Wafer mounting table and method for manufacturing the same

By filling the sintered conductor in the mesh electrode of the wafer mounting stage, the contact area between the connecting parts and the mesh electrode is increased, the problem of heating of the connecting parts in the prior art is solved, and the heat homogenization of the wafer is improved.

CN112185925BActive Publication Date: 2024-11-19NGK INSULATORS LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202010618886.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-01
Filing Date
2020-06-30
Publication Date
2024-11-19
Estimated Expiration
2040-06-30

AI Technical Summary

Technical Problem

The existing wafer is mounted in the table, and the contact area between the connecting parts and the grid electrode is small, which leads to an increase in the heat generation near the connecting parts when powered on, affecting the heat homogenization of the wafer.

Method used

The mesh opening in the mesh electrode is filled with a sintered conductor, which contains a mixture of conductive powder and ceramic raw materials, increases the contact area between the connecting parts and the mesh electrode, reduces the resistance value, and suppresses heat generation.

Benefits of technology

By increasing the contact area, the resistance value of the connecting component and the grid electrode is reduced, the heating is reduced, and the heat homogenization of the wafer is improved, especially at high-frequency voltages, which effectively suppresses the heating of the connecting component.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112185925B_ABST
    Figure CN112185925B_ABST
Patent Text Reader

Abstract

The present invention provides a wafer loading table (10), comprising a ceramic component (12) having a wafer loading surface (12a), a grid electrode (14) embedded in the ceramic component (12), a conductive connecting component (16) contacting the grid electrode (14) and exposed to the outside from a surface (12b) of the ceramic component (12) opposite to the wafer loading surface (12a), and an external current-carrying component (18) joined to the surface of the connecting component (16) exposed to the outside. A sintered conductor (15) is filled in a grid opening (14a) located in a region of the grid electrode (14) facing the connecting component (16), the sintered conductor being a sintered body containing a mixture of conductive powder and a ceramic raw material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a wafer mounting table and a manufacturing method thereof. Background Art

[0002] As a wafer stage, a device described in Patent Document 1 is known. Patent Document 1 discloses a wafer stage having a ceramic component, a grid electrode, a conductive connection component, and an external power supply component as such a wafer stage. The ceramic component has a wafer mounting surface. The grid electrode is embedded in the ceramic component. The connection component contacts the grid electrode and is exposed to the outside from the surface of the ceramic component on the opposite side to the wafer mounting surface. The external power supply component is bonded to the surface of the connection component exposed to the outside via a bonding layer.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: International Publication No. 2015 / 198892 Pamphlet Summary of the invention

[0006] Problems to be solved by the invention

[0007] However, since the connection component is in contact with the grid electrode line, the actual contact area between the contact component and the grid electrode is small. Therefore, when current flows from the external current-carrying component to the grid electrode via the connection component, the heat generated near the connection component increases, and sometimes the thermal uniformity of the chip is impaired.

[0008] The present invention has been made to solve such a problem, and a main object of the present invention is to suppress heat generation of a connecting member when electricity is supplied to a mesh electrode.

[0009] Solutions to Solve Problems

[0010] The wafer stage of the present invention comprises:

[0011] A ceramic component having a wafer mounting surface;

[0012] A grid electrode embedded in the ceramic component;

[0013] a conductive connection member that contacts the grid electrode and is exposed to the outside from a surface of the ceramic member that is opposite to the wafer placement surface; and

[0014] an external current-carrying member connected to the surface of the connecting member exposed to the outside,

[0015] The wafer stage is characterized in that:

[0016] The mesh openings in the mesh electrode in the region facing the connection member are filled with a sintered conductor, which is a sintered body containing a mixture of conductive powder and a ceramic raw material.

[0017] In the wafer stage, a sintered conductor is filled in a mesh opening in a region of the mesh electrode that is located opposite to the connection component. The sintered conductor is a sintered body containing a mixture of conductive powder and ceramic raw material (granules or powder). The connection component is in contact with the mesh electrode through the sintered conductor in addition to the line contact constituting the mesh electrode. Therefore, the actual contact area between the connection component and the mesh electrode is larger than that of the prior art. As a result, the resistance value between the connection component and the mesh electrode is lower than that of the prior art, and the heating of the connection component when the current from the external current-carrying component flows to the mesh electrode through the connection component can be suppressed.

[0018] In the wafer stage of the present invention, the grid electrode may be an RF electrode to which a high-frequency voltage is applied. When a high-frequency voltage is applied to the grid electrode, the connection component itself is easily heated by the high-frequency current flowing from the external energizing component to the grid electrode via the connection component. However, since the resistance value between the connection component and the grid electrode is lower than that of the prior art as described above, the heating of the connection component itself can be suppressed.

[0019] In the wafer stage of the present invention, the mesh openings may be square with a side length of 0.3 mm to 1 mm, and the conductive powder may have a particle size of 1 μm to 10 μm.

[0020] In the wafer stage of the present invention, the conductive powder is preferably a powder of the same material as the mesh electrode. In this way, since the thermal expansion coefficients of the sintered conductor and the mesh electrode are close to each other, it is possible to prevent the ceramic component from cracking due to thermal stress. In addition, the thermal expansion coefficients of the conductive powder and the mesh electrode are preferably close to each other.

[0021] The method for manufacturing a wafer stage of the present invention is characterized by comprising the following steps:

[0022] (a) a grid electrode is arranged on a substrate which is a ceramic formed body or a ceramic sintered body, and a conductive powder is placed in a grid opening located in a predetermined area of ​​the grid electrode;

[0023] (b) disposing a conductive connecting member on the predetermined area of ​​the grid electrode;

[0024] (c) laminating a ceramic raw material on the substrate so as to cover the grid electrode and the connection member to form a laminate;

[0025] (d) hot pressing and firing the laminate to integrate the substrate and the ceramic raw material to form a ceramic component; and

[0026] (e) A hole is formed in the ceramic component so as to reach the connecting component from the surface opposite to the wafer mounting surface, an external conducting component is inserted into the hole, and the external conducting component is joined to the exposed surface of the connecting component.

[0027] According to this method of manufacturing a wafer stage, the wafer stage of the present invention described above can be manufactured relatively easily. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a longitudinal sectional view of the main part of the wafer stage 10.

[0029] Figure 2 is a partial top view of the grid electrode 14 .

[0030] Figure 3 It is a manufacturing process diagram of the wafer stage 10.

[0031] Figure 4 It is a longitudinal sectional view of the main parts of the first reference example.

[0032] Figure 5 It is a longitudinal sectional view of the main parts of the second reference example.

[0033] Figure 6 It is a longitudinal sectional view of the main parts of the third reference example. DETAILED DESCRIPTION

[0034] Next, a wafer stage 10 as a preferred embodiment of the present invention will be described below. Figure 1 is a longitudinal sectional view of a main part of the wafer stage 10, Figure 2 is a partial top view of the grid electrode 14 .

[0035] The wafer stage 10 is a device used to place a wafer for etching, CVD or other processing, and is provided in a vacuum chamber (not shown). The wafer stage 10 includes a ceramic member 12, a mesh electrode 14, a sintered conductor 15, a connecting member 16, an external current supply member 18, and a guide member 22.

[0036] The ceramic member 12 is formed in a disk shape, and one side of the surface is a wafer mounting surface 12a for mounting a wafer. Figure 1In the figure, the wafer loading surface 12a faces downward, but in fact, when the wafer loading table 10 is used, the wafer loading surface 12a faces upward. As the material of the ceramic component 12, for example, aluminum nitride, aluminum oxide, silicon carbide, silicon nitride, etc. are preferred. In addition, a bottomed cylindrical hole 12c is formed on the surface 12b of the ceramic component 12 on the side opposite to the wafer loading surface 12a. The ceramic component 12 can also be, for example, 150 to 500 mm in diameter and 0.5 to 30 mm in thickness. The hole 12c can also be, for example, 5 to 15 mm in diameter and 5 to 25 mm in depth.

[0037] The grid electrode 14 is an RF electrode (electrode to which a high frequency voltage is applied) embedded in the ceramic member 12 and is a circular metal mesh provided along the wafer mounting surface 12a. The material of the grid electrode 14 is preferably tungsten, molybdenum, niobium, tantalum, platinum, alloys thereof, compounds thereof, and the like. Figure 2 The mesh opening A (the length of one side of the square mesh opening 14a), the mesh (the number of meshes between the vertical and horizontal lines of 1 inch) M, the wire diameter d, and the mesh opening ratio ε of the grid electrode 14 shown are not particularly limited, but the mesh opening A is preferably greater than 0.3 mm and less than 1 mm, the mesh M is preferably greater than 10 and less than 100, the wire diameter d is preferably greater than 0.1 mm and less than 1 mm, and the mesh opening ratio ε is preferably greater than 40% and less than 60%.

[0038] The sintered conductor 15 is a sintered body containing a mixture of conductive powder P and ceramic raw material (particles or powder), and is filled in the mesh opening 14a located in the area of ​​the mesh electrode 14 facing the connecting member 16. The sintered conductor 15 contacts the side surface of the wire constituting the mesh electrode 14 and contacts the horizontal surface 16b of the connecting member 16. The material of the conductive powder P contained in the sintered conductor 15 preferably has a thermal expansion coefficient close to that of the mesh electrode 14, and more preferably has a material that is the same as that of the mesh electrode 14. In addition, the thermal expansion coefficients of the mesh electrode 14 and the conductive powder P are preferably close to the thermal expansion coefficient of the ceramic member 12. For example, when the material of the ceramic member 12 is aluminum nitride, the material of the mesh electrode 14 and the conductive powder P is preferably a molybdenum compound such as molybdenum, tungsten, or molybdenum carbide, or a tungsten compound such as tungsten carbide. When the material of the ceramic member 12 is aluminum oxide, the material of the mesh electrode 14 and the conductive powder P is preferably niobium or a niobium compound such as niobium carbide.

[0039] The connecting member 16 is a cylindrical metal member buried in a manner that reaches the mesh electrode 14 from the bottom surface of the hole 12c in the ceramic member 12. The connecting member 16 may be a bulk metal or a member formed by sintering metal powder. The material of the connecting member 16 is preferably a material having a thermal expansion coefficient close to that of the ceramic member 12, or a material having a thermal expansion coefficient close to that of the mesh electrode 14 and the conductive powder P. The material of the connecting member 16 is preferably the same as that of the mesh electrode 14 and the conductive powder P. The exposed surface 16a of the connecting member 16 that is exposed to the bottom surface of the hole 12c is flush with the bottom surface of the hole 12c. The diameter of the connecting member 16 is preferably 2 to 5 mm, and the height is preferably 1 to 5 mm.

[0040] The external current-carrying component 18 includes: a first portion 18a, which is bonded to the connection component 16 via a conductive bonding layer 20; and a second portion 18b, which is bonded to the surface of the first portion 18a on the opposite side of the bonding surface with the connection component 16 via a conductive intermediate bonding portion 18c. Considering the use in a plasma atmosphere or a corrosive gas atmosphere, the second portion 18b is made of a metal with high oxidation resistance. However, a metal with high oxidation resistance generally has a large thermal expansion coefficient, so if it is directly bonded to the connection component 16, the bonding strength is reduced due to the difference in thermal expansion between the two. Therefore, the second portion 18b is bonded to the ceramic component 12 via the first portion 18a composed of a metal having a thermal expansion coefficient close to the thermal expansion coefficient of the connection component 16. Such a metal has insufficient oxidation resistance in most cases. Therefore, the first portion 18a is surrounded by a guide component 22 composed of a metal with high oxidation resistance so as not to be in direct contact with the plasma atmosphere or the corrosive gas atmosphere. As the material of the second part 18b, pure nickel, nickel-based heat-resistant alloy, gold, platinum, silver and their alloys are preferred. As the material of the first part 18a, molybdenum, tungsten, molybdenum-tungsten alloy, tungsten-copper-nickel alloy, Kovar iron nickel cobalt alloy and the like are preferred. The bonding layer 20 is bonded by solder. As the solder, metal solder is preferred, for example, Au-Ni solder, Al solder, Ag solder and the like are preferred. The bonding layer 20 bonds the bottom surface of the hole 12c including the exposed surface 16a of the connecting part 16 with the end surface of the first part 18a. The intermediate bonding part 18c of the external current-carrying part 18 bonds the first part 18a with the second part 18b, and fills the gap between the inner peripheral surface of the guide part 22 and the entire outer peripheral surface of the first part 18a or a part thereof, and the gap between the inner peripheral surface of the guide part 22 and a part of the outer peripheral surface of the second part 18b. Therefore, the first part 18a is blocked from contact with the surrounding atmosphere by the intermediate bonding part 18c. In addition, the intermediate joint portion 18c can also be made of the same material as the joint layer 20. The first portion 18a can also have a diameter of 3 to 6 mm and a height of 2 to 5 mm, and the second portion 18b can also have a diameter of 3 to 6 mm and an arbitrary height.

[0041] The guide member 22 is a cylindrical member surrounding at least the first portion 18a of the external current-carrying member 18, and is formed of a material having higher oxidation resistance than that of the first portion 18a. The inner diameter of the guide member 22 is larger than the outer diameters of the first portion 18a and the second portion 18b, the outer diameter (excluding the flange) is smaller than the diameter of the hole 12c, and the height is higher than the height of the first portion 18a. The end surface of the guide member 22 facing the bottom surface of the hole 12c is bonded to the connecting member 16, the external current-carrying member 18, and the ceramic member 12 via the bonding layer 20. The material of the guide member 22 can use the material exemplified as the material of the second portion 18b of the external current-carrying member 18.

[0042] Next, an example of using the wafer stage 10 is described. In a chamber (not shown), the wafer stage 10 is arranged with the wafer mounting surface 12a facing upward, and a wafer is mounted on the wafer mounting surface 12a. An AC high-frequency voltage of an RF power source (not shown) is applied to the grid electrode 14 via the external power supply member 18, the bonding layer 20, and the connecting member 16, so that plasma is generated between parallel plate electrodes composed of the opposed horizontal electrodes (not shown) disposed above the chamber and the grid electrode 14 embedded in the wafer stage 10, and the plasma is used to perform CVD film formation or etching on the wafer.

[0043] Next, based on Figure 3 First, a grid electrode 14 is arranged on the upper surface of a base 112, which is a ceramic formed body formed by pressing a ceramic raw material (granules or powder) into a circular plate, and a conductive powder P (see FIG. 1 ) is placed in a grid opening 14a located in a predetermined area 14p of the grid electrode 14. Figure 3 (a)). The predetermined area 14p is an area where the connecting member 16 is to be arranged. In addition, the lower surface of the base 112 becomes the top surface of the wafer mounting table 10 after processing, and finally becomes the wafer mounting surface 12a side. Next, a cylindrical connecting member 16 is arranged on the predetermined area 14p of the grid electrode 14 (refer to Figure 3 (b)). Thus, the connection member 16 is in contact with the grid electrode 14 and the conductive powder P. Next, ceramic raw materials (granules or powders) are stacked on the substrate 112 in a manner covering the grid electrode 14 and the connection member 16 and are press-formed to form a stacked body 114 (see Figure 3 (c)). The laminate 114 includes a substrate 112 and a ceramic formed body 113 laminated thereon. Next, the laminate 114 is hot-pressed to integrate the substrate 112 and the ceramic formed body 113, thereby forming a ceramic component 12 (see Figure 3(d)). Thus, the conductive powder P placed in the mesh opening 14a located in the predetermined area 14p is sintered in a state mixed with the ceramic raw material to form a sintered conductor 15. Next, a hole 12c is opened in a manner such that the surface 12b on the side opposite to the wafer mounting surface 12a in the ceramic component 12 reaches the connecting component 16, and a component of the external conducting component 18 is inserted into the hole 12c, and the external conducting component 18 is joined to the exposed surface 16a of the connecting component 16, thereby obtaining the wafer mounting table 10 (see Figure 3 (e)). When the hole 12c is opened, the bottom surface of the hole 12c is processed in such a way that it is flush with the exposed surface 16a of the connecting member 16. When the components of the external current-carrying member 18 are joined to the exposed surface 16a of the connecting member 16, a solder forming a joining layer 20 is applied to the bottom surface of the hole 12c, and the first portion 18a of the external current-carrying member 18, the solder forming the intermediate joining portion 18c, and the second portion 18b of the external current-carrying member 18 are sequentially deposited thereon, and a guide member 22 is arranged around them, and then the solder is heated under non-oxidizing conditions to melt it, and then solidified, thereby obtaining Figure 1 The wafer stage 10 shown in FIG. 1 is a non-oxidizing condition. The non-oxidizing condition refers to a vacuum or a non-oxidizing atmosphere (for example, an inert atmosphere such as an argon atmosphere or a nitrogen atmosphere). The wafer stage 10 can be manufactured relatively easily according to the above manufacturing method.

[0044] In the wafer stage 10 of the present embodiment described above, the mesh opening 14a located in the area of ​​the mesh electrode 14 facing the connection member 16 is filled with the sintered conductor 15. The connection member 16 is in contact with the mesh electrode 14 through the sintered conductor 15 in addition to the line contact constituting the mesh electrode 14. Therefore, the actual contact area between the connection member 16 and the mesh electrode 14 is larger than that in the case where the sintered conductor 15 is not provided. As a result, the resistance value between the connection member 16 and the mesh electrode 14 is lower than that in the case where the sintered conductor 15 is not provided, and the heat generation of the connection member 16 when the current is passed from the external current supply member 18 to the mesh electrode 14 through the connection member 16 can be suppressed. Therefore, the connection member 16 is less likely to become a hot spot, and the thermal uniformity of the wafer is improved.

[0045] In particular, when a high-frequency voltage is applied to the mesh electrode 14, the connection member 16 itself is easily heated by the high-frequency current flowing from the external energizing member 18 to the mesh electrode 14 via the connection member 16. However, since the resistance value between the connection member 16 and the mesh electrode 14 is reduced as described above, the heating of the connection member 16 itself can be suppressed.

[0046] Furthermore, it is preferred that the mesh opening 14 a has a square shape with a side length of 0.3 mm to 1 mm, and the particle diameter of the conductive powder P is 1 μm to 10 μm.

[0047] The conductive powder P is preferably made of the same material as the mesh electrode 14. In this way, the thermal expansion coefficients of the sintered conductor 15 and the mesh electrode 14 match each other, thereby preventing the ceramic member 12 from cracking due to thermal stress.

[0048] The inventors have also studied the following structures, instead of filling the mesh opening 14a of the predetermined area 14p with the conductive powder P to form the sintered conductor 15: a structure in which a metal foil 30 is arranged on the predetermined area 14p of the mesh electrode 14 and a connecting member 16 is placed on the metal foil 30 (first reference example, see Figure 4 ); a structure in which a metal foil 32 is embedded in a grid opening portion located in a predetermined region 14p of the grid electrode 14 (a second reference example, referring to Figure 5 ); a structure in which a convex portion 16p protruding from the lower surface of the connecting member 16 is inserted into the grid opening portion 14p of the predetermined area of ​​the grid electrode 14 (the third reference example, referring to Figure 6 ). However, in Figure 4 In the structure of , when the ceramic component 12 is made by hot pressing, cracks are generated starting from the edge of the metal foil 30. Figure 5 In the structure of , the metal foil 32 embedded in the ceramic component 12 is not in sufficient contact with the connecting component 16, and the heat generation of the connecting component 16 cannot be suppressed. Figure 6 In the structure, when the ceramic component 12 is made by hot pressing, cracks are generated starting from the tip of the protrusion 16p inserted into the mesh opening. The sintered conductor 15 of the above-mentioned embodiment is a mixture of conductive powder and ceramic raw material (granules or powder) during hot pressing and has fluidity, which is different from the metal foil 32, so it is considered that the generation of cracks is suppressed.

[0049] In addition, the present invention is not limited to any of the above-mentioned embodiments, and it is needless to say that the present invention can be implemented in various forms within the technical scope of the present invention.

[0050] For example, in the above-mentioned embodiment, the grid electrode 14 as the RF electrode is buried in the ceramic component 12, but instead, an electrostatic electrode for adsorbing the chip to the chip mounting surface 12a may be buried, and a heating electrode (resistance heating element) for heating the chip may also be buried.

[0051] In the above-mentioned embodiment, the grid electrode 14 is used as an RF electrode, but the grid electrode 14 may be used as an electrostatic electrode or a heating electrode (resistance heating element).

[0052] In the above-described embodiment, the wafer placement surface 12 a may be a flat surface, but may be a surface on which a plurality of protrusions are formed by embossing or the like.

[0053] In the above-mentioned embodiment, a cylindrical shaft made of the same material as the ceramic component 12 can also be integrated with the ceramic component 12 on the surface 12b of the wafer mounting table 10 on the opposite side to the wafer mounting surface 12a. In this case, an external current-carrying component 18 or the like is arranged in the hollow interior of the shaft. And, after the shaft and the ceramic component 12 are integrated, the external current-carrying component 18 is installed. When manufacturing the shaft, for example, a metal mold is used and a ceramic raw material (granules or powder) is formed by CIP, and it is fired at a predetermined temperature in a normal pressure furnace, and after firing, it is processed into a predetermined size. And, when the shaft and the ceramic component 12 are integrated, for example, the end face of the shaft is butted against the surface 12b of the ceramic component 12, and the temperature is raised to a predetermined temperature to join the two, and the integration is performed.

[0054] In the above-described embodiment, in the method of manufacturing the wafer stage 10, a ceramic compact is used as the base 112, but a ceramic sintered body may be used as the base 112, or a ceramic calcined body may be used.

[0055] In the above-mentioned embodiment, it is shown Figure 3 The present invention is an example of a manufacturing process, but is not particularly limited thereto. For example, a grid electrode 14 may be arranged on the upper surface of a ceramic green sheet, a conductive powder P may be placed in the grid opening 14a, a connecting member 16 may be arranged thereon, and other ceramic green sheets may be placed and compressed to form a laminate, and the laminate may be fired at normal pressure. In this case, during compression, the conductive powder P is mixed with the ceramic raw material (granules or powder) in the ceramic green sheet in the grid opening 14a, and becomes a sintered conductor by subsequent normal pressure firing.

[0056] This application claims priority based on Japanese Patent Application No. 2019-122749 filed on July 1, 2019, the entire contents of which are incorporated herein by reference.

Claims

1. A wafer stage, comprising: A ceramic component having a wafer mounting surface; A grid electrode embedded in the ceramic component; a conductive connection member that contacts the grid electrode and is exposed to the outside from a surface of the ceramic member that is opposite to the wafer placement surface; and an external current-carrying member connected to the surface of the connecting member exposed to the outside, The wafer stage is characterized in that: A mesh opening located in a region of the mesh electrode facing the connection member is filled with a sintered conductor including a mixture of conductive powder and ceramic raw material from one surface to the other surface of the mesh electrode.

2. The wafer stage according to claim 1, wherein: The grid electrode is an RF electrode to which a high-frequency voltage is applied.

3. The wafer stage according to claim 1 or 2, characterized in that: The mesh openings are in a square shape with a side length of 0.3 mm to 1 mm, and the conductive powder has a particle size of 1 μm to 10 μm.

4. The wafer stage according to claim 1 or 2, characterized in that: The conductive powder is made of the same material as the mesh electrode.

5. A method for manufacturing a wafer mounting table, characterized in that: Including the following processes: (a) a grid electrode is arranged on a substrate which is a ceramic formed body or a ceramic sintered body, and a conductive powder is placed in a grid opening located in a predetermined area of ​​the grid electrode, wherein the grid opening is a square with a side length of 0.3 mm to 1 mm, and the particle size of the conductive powder is 1 μm to 10 μm; (b) disposing a conductive connecting member on the predetermined area of ​​the grid electrode; (c) laminating a ceramic raw material on the substrate so as to cover the grid electrode and the connection member to form a laminate; (d) hot pressing and firing the laminate to integrate the substrate and the ceramic raw material to form a ceramic component; and (e) A hole is formed in the ceramic component so as to reach the connection component from the surface opposite to the wafer mounting surface, an external current-carrying component is inserted into the hole, and the external current-carrying component is bonded to the exposed surface of the connection component.

Citation Information

Cited By

  • Heater terminal for semiconductor manufacturing equipment

    TWI926713B