A CNC welding process technology for double ring weld of aluminum alloy conductive terminal conductor

By using a combination of a double-ring seam CNC machine tool and a pulse melting electrode welding power source in the aluminum alloy welding conductor process, automatic welding of the girth welds at both ends of the conductor is achieved, solving the problems of high labor intensity and low efficiency for welders, and improving the welding speed. and environmental safety.

CN111822958BActive Publication Date: 2024-10-01JINAN SHENGYUAN ELECTRIC APPLIANCE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202010740699.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-28
Publication Date
2024-10-01
Estimated Expiration
2040-07-28

AI Technical Summary

Technical Problem

The existing aluminum alloy welding conductor process has problems such as high labor intensity for welders, slow welding speed, low labor efficiency, poor working environment, and is not conducive to the occupational health and safety of employees.

Method used

Using a double ring welding CNC machine tool, two pulse melting electrode welding power sources and an automatic wire feeding device, the wire pusher gun advances the control mechanism and the argon gas shielded welding pool to realize automatic welding of the ring welds at both ends of the conductor, replacing ordinary manual non-stop welding. Magnet arc welding reduces the heating steps before welding.

Benefits of technology

It reduces the labor intensity of welders, increases welding speed and labor efficiency, improves the working environment, and enhances the occupational health and safety of employees.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111822958B_ABST
    Figure CN111822958B_ABST
Patent Text Reader

Abstract

The invention provides a CNC welding process technology for double-ring welds of aluminum alloy conductive terminal conductors, including the following process flow: blanking and processing of terminals and aluminum tubes, adjusting the clamping distance of a welding machine, adjusting the welding position of a wire-pushing welding gun, adjusting the position of a fume hood, adjusting the position and height of a bracket, clamping and mounting welding workpieces, connecting an argon gas pipeline, installing welding wire, adjusting the position of the welding wire and a weld, inputting or calling out a program, checking or adjusting process parameters, starting automatic welding, disassembling workpieces, trimming the weld surface of the workpiece, and inspecting weld quality; the invention also adopts a welding method of a wire-pushing welding gun advancing a regulating mechanism and an argon gas-shielded welding pool, and starting a welding program can automatically complete the process technology of the ring welds at both ends of the conductor at one time; it replaces ordinary manual non-melting electrode argon arc welding, and does not need to heat the welding part before welding, thereby reducing the labor intensity of welders, increasing the welding speed, improving the working environment, and being beneficial to the occupational health and safety of employees.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of numerical control welding, and in particular to a numerical control welding process technology for a double-ring weld of an aluminum alloy conductive terminal conductor. Background Art

[0002] At present, aluminum alloy welding conductors are welded by welding terminals at both ends and aluminum alloy tubes, and the parent materials are aluminum-magnesium alloy bars, tubes and cast aluminum alloys. The welding process uses ordinary manual argon arc welding and the welding parts need to be heated before welding. There are problems such as high labor intensity for welders, slow welding speed, low labor efficiency, poor working environment and unfavorable occupational health and safety of employees. Summary of the invention

[0003] In view of the above-mentioned technical deficiencies, the purpose of the present invention is to provide a CNC welding process technology for double-ring welds of aluminum alloy conductive terminal conductors, which adopts a double-ring weld CNC machine tool, is equipped with two pulse melting electrode welding power supplies and an automatic wire feeding device, adopts a wire push welding gun to advance the control mechanism and an argon gas to protect the welding molten pool, and starts the welding program to automatically complete the process technology of the ring welds at both ends of the conductor at one time, replacing ordinary manual non-melting electrode argon arc welding, and does not require reheating before welding, which solves the problems of high labor intensity, slow welding speed, low labor efficiency, poor working environment and being unfavorable to the occupational health and safety of employees.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0005] A CNC welding process technology for double-ring welds of aluminum alloy conductive terminals includes the following steps:

[0006] 1) Cut the terminals and aluminum tubes into the required length using a CNC sawing machine;

[0007] 2) Terminal and aluminum tube processing: use a lathe to perform end face and groove cutting on the terminal and aluminum tube, and use a drilling machine to perform the necessary drilling and tapping operations on the terminal and aluminum tube;

[0008] 3) Adjust the clamping distance of the welding machine, adjust the position of the chuck and pneumatic ejector on the CNC welding machine, and adjust the appropriate distance according to the clamping length of the workpiece to be processed;

[0009] 4) Adjust the welding position of the welding gun, adjust the wire pushing welding gun advancing control mechanism on the CNC welding machine, and adjust it to a suitable position according to the length and height of the weld mouth of the workpiece;

[0010] 5) Adjust the position of the mobile fume hood and move the fume purifier's fume pipe to a suitable position to ensure that the welding fume can be sucked into the fume purifier through the fume pipe;

[0011] 6) Adjust the position and height of the bracket on the CNC welding machine to ensure that the two terminals are parallel to the aluminum tube;

[0012] 7) Clamp the welding workpiece, clamp the workpiece on the CNC welding machine through the chuck and pneumatic ejector, and clamp the terminal and the aluminum tube firmly;

[0013] 8) Connect the argon gas pipeline and turn on the flow meter on the argon gas pipeline;

[0014] 9) Install welding wire and use automatic CNC wire feeder to install welding wire for wire push welding gun;

[0015] 10) Adjust the position of the welding wire and the weld, and adjust the welding wire to extend out of the weld to a suitable distance according to the workpiece to be processed;

[0016] 11) Input or call out the program, input or call out the corresponding welding work program of the workpiece to be processed in the CNC panel of the CNC welding machine tool;

[0017] 12) Check or adjust process parameters to ensure correct processing;

[0018] 13) Turn on the switches on the CNC welding machine, welding power supply, CNC wire feeder, wire push welding gun and argon gas pipeline; start the automatic welding program and implement automatic welding of double ring welds;

[0019] 14) Disassemble the workpiece, loosen the chuck and pneumatic tightening device, and hang down the welded workpiece;

[0020] 15) Repair the weld surface of the workpiece, and repair the defects such as spatter, pile-up, and lack of fusion on the weld surface of the workpiece;

[0021] 16) Weld quality inspection: Use visual inspection or measuring tools to inspect the workpiece after welding to ensure that there are no defects such as pores and lack of fusion on the weld surface.

[0022] Preferably, the welding equipment used in the welding process includes a CNC welding machine, a smoke purifier, two pulse melting electrode welding power supplies and two CNC wire feeders, and the CNC welding machine is a double-ring weld CNC machine, the double-ring weld CNC machine is provided with a fixed head and a movable tailstock, the fixed head is equipped with a CNC system and an adjustment panel, the fixed head and the movable tailstock are both equipped with wire pushing welding guns, the CNC wire feeder is installed on the propulsion and control mechanism of the wire pushing welding gun, the pulse melting electrode welding power supply is connected to the wire pushing welding gun through a soft insulated cable, a smoking pipe is installed on the upper part of the wire pushing welding gun, the smoking pipe is connected to the smoke purifier, the double-ring weld CNC machine is also provided with two movable and adjustable ball brackets, and a pneumatic ejector is also installed on the movable tailstock.

[0023] The beneficial effects of the present invention are as follows: the present design adopts a double-ring weld CNC machine tool, is equipped with two pulse melting electrode welding power supplies and two automatic wire feeding devices, and two wire push welding gun advancement control mechanisms, and adopts an argon gas protection welding molten pool welding method. Starting the welding program can automatically complete the process technology of the ring welds at both ends of the conductor at one time, replacing ordinary manual non-melting electrode argon arc welding. There is no need to heat the welding part before welding, which reduces the labor intensity of the welder, improves the welding speed and labor efficiency, improves the working environment, and is beneficial to the occupational health and safety of employees. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 A schematic diagram of a process flow of a double-ring weld CNC welding process technology for an aluminum alloy conductive terminal conductor provided by an embodiment of the present invention;

[0026] Figure 2 It is a structural schematic diagram of the double-ring weld CNC machine tool.

[0027] Description of reference numerals:

[0028] 1-Double ring welding CNC machine, 2-Fixed machine head, 3-Mobile tailstock, 4-CNC wire feeder, 5-Pulse melting electrode welding power supply, 6-Wire push welding gun, 7-Chuck, 8-Ball bracket, 9-Pneumatic ejector. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] like Figures 1 to 2 As shown, a CNC welding process technology for double-ring weld of aluminum alloy conductive terminal conductor includes the following steps:

[0031] 1) Cut the terminals and aluminum tubes into the required length using a CNC sawing machine;

[0032] 2) Terminal and aluminum tube processing: use a lathe to perform end face and groove cutting on the terminal and aluminum tube, and use a drilling machine to perform the necessary drilling and tapping operations on the terminal and aluminum tube;

[0033] 3) Adjust the clamping distance of the welding machine, adjust the position of the chuck 7 and the pneumatic ejector 9 on the CNC welding machine, and adjust the appropriate distance according to the clamping length of the workpiece to be processed;

[0034] 4) Adjust the welding position of the welding gun, adjust the push control mechanism of the wire push welding gun 6 on the CNC welding machine, and adjust it to a suitable position according to the length and height of the weld mouth of the workpiece;

[0035] 5) Adjust the position of the mobile fume hood and move the fume purifier's fume pipe to a suitable position to ensure that the welding fume can be sucked into the fume purifier through the fume pipe;

[0036] 6) Adjust the position and height of the bracket 8, and adjust the position and height of the bracket on the CNC welding machine to ensure that the two terminals are parallel to the aluminum tube;

[0037] 7) Clamp the welding workpiece, clamp the workpiece on the CNC welding machine through the chuck 7 and the pneumatic ejector 9, and clamp the terminal and the aluminum tube firmly;

[0038] 8) Connect the argon gas pipeline and turn on the flow meter on the argon gas pipeline;

[0039] 9) Install welding wire and use automatic CNC wire feeder to install welding wire for wire push welding gun;

[0040] 10) Adjust the position of the welding wire and the weld, and adjust the welding wire to extend out of the weld to a suitable distance according to the workpiece to be processed;

[0041] 11) Input or call out the program, input or call out the corresponding welding work program of the workpiece to be processed in the CNC panel of the CNC welding machine tool;

[0042] 12) Check or adjust process parameters to ensure correct processing;

[0043] 13) Turn on the switches on the CNC welding machine, welding power supply, CNC wire feeder 4, wire pusher welding gun 6 and argon gas pipeline; start the automatic welding program and implement double ring weld automatic welding;

[0044] 14) Disassemble the workpiece, loosen the chuck and pneumatic tightening device, and hang down the welded workpiece;

[0045] 15) Repair the weld surface of the workpiece, and repair the defects such as spatter, pile-up, and lack of fusion on the weld surface of the workpiece;

[0046] 16) Weld quality inspection: Use visual inspection or measuring tools to inspect the workpiece after welding to ensure that there are no defects such as pores and lack of fusion on the weld surface.

[0047] Furthermore, the welding equipment used in the welding process includes a CNC welding machine, two smoke purifiers, two pulse melting electrode welding power supplies 5 and two CNC wire feeders 4, and the CNC welding machine is a double-ring weld CNC machine 1, the double-ring weld CNC machine 1 is provided with a fixed machine head 2 and a movable tailstock 3, the fixed machine head 1 is equipped with a CNC system and an adjustment panel, the fixed machine head 2 and the movable tailstock 3 are both equipped with a wire pushing welding gun 6, the CNC wire feeder 4 is installed on the propulsion control mechanism of the wire pushing welding gun 6, the pulse melting electrode welding power supply 5 is connected to the wire pushing welding gun 6 through a soft insulated cable, and the model of the pulse melting electrode welding power supply 5 is Puise MIG-500 adopts argon as the shielding gas to protect the welding pool. By replacing the welding wire and the shielding gas, it can also realize the welding of non-ferrous metals such as carbon steel, stainless steel, copper and copper alloy. The welding power supply can reliably ensure the stability of the output welding voltage and welding current, and improve the quality of welding. A smoking pipe is installed on the upper part of the wire-pushing welding gun 6, and the smoking pipe is connected to the smoke purifier. The smoke generated during welding can be sucked into the smoke purifier through the smoking pipe for purification. The double-ring welding seam CNC machine tool 1 is also provided with two movable and adjustable ball brackets 8 for adjusting the height and parallelism of the weldment. A pneumatic ejector 9 is also installed on the movable tailstock 3 for quickly clamping and fixing the workpiece.

[0048] The design of the present invention adopts a double-ring weld CNC machine tool, is equipped with two pulse melting electrode welding power supplies and two automatic wire feeding devices, and two wire push welding gun advancement control mechanisms, adopts an argon gas protection welding molten pool welding method, and starts the welding program to automatically complete the process technology of the ring welds at both ends of the conductor at one time, replacing ordinary manual non-melting electrode argon arc welding. There is no need to heat the welding part before welding, which reduces the labor intensity of the welder, improves the welding speed and labor efficiency, improves the working environment, and is beneficial to the occupational health and safety of employees.

[0049] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A CNC welding process for double-ring welds of aluminum alloy conductive terminals, characterized in that: The process includes the following steps: 1) Cutting the terminals and aluminum tubes into required lengths using a CNC sawing machine; 2) Processing the terminals and aluminum tubes using a lathe to perform end face and groove cutting on the terminals and aluminum tubes, and using a drilling machine to perform required drilling and tapping operations on the terminals and aluminum tubes; 3) Adjusting the clamping distance of the welding machine, adjusting the position of the chuck and the pneumatic ejector on the CNC welding machine, and adjusting the appropriate distance according to the clamping length of the workpiece to be processed; 4) Adjust the welding position of the wire-pushing welding gun, and adjust the wire-pushing welding gun on the CNC welding machine to a suitable position according to the length of the weld of the workpiece; 5) Adjust the position of the mobile exhaust hood, move the exhaust pipe of the smoke purifier to a suitable position, and ensure that the welding smoke can be sucked into the smoke purifier through the exhaust pipe; 6) Adjust the position and height of the bracket, adjust the position and height of the bracket on the CNC welding machine, and ensure that the two terminals are parallel to the aluminum tube; 7) Clamp the welding workpiece, clamp the workpiece to the CNC welding machine through the chuck and pneumatic ejector, and clamp the two terminals to the aluminum tube firmly; 8) Connect the argon gas pipeline and turn on the flow meter on the argon gas pipeline; 9) Install the welding wire, use the automatic CNC wire feeder to install the welding wire for the wire push welding gun; 10) Adjust the position of the welding wire and the weld, and adjust the welding wire to extend out of the weld to a suitable distance according to the workpiece to be processed; 11) Enter or call out the program, enter or call out the corresponding welding work program of the workpiece to be processed in the CNC panel of the CNC welding machine; 12) Check or adjust the process parameters to ensure that the program is processed correctly; 13) Turn on the switches on the CNC welding machine, welding power supply, CNC wire feeder, wire push welding gun and argon gas pipeline; start the automatic welding program and implement automatic double ring weld welding; 14) Disassemble the workpiece, loosen the chuck and pneumatic clamping device, and hang down the welded workpiece; 15) Trim the weld surface of the workpiece, and trim the defects such as pores and lack of fusion on the weld surface of the workpiece; 16) Weld quality inspection, use visual inspection or measuring tools to inspect the workpiece after welding to ensure that there are no defects such as pores and lack of fusion on the weld surface; The welding equipment used in the welding process includes a CNC welding machine, a smoke purifier, two pulse melting electrode welding power supplies and two CNC wire feeders, and the CNC welding machine is a double-ring weld CNC machine, which is provided with a fixed head and a movable tailstock, the fixed head is equipped with a CNC system and an adjustment panel, the fixed head and the movable tailstock are both equipped with wire pushing welding guns, the CNC wire feeder is installed on the propulsion and control mechanism of the wire pushing welding gun, the pulse melting electrode welding power supply is connected to the wire pushing welding gun through a soft insulated cable, a smoking pipe is installed on the upper part of the wire pushing welding gun, the smoking pipe is connected to the smoke purifier, the double-ring weld CNC machine is also provided with two movable and adjustable ball brackets, and a pneumatic ejector is also installed on the movable tailstock.

Citation Information

Patent Citations

  • Automatic welding platform for double annular welding seams and welding process

    CN102626812A

  • Motorized tungsten electrode argon arc welding method for rotor shield sleeve and rotor protective ring of main pump motor

    CN104384674A

  • Production of rear -axle housing assembly connects device with two circular seam welding

    CN207930245U

  • Aluminum alloy conductive terminal double-end circumferential weld numerical control welding equipment

    CN212665346U

  • Method and apparatus to automatically determine type of gun connected to a wire feeder

    US6855914B1