A tool and a method for welding the tool

By setting tips on the shank of the printed circuit board drill bit and using pressure welding technology, the problem of low welding strength between the blade and the handle is solved, the welding strength and product quality are improved, and cost and environmental pollution are reduced.

CN111975047BActive Publication Date: 2024-11-12SHENZHEN JINZHOU PRECISION TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202010941889.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-09
Publication Date
2024-11-12
Estimated Expiration
2040-09-09

AI Technical Summary

Technical Problem

In the prior art, the welding strength of the blade and the handle of the drill bit for printed circuit board is relatively low, resulting in incomplete bonding of the joint surface and affecting product quality.

Method used

Pressure welding technology is used to weld the handle part to the edge part, and a pointed point part is provided at the end of the handle part. Welding is done by setting the forging force, current and time to ensure that the joint surface is fully integrated.

Benefits of technology

The welding strength between the blade and the handle is improved, the flexural strength and aesthetics of the product are enhanced, the manufacturing cost is reduced, and the occurrence of welding scars is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111975047B_ABST
    Figure CN111975047B_ABST
Patent Text Reader

Abstract

The present invention discloses a tool and a welding method for the tool, which belongs to the technical field of tool processing. The tool comprises: a shank, the shank comprises a body and a first truncated cone structure arranged at one end of the body, the lower bottom surface of the first truncated cone structure is connected to the end of the shank, the shank also comprises a pointed point, the pointed point is arranged on the upper bottom surface of the first truncated cone structure, the pointed point is a cone or a truncated cone, the diameter of the lower bottom surface of the pointed point is the same as the diameter of the upper bottom surface of the first truncated cone structure; a blade; one end of the shank provided with the pointed point is welded to the blade. The welding method of the tool is pressure welding, which is used to weld the blade of the above-mentioned tool to one end of the shank provided with the pointed point. The present invention can solve the technical problem of low welding strength between the shank and the blade existing in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of tool processing, and in particular to a tool and a tool welding method. Background Art

[0002] When processing a hole structure on a printed circuit board, a printed circuit board drill is generally used to drill a hole on the printed circuit board to complete the processing of the hole structure. The printed circuit board drill includes a stainless steel shank and a cemented carbide blade provided at the end of the stainless steel shank, and the cemented carbide blade is provided with a blade for drilling.

[0003] In the prior art, the manufacturing method of the drill bit for printed circuit boards is generally to weld the blade and the shank together.

[0004] However, in the prior art, when welding the blade and the handle, the joint surface may not be fully bonded, resulting in low welding strength.

[0005] Therefore, there is an urgent need for a tool and a welding method for the tool to solve the above problems. Summary of the invention

[0006] The object of the present invention is to provide a tool and a method for welding the tool, so as to solve the technical problem of low welding strength between the handle and the blade in the prior art.

[0007] As conceived above, the technical solution adopted by the present invention is:

[0008] A cutting tool, comprising:

[0009] A handle, the handle comprising a body and a first truncated cone structure provided at one end of the body, the lower bottom surface of the first truncated cone structure being connected to the end of the handle, the handle further comprising a pointed portion, the pointed portion being provided on the upper bottom surface of the first truncated cone structure, the pointed portion being a cone or a truncated cone, and the diameter of the lower bottom surface of the pointed portion being the same as the diameter of the upper bottom surface of the first truncated cone structure;

[0010] Blade;

[0011] One end of the handle portion provided with the pointed portion is welded to the blade portion.

[0012] Optionally, the diameter of the upper bottom surface of the first truncated cone structure is greater than the diameter of the blade portion.

[0013] Optionally, the handle is made of stainless steel, and the blade is made of cemented carbide.

[0014] Optionally, the apex angle of the pointed point is 140°-155°.

[0015] Optionally, the handle is a body of revolution.

[0016] Optionally, the diameter of the upper bottom surface of the first truncated cone structure is 0.6 mm-1.5 mm.

[0017] A method for welding a tool, wherein the method for welding the tool is pressure welding, and is used to weld the blade of the tool to one end of the handle provided with the pointed portion, and comprises the following steps:

[0018] S1, clamping the handle and the blade according to the set position;

[0019] S2. Welding the handle and the blade by using a set upsetting force, a set current, a set time and a set welding curve.

[0020] Optionally, in step S2, the set upsetting force is 15kgf-50kgf.

[0021] Optionally, in step S2, a DC inverter welding power supply or a transistor welding power supply is used to control the set current and the set time.

[0022] Optionally, in step S2, the set current is 500A-2000A, and the set time is 3ms-7ms.

[0023] The tool and the welding method of the tool proposed in the present invention use pressure welding to weld the shank and the blade together during welding. Since the end of the shank is provided with a sharp point, the sharp point can ensure that the welding position is concentrated, so that the shank and the blade are completely combined at the joint surface, thereby improving the welding strength of the joint and further improving the product quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is a schematic structural diagram of a handle provided by an embodiment of the present invention;

[0025] Figure 2 is a schematic structural diagram of a sharp point portion provided by an embodiment of the present invention;

[0026] Figure 3 is a schematic structural diagram of a tool provided by an embodiment of the present invention;

[0027] Figure 4 is a schematic diagram of the handle and the blade abutting against each other before welding provided by an embodiment of the present invention;

[0028] Figure 5 It is a schematic cross-sectional view of the welding surface after the shank and the blade are welded according to an embodiment of the present invention.

[0029] In the figure:

[0030] 1. handle; 11. first truncated cone structure; 111. point;

[0031] 2. Blade;

[0032] 9. Gap. DETAILED DESCRIPTION

[0033] In order to make the technical problems solved by the present invention, the technical solutions adopted and the technical effects achieved clearer, the technical solutions of the present invention are further described below in conjunction with the accompanying drawings and through specific implementation methods. It is understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention. It should also be noted that, for the convenience of description, only the parts related to the present invention are shown in the accompanying drawings, not all.

[0034] In the description of the present invention, it should be noted that the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance. Among them, the terms "first position" and "second position" are two different positions.

[0035] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection or a detachable connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0036] See also Figure 1-Figure 3 The present embodiment provides a tool, including a handle 1 and a blade 2, both of which are rotating body structures, and the axes of the handle 1 and the blade 2 coincide. Specifically, in the present embodiment, the tool is a drill bit for printed circuit boards, the handle 1 is made of stainless steel, and the blade 2 is made of cemented carbide.

[0037] The handle 1 includes a body and a first truncated cone structure 11 disposed at one end of the body, the lower bottom surface of the first truncated cone structure 11 is connected to the end of the handle 1, and the handle 1 also includes a sharp point 111, which is disposed on the upper bottom surface of the first truncated cone structure 11. The sharp point 111 is a cone or a truncated cone, and the diameter of the lower bottom surface of the sharp point 111 is the same as the diameter of the upper bottom surface of the first truncated cone structure 11. One end of the handle 1 provided with the sharp point 111 is welded to the blade 2, and the axes of the handle 1 and the blade 2 coincide after welding.

[0038] As is known, the upper bottom surface of the truncated cone structure is an end surface of the truncated cone with a smaller cross-sectional area, and the lower bottom surface of the truncated cone structure is an end surface of the truncated cone with a larger cross-sectional area.

[0039] Specifically, in this embodiment, the end face of the blade 2 is the blade welding surface, and the blade welding surface is formed into a plane by alloy cutting or direct die-casting. The handle 1 is formed by grinding or turning to form a sharp point 111.

[0040] The tool provided in this embodiment uses pressure welding to weld the shank 1 and the blade 2 together. Since the end of the shank 1 is provided with a pointed portion 111, the welding position can be ensured to be concentrated, so that the shank 1 and the blade 2 are completely combined at the joint surface, thereby improving the welding strength of the joint and further improving the product quality.

[0041] Specifically, in the present embodiment, the handle 1 is an integrally formed structure, and one end of the handle 1 away from the pointed portion 111 is provided with a chamfer.

[0042] In order to further improve the welding strength between the handle 1 and the blade 2, preferably, the diameter of the upper bottom surface of the first truncated cone structure 11 is larger than the diameter of the blade 2. Since the diameter of the lower bottom surface of the pointed portion 111 is the same as the diameter of the upper bottom surface of the first truncated cone structure 11, the diameter of the lower bottom surface of the pointed portion 111 is larger than the diameter of the blade 2.

[0043] See also Figure 4 Before welding, the top of the sharp point portion 111 is brought into contact with the end face of the blade portion 2. Since the sharp point portion 111 is a cone or a truncated cone, there is a gap 9 between the side face of the sharp point portion 111 and the end face of the blade portion 2.

[0044] If the diameter of the lower bottom surface of the pointed portion 111 is smaller than the diameter of the blade 2, in order to ensure that the shank 1 and the blade 2 can be fully and completely fused together during welding, a larger volume of the shank 1 needs to be melted, which requires a larger welding heat. Excessive welding heat may cause the surface and interior of the blade 2 made of cemented carbide to break.

[0045] When the diameter of the lower bottom surface of the pointed portion 111 is smaller than the diameter of the blade 2, after welding is completed, a destructive pressure test is performed on the blade 2 at a position 3 mm away from the welding surface, and its flexural strength is only 2.8 kgf. During use, the blade 2 is very likely to fail or even break.

[0046] In this embodiment, the diameter of the lower bottom surface of the sharp point portion 111 is larger than the diameter of the blade portion 2, and the volume of the shank portion 1 that needs to be melted during the welding process is smaller, and the welding heat required is also smaller, and the molten part of the shank portion 1 is just filled into the gap 9 between the shank portion 1 and the blade portion 2. That is, in this embodiment, the diameter of the lower bottom surface of the sharp point portion 111 is larger than the diameter of the blade portion 2, which can ensure that the shank portion 1 and the blade portion 2 are fully combined under the condition of moderate welding energy and without damaging the blade portion 2.

[0047] Specifically, see Figure 5 , Figure 5 It is a schematic cross-sectional view of the welding surface formed after the shank 1 and the blade 2 are welded, wherein area A is the area where the molten part of the shank 1 fills the gap 9, area B is the area where the shank 1 and the blade 2 are fully penetrated, and area C is the bonding area of ​​the part of the shank 1 and the blade 2 exposed at high temperature.

[0048] The smaller the cross-sectional area of ​​the C region, the higher the bending strength of the tool. The structure of the handle 1 in this embodiment can minimize the C region after pressure welding. In a destructive pressure test under the same conditions, the bending strength of the tool in this embodiment can reach 5.5 kgf, which is nearly doubled.

[0049] At the same time, in this embodiment, the diameter of the lower bottom surface of the pointed portion 111 is larger than the diameter of the blade portion 2, so that the volume of the handle portion 1 that needs to be melted during welding is smaller, thereby significantly reducing the weld scar after welding is completed.

[0050] Furthermore, in this embodiment, the value obtained by subtracting the diameter of the blade 2 from the diameter of the lower bottom surface of the pointed portion 111 does not exceed 0.4 mm. Compared with the structure in which the diameter of the lower bottom surface of the pointed portion 111 is smaller than the diameter of the blade 2, the efficiency of the tool in this embodiment will be doubled during the post-grinding process.

[0051] Optionally, the apex angle of the pointed portion 111 is 140°-155°.

[0052] If the diameter of the blade to be welded is less than or equal to 0.5 mm, the diameter of the upper bottom surface of the first truncated cone structure 11 is 0.6 mm-1.5 mm, that is, in this embodiment, the diameter of the lower bottom surface of the pointed portion 111 is 0.6 mm-1.5 mm.

[0053] Specifically, Figure 3 The angle α is used to represent the vertex angle of the sharp point portion 111, and α is 140°-155°; Figure 3 In FIG. 1 , d represents the diameter of the lower bottom surface of the pointed portion 111 .

[0054] If the pointed portion 111 is a truncated cone, the diameter of the upper bottom surface of the pointed portion 111 does not exceed 0.2 mm.

[0055] This embodiment also provides a method for welding a tool, which is used to weld the blade 2 of the tool to an end of the handle 1 provided with a sharp point 111 .

[0056] Specifically, the welding method provided in this embodiment is applicable to the welding of knives with a blade 2 having a diameter not greater than 0.5 mm, and is also applicable to the welding of knives with a blade 2 having a diameter of 0.5 mm-1.35 mm.

[0057] The welding method is pressure welding, comprising the following steps:

[0058] S1, clamping the handle 1 and the blade 2 according to the set position;

[0059] Specifically, before step S1, the handle 1 and the blade 2 need to be cleaned to remove foreign matter on the welding end surface to ensure a stable welding process.

[0060] Specifically, in step S1, the handle 1 and the blade 2 are clamped on a material bracket, and the material bracket is placed in a pressure welding device. Further, the handle 1 is clamped on the handle bracket, and the blade 2 is clamped on the blade bracket, so that the end of the point portion 111 abuts against the end surface of the blade 2.

[0061] S2. Welding the handle 1 and the blade 2 by using a set upsetting force, a set current, a set time and a set welding curve.

[0062] The upsetting force refers to the compressive force applied to the workpieces during welding, in order to ensure close contact between the workpieces during welding. Sufficient upsetting force is required to ensure full contact and fusion between the workpieces. If the upsetting force is too large, it will lead to poor fusion of the workpieces, insufficient welding strength, and may also easily cause cracks and breakage on the blade 2 made of cemented carbide; if the upsetting force is too small, it will lead to loose fusion and insufficient welding strength. Therefore, it is necessary to select a suitable upsetting force for welding.

[0063] Specifically, in step S2, the upset force is set to 15kgf-50kgf. Specifically, the handle 1 and the blade 2 are subjected to external force by a spring, a cylinder or a motor, etc., to ensure that there is an upset force of 15kgf-50kgf between the two.

[0064] It can be known from Joule's law that the greater the welding current, the greater the welding energy. During the welding process, if the welding current is too large, the welding part will be deformed, and the blade 2 made of cemented carbide will easily become brittle and break; if the welding current is too small, the welding part will not have enough heat, which will seriously affect the welding strength. Therefore, the welding current needs to be strictly controlled.

[0065] Specifically, in step S2, the current is set to 500A-2000A.

[0066] Welding time has a certain impact on the fusion size and weld strength. If the welding time is too long, it will lead to a large loss of welding heat, which will lead to greater loss and unreliable welding quality; if the welding time is too short, it will lead to insufficient welding and low weld strength.

[0067] By selecting appropriate welding current and welding time, the welding quality can be best.

[0068] In step S2, the time is set as welding time, and the set time is 3ms-7ms.

[0069] Furthermore, in step S2, a DC inverter welding power supply or a transistor welding power supply is used to control the set current and the set time.

[0070] According to the different steel handle and alloy materials, reasonable selection of welding curves can further improve the welding quality. Optionally, the welding curve can be set to a single-stage welding curve, a double-stage welding curve or a multi-stage welding curve.

[0071] Specifically, each welding curve includes three stages: an ascending curve, a stable curve and a descending curve. Preferably, the time occupied by the stable curve needs to account for more than 50% of the total welding time.

[0072] Through the proposed welding curve boundary, the welding process can be effectively controlled in a stable state.

[0073] The welding method provided in this embodiment adopts pressure welding to weld the handle 1 and the blade 2. Since the end of the handle 1 is provided with a sharp point 111, it can ensure that the welding position is concentrated, so that the handle 1 and the blade 2 are completely combined at the joint surface, thereby improving the welding strength of the joint and further improving the product quality.

[0074] In the prior art, the blade and the handle are welded together by brazing. Brazing requires welding sheets and flux as auxiliary materials for welding. However, welding sheets are generally expensive metals such as silver and manganese, resulting in high manufacturing costs; the flux is mainly a lipid compound, which will produce white smoke with a peculiar smell during heating, affecting the processing environment and the health of the processing personnel. In addition, the flux left on the handle will produce welding scars and even cause rust when volatilizing, affecting the appearance of the product.

[0075] The welding method provided in this embodiment uses pressure welding to weld the handle 1 and the blade 2. Compared with brazing in the prior art, it reduces welding costs, does not pollute the processing environment, and can also improve the appearance of the product.

[0076] The above embodiments are only to illustrate the basic principles and characteristics of the present invention. The present invention is not limited by the above embodiments. Without departing from the spirit and scope of the present invention, the present invention may be subject to various changes and modifications, which are within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A cutting tool, characterized in that: include: A handle (1), the handle (1) comprising a body and a first truncated cone structure (11) arranged at one end of the body, the lower bottom surface of the first truncated cone structure (11) being connected to the end of the handle (1), the handle (1) further comprising a pointed portion (111), the pointed portion (111) being arranged on the upper bottom surface of the first truncated cone structure (11), the pointed portion (111) being a cone or a truncated cone, the diameter of the lower bottom surface of the pointed portion (111) being the same as the diameter of the upper bottom surface of the first truncated cone structure (11); Blade (2); One end of the handle (1) provided with the pointed portion (111) is welded to the blade (2); The diameter of the upper bottom surface of the first truncated cone structure (11) is greater than the diameter of the blade portion (2); The diameter of the upper bottom surface of the first truncated cone structure (11) is 0.6 mm to 1.5 mm; The value obtained by subtracting the diameter of the blade (2) from the diameter of the lower bottom surface of the pointed portion (111) does not exceed 0.4 mm.

2. The tool according to claim 1, characterized in that The material of the handle (1) is stainless steel, and the material of the blade (2) is hard alloy.

3. The tool according to claim 1, characterized in that The apex angle of the pointed portion (111) is 140°-155°.

4. The tool according to claim 1, characterized in that The handle (1) is a rotating body.

5. A method for welding a tool, characterized in that: The welding method of the tool is pressure welding, which is used to weld the blade (2) of the tool according to any one of claims 1 to 4 to one end of the handle (1) provided with the sharp point (111), comprising the following steps: S1, clamping the handle (1) and the blade (2) according to a set position; S2. Welding the handle (1) and the blade (2) by using a set upsetting force, a set current, a set time and a set welding curve.

6. The welding method according to claim 5, characterized in that: In the step S2, the set upsetting force is 15kgf-50kgf.

7. The welding method according to claim 6, characterized in that: In the step S2, a DC inverter welding power supply or a transistor welding power supply is used to control the set current and the set time.

8. The welding method according to claim 7, characterized in that: In the step S2, the set current is 500A-2000A, and the set time is 3ms-7ms.

Citation Information

Patent Citations

  • Wolfram steel drill bit

    CN206981822U

  • Single-blade reverse forming cutter for machining inner hole of martensitic stainless steel valve body

    CN209272568U

  • Cutter

    CN212443386U

  • Drill

    JP2005014115A