Composite component consisting of three stacked mating parts
By using solders with different melting temperatures and designing solder compensation openings in power electronic devices, the problem of sinking of joint mating parts caused by volume shrinkage during reflow soldering is solved, stable electrical and thermal connections are achieved, and functions are improved. performance.
Patent Information
- Application Number
- CN201980031989.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-05-10
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-05-10
AI Technical Summary
In power electronic devices, the volume shrinkage during reflow soldering causes the joint mating parts to sink, resulting in reduced connection area, increased resistance and thermal resistance, reduced functionality, and even shortened life.
By selecting the appropriate geometry of the brazing material and the joining partner, using filler metals with different melting temperatures between the upper and lower brazing layers and designing upwardly open solder compensation openings in the upper joining partner , to fill the gap during the brazing process, compensate for the volume shrinkage, and ensure a stable connection between the joined mating parts.
The structural functionality in terms of electrical connection and thermal heat dissipation is achieved beyond the tolerance range, ensuring stable connection between mating mating parts, and improving the quality of electrical connection and thermal connection.
Smart Images

Figure CN112136210B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a composite component consisting of three stacked mating parts. A method for connecting a stack consisting of three mating parts is also the subject of the invention. Background Art
[0002] The structural elements or joint partners in power electronic devices are usually thermally and electrically connected to each other through a reflow soldering process. In order to be able to cost-effectively manufacture complex structures with multiple structural elements or joint partners and soldering locations, all the connection locations are soldered in one step. During this process, about 50% volume shrinkage occurs in the solder. This causes the upper structural element or joint partner to sink to the lower structural element or lower joint partner. In a stack consisting of three joint partners, in which the upper joint partner and the lower joint partner are fixed at their height, such sinking is impossible due to the structure. Due to the volume shrinkage during the soldering process, a reduction in the solder connection area and / or a shrinkage cavity may result. This can lead to an increase in electrical resistance and thermal resistance and thus a reduction in functionality and even a reduction in life.
[0003] Document DE 102 52 577 B4 discloses a method for producing a solder connection by capillary solder flow. The disclosed method for connecting a first soldering partner and a second soldering partner comprises the following steps: placing a first soldering partner, a second soldering partner and a solder pile so that the surface of the first soldering partner is opposite to the surface of the second soldering partner, and the solder pile is arranged outside the connection area of the opposite surfaces and adjacent to the connection area, wherein the opposite surfaces of the soldering partners in the connection area can be wetted by the solder of the solder pile, and heating the soldering partners and the solder pile so that the solder pile melts and is pulled into the connection area by capillary forces, so as to connect the soldering partners through a connection layer. Here, the first soldering partner is a substrate and the second soldering partner is a semiconductor component, and the semiconductor component is smaller than the substrate. Summary of the invention
[0004] The composite assembly of the present invention, which is composed of three stacked mating parts, and the method for connecting a laminate composed of three mating parts, respectively have the advantage that the volume shrinkage during the soldering process in the laminate composed of three mating parts can be compensated by appropriately selecting the solder and the geometry of the mating parts. This ensures that the mating parts are connected to each other with a sufficiently large area. The structural functionality in terms of electrical connection and heat dissipation is ensured in an advantageous manner over all tolerance ranges.
[0005] An embodiment of the present invention provides a composite assembly consisting of three stacked joint partners, which are connected to each other by an upper solder layer and a lower solder layer material connection, wherein the upper joint partner and the lower joint partner are fixed in terms of their height and have a predetermined distance between each other. Here, an upper solder layer formed by a first solder having a first melting temperature is constructed between the upper joint partner and the middle joint partner, and a second solder layer formed by a second solder having a higher second melting temperature is constructed between the middle joint partner and the lower joint partner. In addition, the upper joint partner has an upwardly open solder compensation opening filled with a first solder, and the first solder flows from the solder compensation opening into the gap between the upper joint partner and the middle joint partner to fill the gap.
[0006] In addition, a method for connecting a stack consisting of three joining partners is proposed, wherein the upper joining partner and the lower joining partner are fixed in terms of their height and have a predetermined distance from each other. The method comprises the following steps: applying a first solder paste to a first solderable surface of the upper joining partner and a second solderable surface of the middle joining partner, so that the gap between the upper joining partner and the middle joining partner is filled with the first solder paste, and the first solder of the first solder paste has a first melting temperature. Filling the upwardly open solder compensation opening in the first joining partner with the first solder paste, applying a second solder paste to a third solderable surface of the middle joining partner and a fourth solderable surface of the lower joining partner, so that the gap between the middle joining partner and the lower joining partner is filled with the second solder paste, and the second solder of the second solder paste has a higher second melting temperature. Placing the stack in a reflow soldering furnace The lower solder layer is heated to a temperature above the second melting temperature and the stack is subsequently cooled so that during the cooling phase first the lower solder layer solidifies, while the upper solder layer is still molten and causes the intermediate joining partner to descend and the intermediate joining partner to be connected to the lower joining partner over its entire surface, wherein the now larger gap between the intermediate joining partner and the upper joining partner is supplementally filled with the molten solder from the upwardly open solder compensation opening, so that the intermediate joining partner is connected to the upper joining partner over its entire surface while the solder compensation opening is left empty.
[0007] As the first solder, for example, tin-silver-copper solder (SAC) can be used. As the second solder, for example, tin-copper solder (SnCu) can be used, which has a higher melting point than tin-silver-copper solder (SAC) and solidifies first during the cooling process.
[0008] The above-described composite assembly consisting of three stacked joining partners can be advantageously improved by means of the measures and developments listed below.
[0009] It is particularly advantageous that the upper solder layer can be formed over the entire surface between the first solderable surface of the upper joint partner and the second solderable surface of the middle joint partner when the solder compensation opening is left empty. The lower solder layer can be formed over the entire surface between the third solderable surface of the middle joint partner and the fourth solderable surface of the lower joint partner. By connecting the individual joint partners to each other by material bonding over the entire surface, an optimal electrical and thermal connection can be achieved in an advantageous manner.
[0010] In an advantageous embodiment of the composite assembly, the upwardly open solder compensation opening can be formed above the second solderable surface of the intermediate joint partner and penetrate the first solderable surface, so that the first solder can flow directly into the gap between the upper joint partner and the intermediate joint partner during the soldering process.
[0011] In another advantageous embodiment of the composite component, the upwardly open solder compensation opening has a volume that is at least twice the volume of the gap between the upper joining partner and the middle joining partner. This advantageously ensures that a sufficient amount of first solder can flow into the gap between the upper joining partner and the middle joining partner even in the event of a large volume contraction.
[0012] In another advantageous embodiment of the composite component, the first joining partner may be, for example, a stamped grid, the second joining partner may be, for example, a DBC substrate (DBC: Direct Bonded Copper), and the third joining partner may be, for example, a heat sink.
[0013] Here, the first DBC copper structure can form a second solderable surface of the second joint partner, and the second DBC copper structure can form a third solderable surface of the second joint partner. The DBC substrate can advantageously provide very good electrical insulation and very good thermal conductivity between the stamped grid and the heat sink. In addition, the first solder layer and the second solder layer have a significantly lower electrical resistance than a bonded connection. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Embodiments of the present invention are shown in the drawings and explained in detail in the following description. In the drawings, the same reference numerals represent components or elements that implement the same or similar functions.
[0015] Figure 1 A schematic cross-sectional view of a first exemplary embodiment of a composite assembly according to the invention, consisting of three stacked joining partners, is shown before the soldering process.
[0016] Figure 2 Shows Figure 1The illustrated schematic cross-section of a composite component according to the invention after the soldering process.
[0017] Figure 3 A schematic plan view of a detail of a circuit module is shown, which has a second exemplary embodiment of a composite assembly according to the invention, which is composed of three stacked joining partners.
[0018] Figure 4 Shows Figure 3 The composite component according to the invention is shown in a schematic sectional view along the section line IV-IV.
[0019] Figure 5 Shows Figure 3 Schematic sectional view of a composite component according to the invention along the section line VV in FIG. DETAILED DESCRIPTION
[0020] As in Figures 1 to 5 As shown in the figure, the illustrated embodiment of the composite assembly 1, 1A according to the present invention, which is composed of three stacked joint partners 10, 20, 30, respectively comprises an upper joint partner 10, an intermediate joint partner 20 and a lower joint partner 30, which are connected to each other by an upper solder layer 3 and by a lower solder layer 5. Here, the upper joint partner 10 and the lower joint partner 30 are fixed in their height and have a predetermined distance H from each other. The upper solder layer 3 formed by a first solder having a first melting temperature is constructed between the upper joint partner 10 and the intermediate joint partner 20. The second solder layer 5 formed by a second solder having a higher second melting temperature is constructed between the intermediate joint partner 20 and the lower joint partner 30. In addition, the upper joint partner 10 has a solder compensation opening 14 that is open upward and filled with the first solder, and the first solder flows from the solder compensation opening into the gap between the upper joint partner 10 and the intermediate joint partner 20 to fill the gap.
[0021] like Figures 1 to 5 As further shown in the figure, the upper solder layer 3 is formed in its entirety between the solderable first surface 12 of the upper joint partner 10 and the solderable second surface 22 of the middle joint partner 20, while the solder compensation opening 14 is left open. The lower solder layer 5 is formed in its entirety between the solderable third surface 24 of the middle joint partner 20 and the solderable fourth surface 32 of the lower joint partner 30.
[0022] like Figures 1 to 5As further shown in the figure, the upwardly open solder compensation opening 14 is formed in the illustrated embodiment above the solderable second surface 22 of the intermediate joint partner 20 and passes through the solderable first surface 12 of the upper joint partner 10. In addition, the upwardly open solder compensation opening 14 has a volume that is at least twice the volume of the gap between the upper joint partner 10 and the intermediate joint partner 20.
[0023] like Figures 3 to 5 As further shown in the figure, the second embodiment of the composite assembly 1A according to the invention is composed of three bonding partners 10, 20, 30, which are part of a circuit module. Here, the first bonding partner 10 is a stamped grid 10A, the second bonding partner 20 is a DBC substrate 20A (DBC: Direct Bonded Coper) and the third bonding partner 30 is a heat sink 30A. In addition, the first DBC copper structure 22A forms the second solderable second surface 22 of the second bonding partner 20, and the second DBC copper structure 24A forms the third solderable surface 22 of the second bonding partner 20.
[0024] An embodiment of the method according to the invention for connecting a stack consisting of three joining partners 10, 20, 30, wherein the upper joining partner 10 and the lower joining partner 30 are fixed in their height and have a predetermined distance H from each other, comprises the following steps: Applying a first solder paste to a solderable first surface 12 of the upper joining partner 10 and to a solderable second surface 22 of the middle joining partner 20, so that the gap between the upper joining partner 10 and the middle joining partner 20 is filled with the first solder paste, the first solder of which has a first melting temperature. Filling the upwardly open solder compensation opening 14 in the first joining partner 10 with the first solder paste. Applying a second solder paste to a solderable third surface 24 of the middle joining partner 20 and to a solderable fourth surface 32 of the lower joining partner 30, so that the gap between the middle joining partner 20 and the lower joining partner 30 is filled with a second solder paste, the second solder of which has a higher second melting temperature. Figure 1 The stack prepared in this way is shown, which consists of three joining partners 10, 20, 30, before the soldering process in a reflow soldering furnace. Figure 1 As further shown in the figure, in the embodiment shown, the gap between the upper joint partner 10 and the middle joint partner 20 and the gap between the lower joint partner 30 and the middle joint partner 20 are respectively completely filled with corresponding solder pastes. In the embodiment shown, the upwardly open solder compensation opening 14 in the first joint partner 10 is also completely filled with the first solder paste.
[0025] The stack is heated to a temperature above the second melting temperature in a reflow soldering furnace. The stack is then cooled so that during the cooling phase, the lower solder layer 5 solidifies first, while the upper solder layer 3 is still molten and causes the intermediate joint partner 20 to be lowered and the intermediate joint partner 20 to be connected to the lower joint partner 30 over its entire surface. The now larger gap between the intermediate joint partner 20 and the upper joint partner 10 is supplemented with the molten solder from the upwardly open solder compensation opening 14, so that the intermediate joint partner 20 is connected to the upper joint partner 10 over its entire surface while the solder compensation opening 14 is left empty.
[0026] Figure 2 The stack of three joining partners 10, 20, 30 is shown after the soldering process. Figure 2 It can be further seen that the first solder introduced into the solder compensation opening 14 before the soldering process flows almost completely into the gap between the upper joining partner 10 and the intermediate joining partner 20 in order to compensate for the volume loss of the first solder and the lowering of the intermediate joining partner 20 during the soldering process in the reflow soldering furnace.
[0027] In the embodiment shown, a tin-silver-copper solder (SAC) is used as the first solder for the upper solder layer 3. In the embodiment shown, a tin-copper solder (SnCu) having a higher melting point than the tin-silver-copper solder (SAC) of the first solder layer 3 is used as the second solder for the lower solder layer 5. As a result, the second solder of the lower solder layer 5 solidifies before the first solder of the upper solder layer 3 during the cooling process.
[0028] Embodiments of the invention can be used, for example, for all power modules in an inverter and can generally also be used in molded switching modules with reduced power.
Claims
1. A composite assembly (1, 1A) consisting of three stacked joining partners (10, 20, 30), the joining partners being materially connected to one another via an upper solder layer (3) and via a lower solder layer (5), wherein the upper joining partner (10) and the lower joining partner (30) are fixed in height and have a predetermined distance (H) from one another, wherein the upper solder layer (3) formed of a first solder having a first melting temperature is formed between the upper joining partner (10) and the middle joining partner (20), and the lower solder layer (5) formed of a second solder having a higher second melting temperature is formed between the middle joining partner (20) and the lower joining partner (30), and wherein the upper joining partner (10) has an upwardly open solder compensation opening (14) filled with the first solder, the first solder flowing from the solder compensation opening into a gap between the upper joining partner (10) and the middle joining partner (20) in order to fill the gap, It is characterized in that The upper solder layer (3) is formed over its entire surface between a first solderable surface (12) of the upper joining partner (10) and a second solderable surface (22) of the middle joining partner (20) while leaving the solder compensation opening (14) open, and the lower solder layer (5) is formed over its entire surface between a third solderable surface (24) of the middle joining partner (20) and a fourth solderable surface (32) of the lower joining partner (30).
2. The composite component (1, 1A) according to claim 1, It is characterized in that The solder compensation opening (14) which is open upward is formed above the second solderable surface (22) of the intermediate joining partner (20) and passes through the first solderable surface (12).
3. The composite component (1, 1A) according to claim 1 or 2, It is characterized in that The solder compensation opening (14) open upward has a volume which is at least twice the volume of the gap between the upper joining partner (10) and the middle joining partner (20).
4. The composite component (1, 1A) according to claim 1 or 2, It is characterized in that The upper joint partner (10) is a stamped grid (10A).
5. The composite component (1, 1A) according to claim 1 or 2, It is characterized in that The intermediate bonding partner (20) is a DBC substrate (20A).
6. The composite component (1, 1A) according to claim 5, It is characterized in that The first DBC copper structure (22A) forms a solderable second surface (22) of the intermediate joint partner (20), and the second DBC copper structure (24A) forms a solderable third surface (24) of the intermediate joint partner (20).
7. The composite component (1, 1A) according to claim 1 or 2, It is characterized in that The lower engagement partner (30) is a heat sink (30A).
8. A method for connecting a stack of three joining partners (10, 20, 30), wherein the upper joining partner (10) and the lower joining partner (30) are fixed in their height and have a predetermined distance (H) from one another, the method comprising the following steps: A first solder paste is applied to a solderable first surface (12) of the upper joining partner (10) and a solderable second surface (22) of the middle joining partner (20), thereby filling a gap between the upper joining partner (10) and the middle joining partner (20) with the first solder paste to form an upper solder layer (3), wherein a first solder material of the first solder paste has a first melting temperature, filling the upwardly open solder compensation opening (14) in the upper bonding partner (10) with the first solder paste, A second solder paste is applied to the solderable third surface (24) of the middle joining partner (20) and the solderable fourth surface (32) of the lower joining partner (30), thereby filling the gap between the middle joining partner (20) and the lower joining partner (30) with the second solder paste to form a lower solder layer (5), wherein the second solder material of the second solder paste has a second higher melting temperature, heating the laminate in a reflow soldering furnace to a temperature above the second melting temperature, and The stack is subsequently cooled so that during the cooling phase the lower solder layer (5) solidifies first, while the upper solder layer (3) is still molten, and this causes the intermediate joining partner (20) to descend and the intermediate joining partner (20) to be connected over its entire surface to the lower joining partner (30), wherein the larger gap between the intermediate joining partner (20) and the upper joining partner (10) is filled with molten solder from the solder compensating opening (14) open upward, thereby achieving a connection of the intermediate joining partner (20) to the upper joining partner (10) over its entire surface while the solder compensating opening (14) is left empty.
Citation Information
Patent Citations
Process for producing a solder joint by capillary solder flow
DE10252577B4
Semiconductor device and its manufacturing method
JP2004303869A
Semiconductor device
JP2006066716A
Semiconductor device
WO2018021322A1