referred to and recorded as "foaming") .

[0005] As a prior art for manufacturing a polyimide layer by casting, Patent Document 1 discloses that a polyimide layer having a storage elastic coefficient of 1×10 at 300° C. is provided on the polyimide layer in contact with the metal layer. 8 Pa, the storage elastic coefficient at 350°C is 1×10 8 Thermoplastic polyimide layer with a molecular weight of Pa or less. However, in the combination of monomers used in Patent Document 1, the elastic modulus of the thermoplastic polyimide resin layer is too low at high temperatures, so there is a concern that foaming may occur between the polyimide layers during heat treatment.

[0006] In addition, Patent Document 2 proposes that the polyimide layer in contact with the metal foil is a high elastic resin layer comprising a polyimide made of pyromellitic dianhydride and 2,2-bis[4-(4-aminophenoxy)phenyl]propane (2,2-Bis[4-(4-aminophenoxy)phenyl]propane, BAPP), and having a storage elastic coefficient of 1×10 at 350°C. 8 Pa~2×10 9 Pa, and the glass transition temperature is 300℃~400℃.

[0007] Furthermore, Patent Document 3 proposes using 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) in a polyimide layer in contact with a copper foil in order to improve adhesion reliability with the copper foil and reduce dielectric loss tangent in a high frequency region.

[0008] [Prior art literature]

[0009] [Patent Document]

[0010] [Patent Document 1] Japanese Patent Publication No. 2015-515402

[0011] [Patent Document 2] Japanese Patent Application Publication No. 2006-51800

[0012] [Patent Document 3] Japanese Patent No. 5031639 Summary of the invention

[0013] [Problems to be solved by the invention]

[0014] As described above, when a polyimide layer is formed by casting, foaming may occur between layers due to heat treatment at high temperature depending on the drying state of the polyamic acid layer or the amount of residual solvent, which may reduce the yield and reliability of the metal-clad laminate and the circuit board using the same.

[0015] According to the findings obtained by the present inventors, in order to effectively suppress foaming during heat treatment, it is effective to

[0016] i) improving the adhesion between the polyimide layer in contact with the metal layer and the adjacent polyimide layer, ii) improving the adhesion between the polyimide layer in contact with the metal layer and the metal layer,

[0017] iii) increasing the elastic modulus of the polyimide layer in contact with the metal layer. If all of i) to iii) are not satisfied, it is considered that the suppression of foaming becomes insufficient.

[0018] However, in the prior art, the above i) to iii) have not been studied simultaneously, and in particular, there is no technical idea to achieve the suppression of foaming from the viewpoints of the above i) and iii).

[0019] In order to achieve the above i) and ii), it is considered effective to use 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) as the main diamine compound for forming the polyimide layer in contact with the metal layer in the prior art. However, if the diamine compound is used in large amounts, the heat resistance of the polyimide layer in contact with the metal layer decreases, making it difficult to achieve the above iii).

[0020] Furthermore, the above iii) is to suppress the destruction of the polyimide layer due to the increase in internal pressure at high temperature by increasing the elastic modulus. However, if the elastic modulus is increased too much, the adhesion of the interface with the adjacent polyimide layer tends to decrease, making it difficult to achieve the problem of i).

[0021] Therefore, an object of the present invention is to provide a metal-clad laminate which suppresses foaming caused by heat treatment at high temperature by controlling the elastic modulus of a polyimide layer in contact with a metal layer to be high and ensuring the adhesion of the interface with an adjacent polyimide layer.

[0022] [Technical means to solve the problem]

[0023] As a result of diligent research, it was found that the polyimide layer in contact with the metal layer is formed by a polyimide having a specific functional group, and the interaction of the resin components between the polyimide layers is utilized. As a result, it was found that even if the elastic coefficient of the polyimide layer in contact with the metal layer is increased, the adhesion of the interface with the adjacent polyimide layer can be ensured by the interaction, and the above i) to iii) can be achieved at the same time, and foaming can be effectively suppressed, thereby completing the present invention.

[0024] That is, the metal-clad laminate of the present invention includes an insulating resin layer and a metal layer laminated on one or both surfaces of the insulating resin layer.

[0025] The insulating resin layer includes a plurality of polyimide layers including a polyimide layer (A) in contact with the metal layer.

[0026] In the metal-clad laminate of the present invention, the storage elastic coefficient E' of the polyimide layer (A) at 300°C measured using a dynamic viscoelasticity measuring device (DMA (dynamic mechanical analyzer)) is 1.0×10 8 Pa or more, and the storage elastic coefficient E' at 350°C is 1.0×10 7 Pa or above.

[0027] In addition, the polyimide constituting the polyimide layer (A) in the metal-clad laminate of the present invention contains anhydride residues derived from a tetracarboxylic dianhydride component and diamine residues derived from a diamine component, and contains 40 mol parts or more of anhydride residues derived from a tetracarboxylic dianhydride having a keto group (-CO-) in the molecule, relative to a total of 100 mol parts of the anhydride residues.

[0028] Furthermore, the circuit board of the present invention comprises an insulating resin layer and a metal wiring layer laminated on one or both surfaces of the insulating resin layer.

[0029] The insulating resin layer includes a plurality of polyimide layers including a polyimide layer (A) in contact with the metal wiring layer.

[0030] In the circuit board of the present invention, the storage elastic coefficient E' of the polyimide layer (A) at 300°C measured using a dynamic viscoelasticity measuring device (DMA) is 1.0×10 8 Pa or more, and the storage elastic coefficient E' at 350°C is 1.0×10 7 Pa or above.

[0031] In addition, the polyimide constituting the polyimide layer (A) in the circuit substrate of the present invention contains an anhydride residue derived from a tetracarboxylic dianhydride component and a diamine residue derived from a diamine component, and contains 40 mol parts or more of an anhydride residue derived from a tetracarboxylic dianhydride having a keto group (-CO-) in the molecule, relative to a total of 100 mol parts of the anhydride residues.

[0032] In the metal-clad laminate and the circuit board of the present invention, the polyimide constituting the polyimide layer (A) can be represented by a structural unit represented by the following general formula (1).

[0033] [Chemistry 1]

[0034]

[0035] In the general formula (1), Ar is a tetravalent acid anhydride residue derived from an aromatic tetracarboxylic acid anhydride, and R 1 It refers to a divalent diamine residue derived from a diamine compound.

[0036] Furthermore, in the metal-clad laminate and the circuit board of the present invention, the AP value calculated based on the following mathematical formula (i) and serving as an index representing the amount of polar groups contained in the polyimide can be 1.60 or less.

[0037] AP value={(A1+A2+A3) / (B1+B2+B3)}×100···(i)

[0038] [Here,

[0039] A1 = (the number of polar groups in the group Ar) x (the number of moles of the group Ar)

[0040] A2=(base R 1 The number of polar groups in the 1 Number of moles)

[0041] A3 = (number of imide groups) × (number of moles of imide groups)

[0042] B1 = (molecular weight of group Ar) x (number of moles of group Ar)

[0043] B2=(base R 1 molecular weight)×(base R 1 Number of moles)

[0044] B3 = (molecular weight of imide group) × (number of moles of imide group), with respect to the number of the polar groups,

[0045] -X (where X is a halogen atom), -OH, -SH, -O-,

[0046] -S-, -SO-, -NH-, -CO-, -CN, -P=O,

[0047] -PO- is set to 1,

[0048] -SO 2 -, -CONH- are set to 2,

[0049] -SO 3 H, -(CO) 2 N-set to 3 for calculation]

[0050] In the metal-clad laminate and the circuit board of the present invention, the peel strength between the metal layer or the metal wiring layer and the insulating resin layer may be 0.7 kN / m or more.

[0051] In the metal-clad laminate and circuit board of the present invention, the polyimide constituting the polyimide layer (A) may contain 50 to 100 mol parts of diamine residues derived from a diamine compound represented by the following general formula (D1), based on 100 mol parts in total of the diamine residues.

[0052] [Chemistry 2]

[0053]

[0054] [Effects of the Invention]

[0055] The polyimide layer (A) in contact with the metal layer in the metal-clad laminate of the present invention is composed of a polyimide having a high storage elastic coefficient and contains a predetermined amount of anhydride residue derived from a tetracarboxylic dianhydride having a keto group (-CO-) in the molecule, so that the metal-clad laminate has excellent adhesion to the adjacently laminated polyimide layer and can effectively suppress foaming. Therefore, the metal-clad laminate of the present invention can improve the yield or reliability in the manufacture of a circuit substrate such as an FPC using the metal-clad laminate. DETAILED DESCRIPTION

[0056] Hereinafter, embodiments of the present invention will be described in detail.

[0057] [Metal-clad laminate]

[0058] The metal-clad laminate of the present embodiment includes an insulating resin layer and a metal layer laminated on one or both sides of the insulating resin layer. The insulating resin layer has a plurality of polyimide layers including a polyimide layer (A) in contact with the metal layer. The insulating resin layer preferably includes a polyimide layer (X) as a main layer in addition to the polyimide layer (A), and more preferably the polyimide layer (A) is adjacently laminated on one or both sides of the main polyimide layer (X). In addition, the polyimide layer (A) is preferably provided on both sides of the polyimide layer (X).

[0059] Furthermore, in the present invention, the so-called polyimide refers to a heat-resistant resin containing a polymer having an imide group in the structure, such as polyimide, polyamide-imide, polybenzimidazole, polyimide ester, polyetherimide, polysiloxane imide, etc. In addition, the polyimide may be a homopolymer or a copolymer, and in the case of a copolymer, it may be a block copolymer or a random copolymer.

[0060] [Polyimide layer (A)]

[0061] The polyimide layer (A) is a highly elastic and heat-resistant resin layer, and the storage elastic coefficient E' measured at 300°C using a dynamic viscoelasticity measuring device (DMA) is 1.0×10 8 Pa or more, and the storage elastic coefficient E' at 350°C is 1.0×10 7 Pa or above.

[0062] By controlling the storage elastic coefficient E' of the polyimide layer (A) to be high as described above, even if volume expansion occurs due to vaporization of the solvent or imidization water during heat treatment, sufficient strength to withstand the increase in internal pressure between the polyimide layer (X) and the polyimide layer (A) can be maintained, thereby effectively suppressing foaming.

[0063] On the other hand, the storage elastic coefficient E' at 300°C is less than 1×10 8Pa, or the storage elastic coefficient E' at 350°C is less than 1×10 7 Pa, since the strength of the polyimide layer (A) is reduced, the polyimide layer (A) is easily broken due to the increase in internal pressure during heat treatment, and it is difficult to suppress foaming. From this point of view, the storage elastic coefficient E' of the polyimide layer (A) at 300°C is preferably 1×10 8 Pa~3×10 9 Pa. In addition, the storage elastic coefficient E' of the polyimide layer (A) at 350°C is preferably greater than 1×10 8 Pa and 1×10 9 Within the range below Pa.

[0064] As described above, in the polyimide layer (A), the storage elastic coefficient E' at two temperatures of 300° C. and 350° C. is controlled to achieve high elasticity and high heat resistance, thereby effectively suppressing foaming.

[0065] In addition, the glass transition temperature (Tg) of the polyimide constituting the polyimide layer (A) is preferably 250°C or more, more preferably in the range of 280°C to 350°C. In addition, by increasing the Tg of the polyimide layer (A), it is not easy to break during heat treatment, and foaming can be suppressed. When Tg is less than 250°C, the heat resistance of the polyimide layer (A) decreases, so it is difficult to suppress foaming. On the other hand, if Tg exceeds 350°C, it is sometimes impossible to obtain good adhesion between the polyimide layer (A) and the metal layer.

[0066] The coefficient of thermal expansion (CTE) of the polyimide layer (A) is not particularly limited, but is preferably within a range of 0 ppm / K to 100 ppm / K, and more preferably within a range of 5 ppm / K to 80 ppm / K, for example.

[0067] The polyimide constituting the polyimide layer (A) contains an anhydride residue derived from an anhydride component and a diamine residue derived from a diamine component. Polyimide is generally produced by reacting an anhydride component with a diamine component, so by describing the anhydride and diamine compounds, a specific example of polyimide can be understood. Hereinafter, the preferred polyimide for constituting the polyimide layer (A) will be described using anhydrides and diamine compounds. Furthermore, in the present invention, the hydrogen atoms in the two amino groups at the end of the "diamine component" or "diamine compound" may be substituted, for example, -NR 2 R 3 (Here, R 2 , R 3 "independently" refers to any substituent such as an alkyl group).

[0068] <Anhydride residue>

[0069] In order to improve the adhesion with the adjacently laminated polyimide layer (X) and suppress foaming, the polyimide constituting the polyimide layer (A) contains 40 mol parts or more of anhydride residues derived from tetracarboxylic dianhydride having a keto group (-CO-) in the molecule (hereinafter sometimes referred to as "ketone group-containing residues") relative to 100 mol parts of all the anhydride residues. By making the structural unit formed by the ketone group-containing residues abundant in the polyimide layer (A), the adhesion between the polyimide layer (A) and the polyimide layer (X) can be improved by the interaction between the ketone group in the polyimide layer (A) and the functional group contained in the adjacently laminated polyimide layer (X).

[0070] Here, examples of the tetracarboxylic dianhydride having a keto group (—CO—) in the molecule include 3,3′,4,4′-benzophenone tetracarboxylic dianhydride (BTDA), 2,3′,3,4′-benzophenone tetracarboxylic dianhydride, 2,2′,3,3′-benzophenone tetracarboxylic dianhydride, 4,4′-(terephthaloyl)diphthalic anhydride, and 4,4′-(isophthaloyl)diphthalic anhydride. Among these, 3,3′,4,4′-benzophenone tetracarboxylic dianhydride (BTDA), 2,3′,3,4′-benzophenone tetracarboxylic dianhydride, and 2,2′,3,3′-benzophenone tetracarboxylic dianhydride are preferred.

[0071] The functional group having the property of interacting with the keto group is not particularly limited as long as it is a functional group that can generate physical interaction, such as by intermolecular force, or chemical interaction, such as by covalent bond, with the keto group. Representative examples thereof include amino group (-NH 2 ).

[0072] From the above viewpoints, the polyimide constituting the polyimide layer (A) contains 40 mol parts or more of ketone group-containing residues, preferably 50 mol parts to 100 mol parts, and most preferably 75 mol parts to 100 mol parts, relative to a total of 100 mol parts of all acid anhydride residues. When the ketone group-containing residues are less than 40 mol parts, the adhesion improvement effect generated by the interaction with the functional groups contained in the adjacently laminated polyimide layer (X) is insufficient, and therefore it is difficult to suppress foaming.

[0073] The polyimide constituting the polyimide layer (A) may contain an anhydride residue derived from an anhydride component generally used for the synthesis of polyimide as an anhydride residue other than the above. Such anhydride residues are not limited, but are preferably aromatic tetracarboxylic acid residues. In particular, in order to control the storage elastic coefficient E' within the range to suppress foaming, it is preferred to contain a tetravalent anhydride residue (hereinafter, sometimes referred to as "PMDA residue") derived from pyromellitic dianhydride (PMDA). By including a structural unit formed by a PMDA residue in the polyimide, the storage elastic coefficient and Tg of the polyimide layer (A) can be improved.

[0074] With regard to the above viewpoint, relative to the total 100 parts by mole of all anhydride residues, the polyimide constituting the polyimide layer (A) preferably contains PMDA residues in an amount below 25 parts by mole, more preferably contains PMDA residues in the range of 5 parts by mole to 25 parts by mole. When PMDA residue is less than 5 parts by mole, it is difficult to obtain the effect brought by PMDA residues.

[0075] <Diamine residue>

[0076] The polyimide constituting the polyimide layer (A) is not particularly limited, but preferably contains a diamine residue derived from a diamine compound represented by the following general formula (D1) (hereinafter sometimes referred to as "D1 residue") in order to increase Tg and control the storage elastic coefficient E' at 300°C and 350°C within the above range.

[0077] [Chemistry 3]

[0078]

[0079] Preferred specific examples of the diamine compound represented by the general formula (D1) include diamine compounds such as 1,3-bis(3-aminophenoxy)benzene (APB), 1,3-bis(4-aminophenoxy)benzene (TPE-R), and 1,4-bis(4-aminophenoxy)benzene (TPE-Q). These diamine compounds are aromatic diamines having three benzene rings. Due to the two ether bonds (-O-) directly bonded to the central benzene ring, the degree of freedom of the polyimide molecular chain is increased, and the polyimide molecular chain has high flexibility, thereby improving the flexibility of the polyimide molecular chain, increasing Tg, and increasing the storage elastic coefficient E' at high temperature. From this viewpoint, among the diamine compounds represented by General Formula (D1), a compound in which two ether bonds (—O—) directly bonded to the central benzene ring are located at meta-positions to each other is more preferred.

[0080] Therefore, it is believed that the polyimide constituting the polyimide layer (A) contains a specified amount of D1 residues to form a structural unit combined with a ketone-containing residue, and the storage elastic coefficient E' at 300°C and 350°C is easily controlled within the range, and the heat resistance is maintained, the adhesion to the metal layer is improved, and the peel strength is improved. In addition, the dielectric properties (dielectric constant and dielectric loss tangent) of the polyimide layer (A) are achieved by containing a specified amount of D1 residues. From this point of view, the polyimide constituting the polyimide layer (A) preferably contains D1 residues in the range of 50 to 100 molar parts relative to a total of 100 molar parts of all diamine residues, and more preferably contains D1 residues in the range of 75 to 100 molar parts.

[0081] The polyimide constituting the polyimide layer (A) may contain a diamine residue derived from a diamine component generally used for the synthesis of polyimide as a diamine residue. Such a diamine residue is not particularly limited, but is preferably an aromatic diamine residue. In addition, from the viewpoint of improving the adhesion of the polyimide layer (A) to the metal layer and controlling the AP value described later to be low, in combination with the D1 residue, for example, a small amount of a diamine residue derived from 2,2'-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) may be contained.

[0082] <AP value>

[0083] In this embodiment, the polyimide constituting the polyimide layer (A) comprises a structural unit represented by the following general formula (1):

[0084] [Chemistry 4]

[0085]

[0086] [wherein, Ar is a tetravalent acid anhydride residue derived from an aromatic tetracarboxylic anhydride, R 1 refers to a divalent diamine residue derived from a diamine compound]

[0087] When expressing, the AP value calculated based on the following mathematical formula (i) as an index representing the amount of polar groups contained in the polyimide is preferably 1.60 or less.

[0088] AP value={(A1+A2+A3) / (B1+B2+B3)}×100···(i)

[0089] [Here,

[0090] A1 = (the number of polar groups in the group Ar) x (the number of moles of the group Ar)

[0091] A2=(base R1 The number of polar groups in the 1 Number of moles)

[0092] A3 = (number of imide groups) × (number of moles of imide groups)

[0093] B1 = (molecular weight of group Ar) x (number of moles of group Ar)

[0094] B2=(base R 1 molecular weight)×(base R 1 Number of moles)

[0095] B3 = (molecular weight of imide group) × (number of moles of imide group), with respect to the number of the polar groups,

[0096] -X (where X is a halogen atom), -OH, -SH, -O-,

[0097] -S-, -SO-, -NH-, -CO-, -CN, -P=O,

[0098] -PO- is set to 1,

[0099] -SO 2 -, -CONH- are set to 2,

[0100] -SO 3 H, -(CO) 2 N-set to 3 for calculation]

[0101] The AP value is an index indicating the amount of polar groups contained in the polyimide. The larger the AP value, the larger the amount of polar groups in the polyimide. Since the polyimide constituting the polyimide layer (A) contains abundant ketone group-containing residues, the amount of polar groups tends to increase, and it is considered that the dielectric constant and dielectric loss tangent are likely to increase.

[0102] In addition, since the polyimide layer (A) is an adhesive layer connected to a metal layer such as copper foil, the polar groups contained in the polyimide layer (A) become factors that induce the diffusion of copper from the copper wiring, for example. That is, if the polyimide layer (A) contains a large amount of polar groups, the copper from the copper wiring diffuses widely into the polyimide layer (A) during repeated heating. As a result, the adhesion between the insulating resin layer and the wiring layer (metal layer) is weakened, and the peel strength is easily reduced.

[0103] From the above viewpoints, in the present embodiment, by controlling the AP value in the polyimide layer (A) to preferably be 1.60 or less, more preferably 1.55 or less, the amount of polar groups contained in the polyimide layer (A) can be reduced, and the deterioration of dielectric properties (dielectric constant and dielectric loss tangent) and the reduction of adhesiveness can be suppressed. If the AP value exceeds 1.60, the polar groups of the polyimide constituting the polyimide layer (A) increase, resulting in deterioration of dielectric properties and difficulty in coping with high-frequency signal transmission.

[0104] The polar groups used as the basis for calculating the AP value are divided into three stages according to the size of the electric dipole moment. The first stage is -X (where X is a halogen atom), -OH, -SH, -O-, -S-, -SO-, -NH-, -CO-, -CN, -P=O, and -PO-, and these are calculated as polar groups with one number each. The second stage is -SO 2 -, -CONH-, these are calculated as two polar groups. The third area is -SO 3 H, -(CO) 2 N- is calculated as three polar groups.

[0105] As shown in the mathematical formula (i), the AP value can be determined by the number of moles and molecular weight of the anhydride residue and the diamine residue in the polyimide and the number of the polar groups contained in these residues.

[0106] <Dielectric loss tangent>

[0107] From the viewpoint of being able to cope with high-frequency signal transmission, the dielectric loss tangent (Tanδ) at 15GHz measured by a molecular orientation meter in the polyimide layer (A) is preferably less than 0.008, more preferably more than 0.001 and less than 0.005. If the dielectric loss tangent at 15GHz of the polyimide layer (A) exceeds 0.008, it is easy to cause undesirable conditions such as electric signal loss on the high-frequency signal transmission path when used for circuit substrates such as FPC. Furthermore, the lower limit of the dielectric loss tangent is not particularly limited, considering the physical property control when the polyimide layer (A) is applied as the insulating resin layer of the circuit substrate.

[0108] <Dielectric constant>

[0109] From the viewpoint of being able to cope with high-frequency signal transmission, the dielectric constant at 15 GHz measured by a molecular orientation meter in the polyimide layer (A) is preferably 3.3 or less, more preferably 2.7 or more and 3.2 or less. If the dielectric constant of the polyimide layer (A) at 15 GHz exceeds 3.3, the dielectric loss of the insulating resin layer is deteriorated when used for circuit substrates such as FPC, and undesirable conditions such as electrical signal loss on the high-frequency signal transmission path are prone to occur. The lower limit of the dielectric constant is not particularly limited, and the physical property control when the polyimide layer (A) is used as the insulating resin layer of the circuit substrate is considered.

[0110] <Thickness of polyimide layer (A)>

[0111] The thickness of the polyimide layer (A) is not particularly limited, and is preferably in the range of 1 μm to 15 μm, and more preferably in the range of 2 μm to 10 μm. In the metal-clad laminate of this embodiment, the lower limit of the thickness can be reduced to 1 μm by making the polyimide layer (A) have a high elastic modulus.

[0112] [Polyimide layer (X)]

[0113] In the metal-clad laminate of the present embodiment, the polyimide layer (X) is the main polyimide layer. Here, the so-called "main" means having the largest thickness in the insulating resin layer, and preferably having a thickness of 50% or more, more preferably having a thickness of 60% or more relative to the total thickness of the insulating resin layer. In addition, in order to ensure the dimensional stability of the entire insulating resin layer as the main polyimide layer, the polyimide layer (X) is preferably a low thermal expansion resin layer having a thermal expansion coefficient (CTE) of 30ppm / K or less, preferably in the range of -5ppm / K to 25ppm / K.

[0114] The polyimide constituting the polyimide layer (X) contains an acid anhydride residue derived from an acid anhydride component and a diamine residue derived from a diamine component.

[0115] <Anhydride residue>

[0116] The polyimide constituting the polyimide layer (X) is not particularly limited to the subject matter, and in order to control the CTE of the polyimide layer (X) within the range, it is preferred to contain a PMDA residue. Relative to a total of 100 mol parts of all anhydride residues, the PMDA residue preferably contains 50 mol parts or more, and more preferably contains in the range of 60 mol parts to 100 mol parts. When the PMDA residue is less than 50 mol parts, the CTE of the polyimide layer (X) becomes high and the dimensional stability decreases.

[0117] The polyimide constituting the polyimide layer (X) may contain, as an acid anhydride residue, an acid anhydride residue derived from an acid anhydride component generally used for synthesis of polyimide. As such an acid anhydride residue, an aromatic tetracarboxylic acid residue is preferred.

[0118] <Diamine residue>

[0119] The polyimide constituting the polyimide layer (X) is not particularly limited, but preferably contains a diamine residue derived from a diamine compound represented by the following general formula (D2) (hereinafter sometimes referred to as "D2 residue") in order to control the CTE of the polyimide layer (X) within the above range.

[0120] [Chemistry 5]

[0121]

[0122] [In the general formula (D2), the substituent Y independently represents an alkyl group or alkoxy group having 1 to 3 carbon atoms or an alkenyl group having 2 to 3 carbon atoms, and p and q independently represent an integer of 0 to 4]

[0123] The D2 residue has a biphenyl skeleton and thus easily forms an ordered structure, promotes the orientation of the molecular chain in the in-plane direction, and can suppress the increase in the CTE of the polyimide layer (X). From this viewpoint, the polyimide constituting the polyimide layer (X) preferably contains D2 residues in the range of 30 to 100 mol parts, and more preferably contains D2 residues in the range of 50 to 100 mol parts, relative to 100 mol parts in total of all diamine residues.

[0124] Preferred specific examples of the D2 residue include diamine residues derived from diamine compounds such as 2,2'-dimethyl-4,4'-diaminobiphenyl (m-TB), 2,2'-diethyl-4,4'-diaminobiphenyl (m-EB), 2,2'-diethoxy-4,4'-diaminobiphenyl (m-EOB), 2,2'-dipropoxy-4,4'-diaminobiphenyl (m-POB), 2,2'-n-propyl-4,4'-diaminobiphenyl (m-NPB), 2,2'-divinyl-4,4'-diaminobiphenyl (VAB), and 4,4'-diaminobiphenyl. Among these, 2,2'-dimethyl-4,4'-diaminobiphenyl (m-TB) is particularly preferred because it easily forms an ordered structure and has a large effect of suppressing the increase in CTE.

[0125] The polyimide constituting the polyimide layer (X) may contain, as a diamine residue, a diamine residue derived from a diamine component generally used for synthesis of polyimide.

[0126] In addition, as the polyimide constituting the polyimide layer (X), a polyimide rich in amino groups at the end of the polymer chain is preferred. The amino group at the end is a functional group that interacts with the ketone group contained in the polyimide layer (A), so the interlayer adhesion with the polyimide layer (A) can be further improved. Such a polyimide can be formed by designing the input ratio in a manner that the molar ratio of the diamine compound is excessive relative to the acid anhydride as a raw material.

[0127] <Thickness of polyimide layer (X)>

[0128] The thickness of the polyimide layer (X) is not particularly limited and can be appropriately set depending on the intended use. For example, it is preferably in the range of 3 μm to 75 μm, and more preferably in the range of 8 μm to 50 μm.

[0129] [Synthesis of polyimide]

[0130] The polyimide constituting the polyimide layer (A) and the polyimide layer (X) can be produced by reacting an anhydride component with a diamine component in a solvent to generate a polyamic acid and then heating it for ring closure. For example, the anhydride component and the diamine component are dissolved in an organic solvent in approximately equimolar amounts, and the polymerization reaction is carried out by stirring for 30 minutes to 24 hours at a temperature in the range of 0° C. to 100° C., thereby obtaining a polyamic acid as a precursor of the polyimide. During the reaction, the reaction components are dissolved in a manner such that the generated precursor is in the range of 5% by weight to 30% by weight, preferably in the range of 10% by weight to 20% by weight in the organic solvent. As the organic solvent used in the polymerization reaction, for example, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N,N-diethylacetamide, N-methyl-2-pyrrolidone (NMP), 2-butanone, dimethyl sulfoxide (DMSO), hexamethylphosphoramide, N-methylcaprolactam, dimethyl sulfate, cyclohexanone, dioxane, tetrahydrofuran, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, cresol, etc. It is also possible to use two or more of these solvents in combination, and it is also possible to use aromatic hydrocarbons such as xylene and toluene in combination. In addition, the amount of such organic solvent used is not particularly limited, and it is preferably adjusted to an amount of about 5% by weight to 30% by weight so that the concentration of the polyamic acid solution obtained by the polymerization reaction is used.

[0131] The synthesized polyamic acid is usually advantageously used as a reaction solvent solution, and can be concentrated, diluted or replaced with other organic solvents as needed. In addition, polyamic acid is generally excellent in solvent solubility, so it is advantageously used. The viscosity of the solution of polyamic acid is preferably in the range of 500cps to 100,000cps. If it deviates from the range, when a coating operation is performed using a coater, etc., defects such as uneven thickness and stripes are easily produced on the film. The method for synthesizing polyimide by imidizing polyamic acid is not particularly limited, for example, the following heat treatment can be preferably used: in the solvent, heating is performed for 1 hour to 24 hours under temperature conditions in the range of 80°C to 400°C.

[0132] <Optional ingredients>

[0133] The polyimide constituting the polyimide layer (A) and the polyimide layer (X) may contain, for example, an arbitrary component such as a flame retardant and a filler, within a range not impairing the effects of the invention.

[0134] [Metal layer]

[0135] The raw material of the metal layer is preferably a metal foil. As the metal constituting the metal foil, for example, a metal selected from copper, aluminum, stainless steel, iron, silver, palladium, nickel, chromium, molybdenum, tungsten, zirconium, gold, cobalt, titanium, tantalum, zinc, lead, tin, silicon, bismuth, indium or an alloy thereof can be cited. In terms of conductivity, copper foil is particularly preferred. Furthermore, in the case of continuous production of the metal-clad laminate of the present embodiment, as the metal foil, a long strip of metal foil wound into a roll of a predetermined thickness is used.

[0136] In addition, the surface roughness (Rz) of the surface where the metal foil is directly in contact with the polyimide layer (A) is preferably in the range of 0.05 μm to 3.5 μm. The reason is that if it is within the range, the adhesion with the polyimide layer (A) will not be damaged, and even if the internal pressure at the interface between the polyimide layer (X) and the polyimide layer (A) increases during heat treatment, it is difficult for the polyimide layer (A) to break, and foaming can be suppressed. If the Rz of the metal foil exceeds 3.5 μm, it is difficult to perform fine wiring processing. Here, Rz refers to the ten-point average roughness specified in Japanese Industrial Standards (JIS) B 0601 (2001).

[0137] The peel strength between the metal layer and the insulating resin layer in the metal-clad laminate of the present embodiment is preferably 0.7 kN / m or more, and more preferably 1.0 kN / m or more. When the peel strength between the metal layer and the insulating resin layer is less than 0.7 kN / m, wiring peeling is likely to occur during circuit processing, and the manufacturing yield and reliability of the circuit substrate are reduced.

[0138] [Manufacture of Metal-Clad Laminated Plates]

[0139] The metal-clad laminate of the present embodiment can be produced, for example, by the following method.

[0140] First, a coating liquid containing a precursor of a polyimide constituting a polyimide layer (A), i.e., a polyamic acid, is cast on a metal foil as a metal layer, and dried to form the first coating film. Afterwards, a coating liquid containing a precursor of a polyimide constituting a main polyimide layer (X), i.e., a polyamic acid, is cast on the first coating film, and dried to form the second coating film. A coating film can be further laminated by repeatedly casting the coating liquid successively. For example, when the polyimide layer is set to a three-layer structure, a coating liquid containing a precursor of a polyimide constituting a polyimide layer (A), i.e., a polyamic acid, can also be cast on the second coating film, and dried to form the third coating film. The coating method is not particularly limited, and for example, known methods such as a rod coating method, a gravure coating method, a roller coating method, and a die coating method can be appropriately selected and adopted.

[0141] In the casting method, it is preferred to cast in a varnish state containing polyamic acid and a solvent. As the solvent, the organic solvents exemplified above for the polymerization reaction of polyamic acid can be cited. The solvent can also be used alone or in combination of two or more.

[0142] The coating film is dried to an appropriate range when the solvent is included. The drying temperature at this time is preferably carried out at a temperature at which imidization of the polyamic acid is not performed, specifically, it can be 150°C or less, preferably in the range of 110°C to 140°C. The metal-clad laminate of the present embodiment has the above-mentioned structure through the polyimide layer (A) and the polyimide layer (X). As long as the residual amount of the solvent does not become extremely large, foaming can be suppressed even if the residual solvent is vaporized during the heat treatment process of imidization in the following step.

[0143] Thereafter, the laminate including the metal layer and the coating film is imidized by heat treatment, and thus, for example, a single-sided metal-clad laminate having a laminate structure of metal layer / polyimide layer (A) / polyimide layer (X) or a metal-clad laminate having a laminate structure of metal layer / polyimide layer (A) / polyimide layer (X) / polyimide layer (A) can be formed. In the latter case, a metal foil is further laminated on the polyimide layer (A) by a method such as thermocompression bonding, thereby forming a double-sided metal-clad laminate having a laminate structure of metal layer / polyimide layer (A) / polyimide layer (X) / polyimide layer (A) / metal layer.

[0144] As described above, the metal-clad laminate has excellent adhesion between the metal layer and the polyimide layer (A) and between the polyimide layer (A) and the polyimide layer (X), and can be used as a circuit board material represented by FPC to improve the reliability of electronic equipment.

[0145] <Circuit board>

[0146] The circuit board of one embodiment of the present invention can be manufactured by processing the metal layer of the metal-clad laminate into a pattern by a common method to form a metal wiring layer. The patterning of the metal layer can be performed by any method such as photolithography and etching.

[0147] In the circuit substrate of the present embodiment, the peel strength between the metal wiring layer and the insulating resin layer is preferably 0.7 kN / m or more, and more preferably 1.0 kN / m or more. When the peel strength between the metal wiring layer and the insulating resin layer is less than 0.7 kN / m, the wiring is easily peeled off, and the manufacturing yield and reliability of the circuit substrate are reduced.

[0148] [Example]

[0149] The following examples are provided to more specifically describe the features of the present invention. However, the scope of the present invention is not limited to the examples. In the following examples, unless otherwise specified, various measurements and evaluations are performed according to the following.

[0150] [Viscosity measurement]

[0151] The viscosity of the resin was measured at 25° C. using an E-type viscometer (Brookfield, trade name: DV-II+Pro). The rotation speed was set so that the torque reached 10% to 90%, and the value when the viscosity stabilized was read 2 minutes after the start of the measurement.

[0152] [Determination of dielectric constant and dielectric loss tangent]

[0153] A 5 cm×5 cm film sample was prepared, and the dielectric constant and dielectric loss tangent were measured at a frequency of 15 GHz using a microwave molecular orientation meter MOA-6015 in a constant temperature and humidity chamber at 23° C. and 50% RH.

[0154] [Determination of storage elastic coefficient]

[0155] The storage elastic modulus was measured for a polyimide film having a size of 5 mm×20 mm using a dynamic viscoelasticity measuring apparatus (DMA: manufactured by TA Instruments, trade name: RSA3) at a heating rate of 5°C / min from 30°C to 400°C and a frequency of 1 Hz.

[0156] [Determination of peel strength]

[0157] The copper foil circuit of a single-sided copper-clad laminate (copper foil / polyimide layer) was processed into a sample with a width of 1.0 mm, and the surface of the polyimide layer was fixed to an aluminum plate using double-sided tape, and measured using a Tensilon tester (manufactured by Toyo Seiki Seisaku-sho, trade name: Strograph VE-1D). The copper foil was stretched in a 180° direction at a speed of 50 mm / min, and the median strength when peeled off by 10 mm was obtained.

[0158] [Evaluation of foaming]

[0159] When peeling was observed between the copper foil and the polyimide layer, or when peeling or cracking occurred in the polyimide layer, it was determined as “with foaming”, and when there was no peeling or cracking, it was determined as “without foaming”.

[0160] The abbreviations used in Examples and Comparative Examples represent the following compounds.

[0161] m-TB: 2,2'-dimethyl-4,4'-diaminobiphenyl

[0162] TPE-R: 1,3-bis(4-aminophenoxy)benzene

[0163] APB: 1,3-bis(3-aminophenoxy)benzene

[0164] BAPP: 2,2-bis[4-(4-aminophenoxy)phenyl]propane

[0165] 4,4'-DAPE: 4,4'-diaminodiphenyl ether

[0166] PMDA: Pyromellitic Dianhydride

[0167] BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride

[0168] BTDA: 3,3',4,4'-Benzophenonetetracarboxylic dianhydride

[0169] DMAc: N,N-dimethylacetamide

[0170] (Synthesis example 1)

[0171] 45.989 g of m-TB (216.63 mmol), 15.832 g of TPE-R (54.16 mmol), and 680 g of DMAc were added to a 1000 ml separable flask and stirred at room temperature under a nitrogen stream. After complete dissolution, 58.179 g of PMDA (266.73 mmol) was added and stirred at room temperature for 4 hours to obtain a polyamic acid solution A. The viscosity of the obtained polyamic acid solution A was 22,000 cP.

[0172] (Synthesis example 2)

[0173] 8.194g of TPE-R (28.03mmol), 3.836g of BAPP (9.34mmol), and 176g of DMAc were added to a 300ml separable flask and stirred at room temperature under a nitrogen flow. After complete dissolution, 11.971g of BTDA (37.15mmol) was added and stirred at room temperature for 4 hours to obtain a polyamic acid solution B. The viscosity of the obtained polyamic acid solution B is 2,200cP. After the obtained polyamic acid solution B is applied to a copper foil, it is heated and dried below 140°C to remove the solvent. Furthermore, a staged heat treatment is performed from 150°C to 360°C to complete the imidization. For the obtained metal-clad laminate, the copper foil is etched and removed using an aqueous solution of ferric chloride to obtain a polyimide film with a thickness of 20μm. The physical properties of the obtained polyimide film are shown in Table 1.

[0174] (Synthesis example 3)

[0175] 11.584 g of TPE-R (39.63 mmol) and 176 g of DMAc were added to a 300 ml separable flask and stirred at room temperature under nitrogen flow. After complete dissolution, 9.519 g of BTDA (29.54 mmol) and 2.897 g of BPDA (9.85 mmol) were added and stirred at room temperature for 4 hours to obtain a polyamic acid solution C. The viscosity of the obtained polyamic acid solution C was 3,500 cP. The physical properties of the polyimide film prepared in the same manner as in Synthesis Example 2 are shown in Table 1.

[0176] (Synthesis Example 4)

[0177] 10.296 g of TPE-R (35.22 mmol), 1.144 g of APB (3.91 mmol), and 176 g of DMAc were added to a 300 ml separable flask and stirred at room temperature under nitrogen flow. After complete dissolution, 12.560 g of BTDA (38.98 mmol) was added and stirred at room temperature for 4 hours to obtain a polyamic acid solution D. The viscosity of the obtained polyamic acid solution D was 1,500 cP. The physical properties of the polyimide film prepared in the same manner as in Synthesis Example 2 are shown in Table 1.

[0178] (Synthesis Example 5)

[0179] 8.571 g of TPE-R (29.32 mmol), 2.857 g of APB (9.77 mmol), and 176 g of DMAc were added to a 300 ml separable flask and stirred at room temperature under nitrogen flow. After complete dissolution, 12.572 g of BTDA (39.02 mmol) was added and stirred at room temperature for 4 hours to obtain a polyamic acid solution E. The viscosity of the obtained polyamic acid solution E was 1,100 cP. The physical properties of the polyimide film prepared in the same manner as in Synthesis Example 2 are shown in Table 1.

[0180] (Synthesis Example 6)

[0181] 11.452 g of TPE-R (39.18 mmol) and 176 g of DMAc were added to a 300 ml separable flask and stirred at room temperature under nitrogen flow. After complete dissolution, 12.548 g of BTDA (38.94 mmol) was added and stirred at room temperature for 4 hours to obtain a polyamic acid solution F. The viscosity of the obtained polyamic acid solution F was 2,600 cP. The physical properties of the polyimide film prepared in the same manner as in Synthesis Example 2 are shown in Table 1.

[0182] (Synthesis Example 7)

[0183] 11.969 g of TPE-R (40.94 mmol) and 176 g of DMAc were added to a 300 ml separable flask and stirred at room temperature under nitrogen flow. After complete dissolution, 9.816 g of BTDA (30.46 mmol) and 2.215 g of PMDA (10.15 mmol) were added and stirred at room temperature for 4 hours to obtain a polyamic acid solution G. The viscosity of the obtained polyamic acid solution G was 1,400 cP. The physical properties of the polyimide film prepared in the same manner as in Synthesis Example 2 are shown in Table 1.

[0184] (Synthesis Example 8)

[0185] 12.521 g of TPE-R (42.83 mmol) and 176 g of DMAc were added to a 300 ml separable flask and stirred at room temperature under nitrogen flow. After complete dissolution, 6.846 g of BTDA (21.24 mmol) and 4.634 g of PMDA (21.24 mmol) were added and stirred at room temperature for 4 hours to obtain a polyamic acid solution H. The viscosity of the obtained polyamic acid solution H was 2,200 cP. The physical properties of the polyimide film prepared in the same manner as in Synthesis Example 2 are shown in Table 1.

[0186] (Synthesis Example 9)

[0187] 9.727 g of 4,4'-DAPE (48.58 mmol) and 176 g of DMAc were added to a 300 ml separable flask and stirred at room temperature under nitrogen flow. After complete dissolution, 11.646 g of BTDA (36.14 mmol) and 2.628 g of PMDA (12.05 mmol) were added and stirred at room temperature for 4 hours to obtain a polyamic acid solution I. The viscosity of the obtained polyamic acid solution I was 1,100 cP. The physical properties of the polyimide film prepared in the same manner as in Synthesis Example 2 are shown in Table 1.

[0188] (Synthesis Example 10)

[0189] 15.622 g of BAPP (38.06 mmol) and 176 g of DMAc were added to a 300 ml separable flask and stirred at room temperature under nitrogen flow. After complete dissolution, 7.823 g of PMDA (35.86 mmol) and 0.555 g of BPDA (1.89 mmol) were added and stirred at room temperature for 4 hours to obtain a polyamic acid solution J. The viscosity of the obtained polyamic acid solution J was 1,800 cP. The physical properties of the polyimide film prepared in the same manner as in Synthesis Example 2 are shown in Table 1.

[0190] (Synthesis Example 11)

[0191] 9.244 g of 4,4'-DAPE (46.16 mmol) and 176 g of DMAc were added to a 300 ml separable flask and stirred at room temperature under nitrogen flow. After complete dissolution, 14.756 g of BTDA (45.79 mmol) was added and stirred at room temperature for 4 hours to obtain a polyamic acid solution K. The viscosity of the obtained polyamic acid solution K was 1,200 cP. The physical properties of the polyimide film prepared in the same manner as in Synthesis Example 2 are shown in Table 1.

[0192] (Synthesis Example 12)

[0193] 13.204 g of TPE-R (45.17 mmol) and 176 g of DMAc were added to a 300 ml separable flask and stirred at room temperature under a nitrogen stream. After complete dissolution, 6.841 g of PMDA (31.36 mmol) and 3.955 g of BPDA (13.44 mmol) were added and stirred at room temperature for 4 hours to obtain a polyamic acid solution L. The viscosity of the obtained polyamic acid solution L was 2,000 cP. The physical properties of the polyimide film prepared in the same manner as in Synthesis Example 2 are shown in Table 1.

[0194] (Synthesis Example 13)

[0195] 12.664 g of TPE-R (43.32 mmol) and 176 g of DMAc were added to a 300 ml separable flask and stirred at room temperature under nitrogen flow. After complete dissolution, 3.750 g of PMDA (17.19 mmol) and 7.586 g of BPDA (25.78 mmol) were added and stirred at room temperature for 4 hours to obtain a polyamic acid solution M. The viscosity of the obtained polyamic acid solution M was 1,700 cP. The physical properties of the polyimide film prepared in the same manner as in Synthesis Example 2 are shown in Table 1.

[0196] [Table 1]

[0197]

[0198] [Example 1]

[0199] On a copper foil with a thickness of 12 μm and a surface roughness Rz of 0.8 μm, after applying polyamic acid solution B in a manner that the thickness after hardening becomes 2 μm, the solvent is removed by heating and drying below 140 ° C. On it, after applying polyamic acid solution A in a manner that the thickness after hardening becomes 21 μm, the solvent is removed by heating and drying below 140 ° C. Further, on it, after applying polyamic acid solution B in a manner that the thickness after hardening becomes 2 μm, the solvent is removed by heating and drying below 140 ° C. Afterwards, the temperature is raised in stages from 140 ° C to 360 ° C and imidization is performed to prepare a copper-clad laminate 1a. The obtained copper-clad laminate 1a is evaluated for adhesion to the copper foil, and the peel strength is 1.0 kN / m. In addition, as a foaming evaluation, a copper-clad laminate 1b was prepared in the same manner as the copper-clad laminate 1a except that the heating time from 140°C to 360°C was changed to half a minute, but foaming was not confirmed.

[0200] [Example 2]

[0201] Evaluation of adhesion to copper foil and foaming was carried out in the same manner as in Example 1 except that polyamic acid solution C was used instead of polyamic acid solution B. The peel strength was 1.1 kN / m, and there was no foaming.

[0202] [Example 3]

[0203] The adhesion to the copper foil and the evaluation of the foaming were carried out in the same manner as in Example 1 except that the polyamic acid solution D was used instead of the polyamic acid solution B. As a result, the peel strength was 1.0 kN / m, and there was no foaming.

[0204] [Example 4]

[0205] Evaluation of adhesion to copper foil and foaming was carried out in the same manner as in Example 1 except that polyamic acid solution E was used instead of polyamic acid solution B. As a result, the peel strength was 1.0 kN / m, and there was no foaming.

[0206] [Example 5]

[0207] Evaluation of adhesion to copper foil and foaming was carried out in the same manner as in Example 1 except that polyamic acid solution F was used instead of polyamic acid solution B. The peel strength was 1.1 kN / m, and there was no foaming.

[0208] [Example 6]

[0209] Evaluation of adhesion to copper foil and foaming was carried out in the same manner as in Example 1 except that polyamic acid solution G was used instead of polyamic acid solution B. As a result, the peel strength was 1.1 kN / m, and there was no foaming.

[0210] [Example 7]

[0211] Evaluation of adhesion to copper foil and foaming was carried out in the same manner as in Example 1 except that polyamic acid solution H was used instead of polyamic acid solution B. As a result, the peel strength was 1.0 kN / m, and there was no foaming.

[0212] [Example 8]

[0213] Evaluations of adhesion to copper foil and foaming were carried out in the same manner as in Example 1 except that the polyamic acid solution I was used instead of the polyamic acid solution B. As a result, the peel strength was 0.9 kN / m, and there was no foaming.

[0214] [Example 9]

[0215] Copper clad laminate 9a was prepared in the same manner as Example 1 except that polyamic acid solution B was applied so that the thickness after curing became 3 μm, polyamic acid solution A was applied so that the thickness after curing became 44 μm, and polyamic acid solution B was applied so that the thickness after curing became 3 μm. The obtained copper clad laminate 9a was evaluated for adhesion to copper foil, and the peel strength was 1.0 kN / m. In addition, as a foaming evaluation, the heating time from 140°C to 360°C was set to half a minute, and copper clad laminate 9b was prepared in the same manner as copper clad laminate 9a, but foaming was not confirmed.

[0216] [Example 10]

[0217] Evaluation of adhesion to copper foil and foaming was carried out in the same manner as in Example 9 except that polyamic acid solution D was used instead of polyamic acid solution B. As a result, the peel strength was 1.0 kN / m, and there was no foaming.

[0218] [Example 11]

[0219] Evaluation of adhesion to copper foil and foaming was carried out in the same manner as in Example 9 except that polyamic acid solution G was used instead of polyamic acid solution B. As a result, the peel strength was 1.1 kN / m, and there was no foaming.

[0220] [Comparative Example 1]

[0221] Evaluation of adhesion to copper foil and foaming was carried out in the same manner as in Example 1 except that polyamic acid solution J was used instead of polyamic acid solution B. The peel strength was 1.1 kN / m, indicating foaming.

[0222] [Comparative Example 2]

[0223] Evaluation of adhesion to copper foil and foaming was carried out in the same manner as in Example 1 except that polyamic acid solution K was used instead of polyamic acid solution B. As a result, the peel strength was 1.0 kN / m, indicating foaming.

[0224] [Comparative Example 3]

[0225] The adhesion to the copper foil and the evaluation of the foaming were carried out in the same manner as in Example 1 except that the polyamic acid solution L was used instead of the polyamic acid solution B. As a result, the peel strength was 0.4 kN / m, and there was no foaming.

[0226] [Comparative Example 4]

[0227] Evaluation of adhesion to copper foil and foaming was carried out in the same manner as in Example 1 except that polyamic acid solution M was used instead of polyamic acid solution B. As a result, the peel strength was 1.1 kN / m, indicating foaming.

[0228] According to the above results, the polyimide layer in contact with the copper foil is obtained by using 40 mol parts or more of BTDA having a ketone group in the molecule as an anhydride component, and the storage elastic coefficient E' at 300°C is 1.0×10 8 Pa or more and the storage elastic coefficient E' at 350°C is 1.0×10 7 In Examples 1 to 8 where the values ​​were Pa or higher, no foaming was observed, and the peel strength and dielectric properties were also good.

[0229] On the other hand, in Comparative Example 1 and Comparative Example 4 in which BTDA was not used as an acid anhydride component, or Comparative Example 2 in which BTDA was used but the storage elastic coefficient E' was out of the above range, foaming was confirmed. In addition, in Comparative Example 3 in which BTDA was not used, the peel strength was significantly low. This is believed to be due to the excessively high storage elastic coefficient E' at 300°C and 350°C.

[0230] As mentioned above, although embodiment of this invention is described in detail for the purpose of illustration, this invention is not limited to the said embodiment.

Claims

1. A metal-clad laminate for a flexible circuit substrate, comprising an insulating resin layer and a copper foil layer laminated on one or both sides of the insulating resin layer, wherein the metal-clad laminate for a flexible circuit substrate is characterized in that: The insulating resin layer has a plurality of polyimide layers including a polyimide layer (A) in contact with the copper foil layer. The dielectric loss tangent (Tanδ) of the polyimide layer (A) is 0.008 or less, and the storage elastic coefficient E' of the polyimide layer (A) at 300°C measured by a dynamic mechanical analyzer, a dynamic viscoelasticity measuring device, under the conditions of a heating rate of 5°C / min from 30°C to 400°C and a frequency of 1 Hz, is 1.0×10 8 Pa or more, and the storage elastic coefficient E' at 350°C is 1.0×10 7 Pa or above, The polyimide constituting the polyimide layer (A) contains an acid anhydride residue derived from a tetracarboxylic dianhydride component and a diamine residue derived from a diamine component. The anhydride residues contain 40 mol parts or more of anhydride residues derived from tetracarboxylic dianhydride having a keto group, i.e., -CO-, in the molecule, and 5 mol parts to 25 mol parts of anhydride residues derived from pyromellitic dianhydride, relative to 100 mol parts of the total anhydride residues. The tetracarboxylic dianhydride having a keto group, i.e., -CO-, in the molecule includes 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,3',3,4'-benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 4,4'-(terephthalic acid carbonyl)diphthalic anhydride, or 4,4'-(isophthalic acid carbonyl)diphthalic anhydride.

2. The metal-clad laminate for a flexible circuit substrate according to claim 1, wherein the polyimide constituting the polyimide layer (A) is represented by a constituent unit represented by the following general formula (1): In the formula, Ar refers to a tetravalent acid anhydride residue derived from an aromatic tetracarboxylic anhydride, and R1 refers to a divalent diamine residue derived from a diamine compound. The AP value calculated based on the following mathematical formula (i) as an index representing the amount of polar groups contained in the polyimide is 1.60 or less, AP value={(A1+A2+A3) / (B1+B2+B3)}×100···(i) Here, A1 = (the number of polar groups in the group Ar) x (the number of moles of the group Ar) A2 = (the number of polar groups in the group R1) x (the number of moles of the group R1) A3 = (number of imide groups) × (number of moles of imide groups) B1 = (molecular weight of group Ar) x (number of moles of group Ar) B2 = (molecular weight of group R1) x (number of moles of group R1) B3 = (molecular weight of imide group) × (number of moles of imide group), with respect to the number of the polar groups, -X, -OH, -SH, -O-, -S-, -SO-, -NH-, -CO-, -CN, -P=O, -PO- is set to 1, -SO2-, -CONH- are set to 2, The calculation was performed with three -SO3H and three -(CO)2N-, respectively, and X is a halogen atom. 3 . The metal-clad laminate for a flexible circuit board according to claim 1 , wherein the peel strength between the copper foil layer and the insulating resin layer is 0.7 kN / m or more.

4. The metal-clad laminate for a flexible circuit board according to claim 1 or 2, wherein the polyimide constituting the polyimide layer (A) contains a diamine residue derived from a diamine compound represented by the following general formula (D1) in an amount ranging from 50 to 100 parts by mole, relative to 100 parts by mole of the total diamine residue.

5. The metal-clad laminate for a flexible circuit board according to claim 3, wherein the polyimide constituting the polyimide layer (A) contains a diamine residue derived from a diamine compound represented by the following general formula (D1) in an amount ranging from 50 to 100 parts by mole, relative to 100 parts by mole of the total diamine residue.

6. A flexible circuit substrate comprising an insulating resin layer and a copper wiring layer laminated on one or both sides of the insulating resin layer, wherein: The insulating resin layer includes a plurality of polyimide layers including a polyimide layer (A) in contact with the copper wiring layer. The dielectric loss tangent (Tanδ) of the polyimide layer (A) is 0.008 or less, and the storage elastic coefficient E' of the polyimide layer (A) at 300°C measured by a dynamic mechanical analyzer, a dynamic viscoelasticity measuring device, under the conditions of a heating rate of 5°C / min from 30°C to 400°C and a frequency of 1 Hz, is 1.0×10 8 Pa or more, and the storage elastic coefficient E' at 350°C is 1.0×10 7 Pa or above, The polyimide constituting the polyimide layer (A) contains an acid anhydride residue derived from a tetracarboxylic dianhydride component and a diamine residue derived from a diamine component. The anhydride residues contain 40 mol parts or more of anhydride residues derived from tetracarboxylic dianhydride having a keto group, i.e., -CO-, in the molecule, and 5 mol parts to 25 mol parts of anhydride residues derived from pyromellitic dianhydride, relative to 100 mol parts of the total anhydride residues. The tetracarboxylic dianhydride having a keto group, i.e., -CO-, in the molecule includes 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,3',3,4'-benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 4,4'-(terephthalic acid carbonyl)diphthalic anhydride, or 4,4'-(isophthalic acid carbonyl)diphthalic anhydride.

7. The flexible circuit substrate according to claim 6, wherein the polyimide constituting the polyimide layer (A) is represented by a constituent unit represented by the following general formula (1): In the formula, Ar refers to a tetravalent acid anhydride residue derived from an aromatic tetracarboxylic anhydride, and R1 refers to a divalent diamine residue derived from a diamine compound. The AP value calculated based on the following mathematical formula (i) as an index representing the amount of polar groups contained in the polyimide is 1.60 or less, AP value={(A1+A2+A3) / (B1+B2+B3)}×100···(i) Here, A1 = (the number of polar groups in the group Ar) x (the number of moles of the group Ar) A2 = (the number of polar groups in the group R1) x (the number of moles of the group R1) A3 = (number of imide groups) × (number of moles of imide groups) B1 = (molecular weight of group Ar) x (number of moles of group Ar) B2 = (molecular weight of group R1) x (number of moles of group R1) B3 = (molecular weight of imide group) × (number of moles of imide group), with respect to the number of the polar groups, -X, -OH, -SH, -O-, -S-, -SO-, -NH-, -CO-, -CN, -P=O, -PO- is set to 1, -SO2-, -CONH- are set to 2, The calculation was performed with three -SO3H and three -(CO)2N-, respectively, and X is a halogen atom. 8 . The flexible circuit board according to claim 6 , wherein the peel strength between the copper wiring layer and the insulating resin layer is 0.7 kN / m or more.

9. The flexible circuit board according to claim 6 or 7, wherein the polyimide constituting the polyimide layer (A) contains a diamine residue derived from a diamine compound represented by the following general formula (D1) in an amount ranging from 50 to 100 parts by mole, relative to 100 parts by mole of the total diamine residue.

10. The flexible circuit board according to claim 8, wherein the polyimide constituting the polyimide layer (A) contains a diamine residue derived from a diamine compound represented by the following general formula (D1) in an amount ranging from 50 to 100 parts by mole, relative to 100 parts by mole of the total diamine residue.