A thin film laminate structure

By using a combination of two optical adjustment layers and low resistance conductive layers in the thin film stack structure, the refractive index between transparent conductive materials and glass layers is solved by using high-refractive index resin and metal particles, combined with coating and sputtering technology. The etching line and chromatic aberration problems caused by the difference achieve better optical matching and display effects.

CN111446027BActive Publication Date: 2024-11-22BEIJING ZENITHNANO TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010348904.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-04-28
Publication Date
2024-11-22
Estimated Expiration
2040-04-28

AI Technical Summary

Technical Problem

In the prior art, the difference in refractive index between transparent conductive materials and glass or other layers leads to the problem of visible etch lines or laser lines, especially when low resistance conductive materials are used, it is difficult to effectively suppress chromatic aberration.

Method used

A two-layer optical adjustment layer structure is adopted, wherein the first optical adjustment layer is arranged on one side of the substrate layer, the second optical adjustment layer is arranged on the side of the first optical adjustment layer away from the substrate layer, and the low resistance conductive layer is arranged on the optical The adjustment layer is away from the substrate layer, and the reflection difference between the two optical adjustment layers is less than 1. It is formed by combining high refractive index resin and metal particles, combined with coating and sputtering methods to ensure adhesion and light transmission of the optical adjustment layer. Transcendent.

Benefits of technology

It effectively reduces the color difference between the low-resistance conductive layer and other layers, improves the visibility of the display interface, and is especially suitable for low-resistance conductive materials, reduces the reflectance difference and improves the optical adjustment effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111446027B_ABST
    Figure CN111446027B_ABST
Patent Text Reader

Abstract

The present invention discloses a thin film stack structure, comprising a substrate layer, an optical adjustment layer, and a low-resistance conductive layer, wherein the optical adjustment layer comprises a first optical adjustment layer and a second optical adjustment layer, wherein the first optical adjustment layer is arranged on one side of the substrate layer, and the second optical adjustment layer is arranged on the side of the first optical adjustment layer away from the substrate layer; the low-resistance conductive layer is arranged on the side of the optical adjustment layer away from the substrate layer, and the reflectivity difference between the optical adjustment layer and the low-resistance conductive layer is less than 1. After the refractive indices of the two optical adjustment layers are matched with each other, they have a good adjustment and matching effect on the chromatic aberration generated by the low-resistance conductive layer and other layers in the display device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a thin film stacking structure, in particular to a thin film stacking structure containing a color difference adjustment layer. Background Art

[0002] In recent years, electronic devices in the display field have been widely formed by bonding electrode layers and glass cover plates by liquid optical adhesive (OCA). The electrode layer is a conductive film composed of transparent conductive materials stacked on a film composed of a transparent substrate as the main body; the conductive film is then formed into an electrode layer by yellow light etching or laser and other methods. Since the transparent conductive material has a different refractive index compared to glass or other layers such as optical adhesive (OCA), the part of the electrode layer with transparent conductive materials and the part without transparent electrode layers have different refractive indices, and the interference of each layer is different. When the difference in refractive index is large, it is easy to form etching lines or visible laser rays, affecting the visibility of the display interface.

[0003] In the prior art, an optical adjustment layer (IM) is usually provided between the electrode layer and the glass to solve the problem of visible etching lines or laser rays. However, transparent conductive materials are developing in the direction of low resistance, and usually thicker ITO or transparent low-resistance conductive materials different from ITO are selected. Therefore, in conventional optical adjustment layers, it is difficult to fully suppress the color difference formed between the low-resistance electrode layer and other layers. Summary of the invention

[0004] In order to solve the above-mentioned problem of visible etching lines, the present invention proposes a thin film stack structure, including a substrate layer, an optical adjustment layer, and a low-resistance conductive layer, wherein the optical adjustment layer includes a first optical adjustment layer and a second optical adjustment layer, wherein the first optical adjustment layer is arranged on one side of the substrate layer, and the second optical adjustment layer is arranged on a side of the first optical adjustment layer away from the substrate layer; the low-resistance conductive layer is arranged on a side of the optical adjustment layer away from the substrate layer; and the reflectivity difference between the optical adjustment layer and the low-resistance conductive layer is less than 1.

[0005] An optical adjustment layer is provided between the substrate layer and the conductive layer, the purpose of which is to adjust the chromatic aberration problem such as the visible etching line generated after the thin film stacked structure is subsequently attached to the glass cover plate by OCA. The two optical adjustment layers provided in the present invention are particularly suitable for the case where a low-resistance conductive material is used as the conductive layer. Usually, one optical adjustment layer only produces a good refractive index matching effect for a conductive layer greater than 100Ω / □. For special low-resistance conductive materials, the smaller the resistance value, the lower the reflectivity, and the required reflectivity of the optical adjustment layer should be the lower. However, currently a single optical adjustment layer will produce an unnecessary refractive effect for low-resistance conductive materials. Therefore, after the refractive indices of the two optical adjustment layers of the present invention are matched with each other, the reflectivity difference between the low-resistance conductive layer and the optical adjustment layer becomes smaller, thereby having a good adjustment and matching effect on the chromatic aberration generated by the low-resistance conductive layer and other layers in the display device.

[0006] Preferably, the low-resistance conductive layer described in the present invention refers to a conductive layer with a resistance less than 30Ω / □. In practice, when the square resistance of the conductive layer is less than 30Ω, the reflectivity of the conductive layer is R and the reflectivity of the optical adjustment layer is R. IM层 , reflection difference △R=|R–R IM层 |, △R<1 is the best, which has a better optical adjustment effect. Preferably, 0.2<△R<0.7.

[0007] Preferably, the substrate layer refers to a flexible transparent substrate, and the material is selected from one or more of polyethylene terephthalate (PET), polyimide (PI), polypropylene (PP), polystyrene (PS), triacetyl cellulose (TAC), FMH acrylonitrile-butadiene-styrene (ABS), polyvinyl chloride (PVC), polycarbonate (PC), polyethylene (PE), polymethyl methacrylate (PMMA), polytetrafluoroethylene, cycloolefin copolymer (COP, Arton), polyethylene naphthalate (PEN). The purpose of the substrate layer is to carry the conductive layer.

[0008] Preferably, the first optical adjustment layer comprises a high refractive index resin and metal particles. The high refractive index resin refers to a resin with a refractive index in the range of 1.6-1.7. Preferably, the metal particles are evenly distributed in the high refractive index resin. The high refractive index resin is doped with metal particles so that the first optical adjustment layer has both a high refractive index and good light transmittance. The metal particles can make the light diffusely reflected to the first optical adjustment layer, and the reflected light is more uniform. Preferably, the high refractive index resin comprises a plurality of benzene rings and epoxy structures. The metal particles are selected from one or more of silicon (Si), zirconium (Zr), titanium (Ti), iron (Fe), and cobalt (Co).

[0009] Preferably, the particle size of the metal particles is 20-100 nm. Metal particles within this particle size range are particularly suitable for mixing with high refractive index resins, and have good light transmittance and uniform light. Preferably, the particle size of the metal particles is 30 nm, 50 nm, 70 nm, 80 nm, 100 nm, 130 nm, 150 nm or 180 nm.

[0010] Preferably, the first optical adjustment layer has a thickness of 0.5-5 um and a refractive index of 1.6-1.7.

[0011] Preferably, the refractive index is 1.6, 1.62, 1.65, 1.68 or 1.7.

[0012] Preferably, the insulating sheet resistance of the second optical adjustment layer is greater than 10^8Ω / □.

[0013] Preferably, the second optical adjustment layer is a single-layer non-conductive metal layer with a thickness of 0.5 to 80 nm. Preferably, the thickness of the second optical adjustment layer is 10 nm, 30 nm, 50 nm or 70 nm. The material of the second optical adjustment layer is selected from one or more of titanium (Ti), indium (In), tin (Sn), indium tin alloy, and silicon aluminum alloy. Preferably, the weight percentage of indium doping in the indium tin alloy is 0 to 50%, and the weight percentage of aluminum doping in the silicon aluminum alloy is 0 to 50%.

[0014] Preferably, the second optical adjustment layer includes a high refractive index layer and a low refractive index layer.

[0015] Preferably, the thickness of the high refractive index layer is 2 to 200 nm, and its refractive index is 1.8 to 2.4; preferably, the thickness of the high refractive index layer is 10 nm, 30 nm, 50 nm, 80 nm, 120 nm or 160 nm; preferably, the refractive index of the high refractive index layer is 1.8, 1.9, 2.0, 2.1, 2.2, 2.3 or 2.4; preferably, the material of the refractive index layer is selected from metal oxides, nitrides, sulfides or dopants thereof with a refractive index of 1.8 to 2.4. Preferably, the material of the dopant is selected from one or more of aluminum (Al), gallium (Ga), zirconium (Zr), boron (B), yttrium (Y), molybdenum (Mo), and sulfur (S);

[0016] Preferably, the material of the high refractive index layer is TiO2, SnO2, ZnO, Nb2O5, Ta2O5, Si3N4, ZnS, and the dopants include AZO, GZO, YZO, etc.

[0017] Preferably, the thickness of the low refractive index layer is 10 to 500 nm, and its refractive index is 1.2 to 1.7. Preferably, the thickness of the low refractive index layer is 10 nm, 20 nm, 50 nm, 80 nm, 120 nm, 180 nm, 250 nm or 400 nm. Preferably, the refractive index of the low refractive index layer is 1.2, 1.3, 1.4, 1.5, 1.6 or 1.7; the material of the low refractive index layer is selected from metal oxides, non-metal oxides, sulfides, fluorides, carbides with a refractive index of 1.2 to 1.7, preferably, the refractive index material is SiO2, Al2O3, MgF, MgS or SiC.

[0018] Preferably, the first optical adjustment layer is formed by a coating method, and the second optical adjustment layer is formed by a sputtering method. Preferably, the coating method can be spin coating, spray coating, dip coating, slit coating, roller coating, Meyer rod coating, but not limited thereto. It can be understood that when the first optical adjustment layer contains organic materials such as high refractive index resins, the coating method is used to make the coating have good coverage and good light transmittance. Preferably, the sputtering method is magnetron sputtering. The use of the sputtering method can increase the compactness of the second optical adjustment layer.

[0019] Preferably, the thin film stack structure is composed of a substrate layer, a first optical adjustment layer, a second optical adjustment layer, and a low-resistance conductive layer stacked in sequence from bottom to top. It can be understood that the first optical adjustment layer is placed on the substrate layer, and a high-refractive index resin doped with metal particles can be well attached to the substrate layer by a coating method. The second optical adjustment layer can be a single layer or a double layer, and the materials are all inorganic materials. The sputtering method can not only improve the compactness of the second optical adjustment layer, but also increase the adhesion of the inorganic material on the first optical adjustment layer. It can be understood that coating both optical adjustment layers will result in poor adhesion, and sputtering both optical adjustment layers will result in poor light transmittance, causing yellowing to affect the color system. The two optical adjustment layers formed by coating one layer and sputtering one layer not only ensure the adhesion between the stacked layers, but also will not form yellowing to cause color difference. And the second optical adjustment layer (sputtering coating) is adjacent to the low-resistance conductive layer, and both are inorganic material layers, which will not cause corrosion damage to the low-resistance conductive layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 FIG. 4 is a cross-sectional view of an embodiment of a thin film stack structure of the present invention.

[0021] Figure 2 FIG. 4 is a cross-sectional view of another embodiment of the thin film stack structure of the present invention. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0023] Unless otherwise specified, the solvents, reagents, coating methods, technical parameters, coating equipment, etc. used in the present invention are conventional solvents, reagents, methods, parameters, equipment, etc. in the technical field.

[0024] Example 1

[0025] like Figure 1As shown, this embodiment provides a thin film stacking structure, which includes, from bottom to top, a substrate layer 1, a first optical adjustment layer 3, a second optical adjustment layer 5, and a low-resistance conductive layer 7. The substrate layer 1 is PET. The first optical adjustment layer 3 includes a resin with a refractive index in the range of 1.6-1.7 and titanium (Ti) particles, which are disposed on the PET by a coating method. The thickness of the first optical adjustment layer 3 is 2 μm. The second optical adjustment layer 5 is a single-layer non-conductive metal layer, and its material is an indium tin alloy (InSn), wherein the proportion of indium (In) in the alloy is 40%. The indium tin alloy (InSn) is sputtered on the first optical adjustment layer 3 by a magnetron sputtering method. The thickness of the second optical adjustment layer 5 is 30 nm.

[0026] Example 2

[0027] like Figure 2 As shown, this embodiment provides a thin film stacking structure, which includes, from bottom to top, a substrate layer 1, a first optical adjustment layer 3, a second optical adjustment layer 5, and a low-resistance conductive layer 7. The substrate layer 1 is PET. The first optical adjustment layer 3 includes a resin with a refractive index in the range of 1.6-1.7 and silicon (Si) particles, which are disposed on the PET by coating. The thickness of the first optical adjustment layer 3 is 4 μm. The second optical adjustment layer 5 includes a low refractive index layer 51 and a high refractive index layer 52. The material of the low refractive index layer 51 is titanium dioxide (TiO2), which is disposed on the first optical adjustment layer 3 by magnetron sputtering. The thickness of the low refractive index layer is 50 nm. The material of the high refractive index layer 52 is silicon dioxide (SiO2), which is disposed on the low refractive index layer 51 by magnetron sputtering. The thickness of the high refractive index layer 52 is 100 nm.

[0028] Example 3

[0029] like Figure 2 As shown, this embodiment provides a thin film stacking structure, which includes, from bottom to top, a substrate layer 1, a first optical adjustment layer 3, a second optical adjustment layer 5, and a low-resistance conductive layer 7. The substrate layer 1 is PET. The first optical adjustment layer 3 includes a resin with a refractive index in the range of 1.6-1.7 and titanium (Ti) particles, which are disposed on the PET by coating. The thickness of the first optical adjustment layer 3 is 3 μm. The second optical adjustment layer 5 includes a low refractive index layer 51 and a high refractive index layer 52. The material of the low refractive index layer 51 is aluminum oxide (Al2O3), which is disposed on the first optical adjustment layer 3 by magnetron sputtering. The thickness of the low refractive index layer is 400 nm. The material of the high refractive index layer 52 is tin oxide (SnO2), which is disposed on the low refractive index layer 51 by magnetron sputtering. The thickness of the high refractive index layer 52 is 50 nm.

[0030] Example 4

[0031] like Figure 2 As shown, this embodiment provides a thin film stacking structure, which includes, from bottom to top, a substrate layer 1, a first optical adjustment layer 3, a second optical adjustment layer 5, and a low-resistance conductive layer 7. The substrate layer 1 is PMMA. The first optical adjustment layer 3 includes a resin with a refractive index in the range of 1.6-1.7 and silicon aluminum alloy (SiAl) particles (the aluminum content in the silicon aluminum alloy is 40%), which is disposed on the PMMA by coating. The thickness of the first optical adjustment layer 3 is 1 μm. The second optical adjustment layer 5 includes a low refractive index layer 51 and a high refractive index layer 52. The material of the low refractive index layer 51 is magnesium sulfide (MgS), which is disposed on the first optical adjustment layer 3 by magnetron sputtering. The thickness of the low refractive index layer is 250 nm. The material of the high refractive index layer 52 is silicon nitride (Si3N4), which is disposed on the low refractive index layer 51 by magnetron sputtering. The thickness of the high refractive index layer 52 is 10 nm.

[0032] Comparative Example 1

[0033] This comparative example provides a thin film stacking structure, which is different from Example 3 only in that the second optical adjustment layer is made by coating.

[0034] Comparative Example 2

[0035] This comparative example provides a thin film stacking structure, which is different from Example 3 only in that the first optical adjustment layer is made by magnetron sputtering.

[0036] Comparative Example 3

[0037] This comparative example provides a thin film stacking structure, which is different from Example 2 only in that the thickness of the high refractive index layer is 300 nm.

[0038] Comparative Example 4

[0039] This comparative example provides a thin film stack structure, which is different from Example 4 only in that the silicon aluminum alloy (SiAl) is replaced by tin oxide (SnO2).

[0040] The thin film stack structures of the above embodiments and comparative examples were subjected to square resistance test, adhesion test using the hundred-grid test method, and light transmittance test. The results are shown in the following table;

[0041] The difference between the average reflectivity values ​​of the low-resistance conductive layer and the optical adjustment layer in the range of 400-700 nm was measured using a UV-VIS spectrophotometer for the above embodiments and comparative examples, and the results are shown in the following table;

[0042] Resistance (Ω / □) Transmittance (%) Adhesion Reflectivity difference △R Example 1 10.8 90.4 5B 0.38 Example 2 7.2 88.5 5B 0.64 Example 3 15.5 90.2 5B 0.28 Example 4 18.1 90.7 5B 0.21 Comparative Example 1 15.2 86.4 3B 1.58 Comparative Example 2 16.8 87.2 5B 2.98 Comparative Example 3 15.8 86.2 5B 1.46 Comparative Example 4 16.2 85.4 5B 1.87

[0043] Table 1

[0044] As shown in Table 1, Example 3, Comparative Example 1, and Comparative Example 2 can confirm that the first optical adjustment layer is coated and the second optical adjustment layer is sputtered, which can effectively improve the adhesion of the second optical adjustment layer, thereby improving the light transmittance of the thin film stack structure and reducing the reflectivity difference between the low-resistance conductive layer and the optical adjustment layer.

[0045] From Example 2 and Comparative Example 3, it can be confirmed that the thickness of the high refractive index in the optical adjustment layer is 2 to 200 nm, which effectively reduces the resistance of the thin film stack structure.

[0046] From Example 4 and Comparative Example 4, it can be confirmed that the refractive index of the first optical adjustment layer of 1.6 to 1.7 can improve the light transmittance of the thin film stack structure and reduce the reflectivity difference between the low-resistance conductive layer and the optical adjustment layer.

[0047] Although the present invention has been described in detail above, the above description is merely illustrative of the present invention in all aspects and is not intended to limit the scope thereof. Therefore, various modifications or variations can be made without departing from the scope of the present invention.

Claims

1. A thin film stack structure comprising substrate layer; An optical adjustment layer, wherein the optical adjustment layer comprises a first optical adjustment layer and a second optical adjustment layer, wherein the first optical adjustment layer is disposed on one side of the substrate layer, and the second optical adjustment layer is disposed on a side of the first optical adjustment layer away from the substrate layer; A low-resistance conductive layer, wherein the low-resistance conductive layer is disposed on a side of the optical adjustment layer away from the substrate layer; The difference between the average reflectivity values ​​of the low-resistance conductive layer and the optical adjustment layer in the range of 400-700nm is less than 1, the first optical adjustment layer comprises a high-refractive index resin and metal particles, the high-refractive index resin comprises a plurality of benzene rings and epoxy structures, the metal particles are selected from one or more of zirconium (Zr), titanium (Ti), iron (Fe), and cobalt (Co), the first optical adjustment layer is formed by a coating method, the second optical adjustment layer is formed by a sputtering method, the thickness of the first optical adjustment layer is 0.5-5um, and the refractive index is 1.6-1.7, the resistance of the low-resistance conductive layer is less than or equal to 30Ω / □, and the thin film stack structure is composed of a substrate layer, a first optical adjustment layer, a second optical adjustment layer, and a low-resistance conductive layer stacked in sequence from bottom to top.

2. The thin film stack structure according to claim 1, characterized in that: The particle size of the metal particles is 200nm-100nm.

3. The thin film stack structure according to claim 1, characterized in that: The second optical adjustment layer includes a high refractive index layer and a low refractive index layer.

4. The thin film stack structure according to claim 3, characterized in that: The thickness of the high refractive index layer is 2-200 nm, and the refractive index thereof is 1.8-2.4; the thickness of the low refractive index layer is 10-500 nm, and the refractive index thereof is 1.2-1.

7.

5. The thin film stack structure according to claim 1, characterized in that: The second optical adjustment layer is a single non-conductive metal layer with a thickness of 0.5-80 nm, and the material is selected from one or more of Ti, In, Sn, InSn alloy or SiAl alloy.