Thermally conductive sheet
By placing poured anisotropic filler on the surface of the heat conductivity sheet and combining the magnetic field orientation method and vibration treatment, the limit problem of thermal conductivity improvement in the prior art is solved, and efficient thermal conductivity and adhesion are achieved.
Patent Information
- Application Number
- CN201980041501.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-06-18
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2039-06-18
AI Technical Summary
The existing heat conductivity sheet has limits when improving the thermal conductivity in the thickness direction, and the filling material is difficult to oriented in the thickness direction, affecting the heat conductivity.
By placing anisotropic filler material poured at a ratio of 1 to 45% on the surface of the heat conducting sheet, the configuration of the filler material is observed and adjusted by an optical microscope so that it does not appear on the surface, and combined with magnetic field orientation method and vibration treatment , ensure that the fill material is oriented in the thickness direction.
The thermal conductivity of the thickness direction of the heat conductivity sheet is significantly improved, and more efficient thermal conductivity is achieved, while maintaining good adhesion and physical properties balance.
Smart Images

Figure CN112313795B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a thermally conductive sheet, and more particularly to a thermally conductive sheet to be used by being arranged between a heat generating body and a heat radiating body, for example. Background Art
[0002] In electronic devices such as computers, automobile parts, and mobile phones, heat sinks and other heat sinks are generally used to dissipate heat generated by heat generating elements such as semiconductor components and mechanical parts. It is known that a heat conductive sheet is arranged between the heat generating element and the heat dissipating element in order to improve the efficiency of heat transfer to the heat dissipating element.
[0003] Thermally conductive sheets are generally compressed when placed inside electronic devices, and require high flexibility. Therefore, they are formed by mixing a thermally conductive filler with a highly flexible polymer matrix such as rubber or gel. In addition, as for thermally conductive sheets, it is well known that anisotropic fillers such as carbon fibers are oriented in the thickness direction in order to improve thermal conductivity in the thickness direction (see, for example, Patent Documents 1 and 2). In addition, a method of manufacturing a thermally conductive sheet by sandwiching two polyethylene terephthalate (PET) films is also disclosed (see, for example, Patent Document 3).
[0004] Prior Art Literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2018-056315
[0007] Patent Document 2: Japanese Patent Application Publication No. 2018-014534
[0008] Patent Document 3: Japanese Patent Application Publication No. 2011-231242 Summary of the invention
[0009] In recent years, with the high functionality of electrical equipment, the demand for high-performance thermal conductive sheets has increased, and it is hoped that the thermal conductivity in the thickness direction will be further improved. However, as disclosed in Patent Documents 1 and 2, there is a limit to improving the thermal conductivity if the filler is simply oriented in the thickness direction, and further improvement is desired. In addition, it is found that if the manufacturing method is as in Patent Document 3, it is difficult to orient the filler on the surface of the thermal conductive sheet in the thickness direction.
[0010] The present invention has been made in view of the above problems, and an object of the present invention is to provide a thermally conductive sheet capable of sufficiently improving thermal conductivity in the thickness direction.
[0011] As a result of intensive research, the inventors found that the above-mentioned problems can be solved by arranging the anisotropic filler on the sheet surface observed under an optical microscope so as to tilt at a predetermined ratio, thereby completing the present invention. The present invention provides the following technical solutions [1] to
[14] .
[0012] [1] A thermally conductive sheet comprising a polymer matrix and an anisotropic filler, wherein the anisotropic filler is oriented in a thickness direction.
[0013] The anisotropic filler is disposed so as to pour at a ratio of 1 to 45% on the surface of the thermally conductive sheet observed with an optical microscope.
[0014] [2] The thermally conductive sheet according to [1] above,
[0015] The anisotropic filler is not exposed on the surface of the thermally conductive sheet.
[0016] [3] The thermally conductive sheet according to [1] or [2] above,
[0017] The anisotropic filling material is a fiber material.
[0018] [4] The thermally conductive sheet according to [3] above,
[0019] The fiber material is carbon fiber.
[0020] [5] The thermally conductive sheet according to [3] or [4] above,
[0021] The average fiber length of the fiber material is 50 to 500 μm.
[0022] [6] The thermally conductive sheet according to any one of [1] to [5] above,
[0023] Non-anisotropic fill materials are also included.
[0024] [7] The thermally conductive sheet according to [6] above,
[0025] The non-anisotropic filler is at least one selected from the group consisting of aluminum oxide, aluminum, zinc oxide, boron nitride, and aluminum nitride.
[0026] [8] The thermally conductive sheet according to [6] or [7] above,
[0027] The ratio of the volume filling rate of the non-anisotropic filling material to the volume filling rate of the anisotropic filling material is 2-5.
[0028] [9] The thermally conductive sheet according to any one of [1] to [8] above,
[0029] At least a portion of the anisotropic filling material arranged in a poured manner in the surface is arranged to be inclined with respect to the surface.
[0030]
[10] The thermally conductive sheet according to any one of [1] to [9] above,
[0031] The polymer matrix is addition reaction curing type polysiloxane.
[0032]
[11] The thermally conductive sheet according to any one of [1] to
[10] above,
[0033] The thermally conductive sheet has a thickness of 0.1 to 5 mm.
[0034]
[12] The thermally conductive sheet according to any one of [1] to
[11] above,
[0035] The thermal conductivity of the thermally conductive sheet in the thickness direction is 6 w / m·K or more.
[0036]
[13] The thermally conductive sheet according to [4] above,
[0037] The carbon fibers are covered with an insulating layer.
[0038]
[14] The thermally conductive sheet according to
[13] above, wherein the insulating layer contains silicon dioxide.
[0039] According to the present invention, it is possible to provide a thermally conductive sheet capable of sufficiently improving thermal conductivity in the thickness direction. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is a schematic cross-sectional view showing the thermally conductive sheet according to the first embodiment.
[0041] Figure 2 This is a schematic cross-sectional view showing a thermally conductive sheet according to a second embodiment.
[0042] Figure 3 This is a schematic diagram of a thermal resistance measuring machine.
[0043] Figure 4 This is a diagram schematically showing an observation image obtained by observing the surface of the thermally conductive sheet of Example 1 using an optical microscope. DETAILED DESCRIPTION
[0044] Hereinafter, a thermally conductive sheet according to an embodiment of the present invention will be described in detail.
[0045] [First embodiment]
[0046] Figure 1 A thermally conductive sheet according to a first embodiment is shown. Figure 1 , an example in which the anisotropic filler is a fiber material is representatively shown. The thermally conductive sheet 10 according to the first embodiment includes a polymer matrix 12 and an anisotropic filler 13, and the anisotropic filler 13 is oriented in the thickness direction. Near the surface of each surface 10A, 10B of the thermally conductive sheet 10, a part of the anisotropic filler 13 is arranged in an inclined manner. In addition, the so-called near the surface means the surface observed by an optical microscope described later.
[0047] In the thermally conductive sheet 10 of the present embodiment, as shown in the manufacturing method described later, it is difficult to arrange the anisotropic filler 13 on the surfaces 10A and 10B. Therefore, the anisotropic filler 13 does not exist on the surfaces 10A and 10B, and even if it exists, its amount is small, for example, it is sufficiently small compared with the existence ratio of the anisotropic filler 13 at the center position in the thickness direction. As a result, the anisotropic filler 13 is buried in the sheet on the surfaces 10A and 10B, and is not exposed on the surfaces 10A and 10B of the thermally conductive sheet 10. It should be noted that the term "not exposed" means that the anisotropic filler existing on the surface of the thermally conductive sheet is substantially covered by the polymer matrix 12. In addition, the term "covering" here does not necessarily mean that the anisotropic filler 13 must be 100% covered by the polymer matrix 12.
[0048] The anisotropic filler 13 near the surface of each surface 10A, 10B is arranged to tilt at a ratio of 1 to 45%. In the thermally conductive sheet 10 of the present embodiment, the ratio of the anisotropic filler 13 arranged in a tilted manner is 1% or more. This is because it is difficult to adjust the ratio of the anisotropic filler 13 arranged in a tilted manner to less than 1% in practical terms. That is, the ratio of the anisotropic filler 13 arranged in a tilted manner of 1% can be considered to be the minimum value of the ratio of the anisotropic filler 13 arranged in a tilted manner in terms of the relationship with the increase limit of the anisotropic filler 13 oriented in the thickness direction near the surface.
[0049] If the ratio of the anisotropic filler 13 disposed in a tilted manner exceeds 45%, the amount of the anisotropic filler 13 oriented in the thickness direction near the surface decreases, making it difficult to increase the thermal conductivity in the thickness direction.
[0050] The anisotropic filler 13 near the surfaces 10A and 10B is not exposed on the surface and is arranged near the surface to be tilted at a ratio of 1 to 45%, thereby providing the thermally conductive sheet 10 having excellent thermal conductivity and adhesiveness.
[0051] From the viewpoint of improving the thermal conductivity in the thickness direction, the ratio of the tilted arrangement is preferably 1 to 25%, more preferably 1 to 10%, and even more preferably 1 to 5%.
[0052] The ratio of the anisotropic filler arranged in a tilted manner near the surface can be calculated by finding the ratio of the number of anisotropic fillers arranged in a tilted manner to the total number of anisotropic fillers observed in the observation image observed by the optical microscope. By observing the surface of the thermally conductive sheet 10 under the conditions described below using an optical microscope, the anisotropic filler that is not exposed on the surface of the thermally conductive sheet 10 and exists near the surface can be observed.
[0053] Here, the so-called anisotropic filler 13 arranged in a tilted manner refers to a filler that tilts in the observation image to the extent that the portion other than the end face 13A of the anisotropic filler 13 can be substantially observed in the observation image. The so-called substantially observable degree means that the portion other than the end face 13A can be observed with an area (projected area) that is more than twice that of the end face 13A. Therefore, in the case where the anisotropic filler 13 is a fiber material, the fiber material whose outer peripheral surface 13B of the fiber material reaches more than twice the end face 13A of the fiber material in the observation image is regarded as the anisotropic filler arranged in a tilted manner.
[0054] Regarding the image analysis method, it can be observed visually from the observed image. In addition, as long as the ratio of the number of anisotropic fillers arranged in a tilted manner can be calculated based on the above-mentioned benchmark, the analysis method is not limited, and it can also be calculated using image processing software. For example, visualization can be achieved by processing using general image processing software (such as "WINROOF" manufactured by Mitani Shoji Co., Ltd.).
[0055] The observation of the sheet surface with an optical microscope was performed at a magnification of 200 times using a digital microscope VHX1000 (manufactured by Keyence Corporation) in an environment where the illuminance measured with an illuminometer based on JIS Z9110 was 2000 lux.
[0056] The anisotropic filler 13 disposed in a tilted manner near the surfaces 10A and 10B of the thermally conductive sheet may be disposed in a lying manner on the surfaces 10A and 10B of the thermally conductive sheet, or may be disposed in a tilted manner relative to the surfaces 10A and 10B. In addition, the tilt angle of the anisotropic filler 13 disposed in a tilted manner relative to the thickness direction is preferably about 45 to 90°. In addition, regarding the tilt angle, when the angle of the configuration is greater than 90°, the supplementary angle is used as the tilt angle.
[0057] The anisotropic filler 13 disposed in a lying manner near the surface of the thermally conductive sheet is substantially an anisotropic filler disposed along the surface 10A (or 10B). Figure 1 In the figure, anisotropic filling material 13X is used.
[0058] The anisotropic filler inclined relative to the surface is an anisotropic filler inclined in such a manner that one end face 13A of the anisotropic filler 13 is separated from the surface 10A (or 10B). Figure 1 In the figure, anisotropic filling material 13Y is used.
[0059] The anisotropic filler 13 tilted near each surface 10A, 10B preferably includes an anisotropic filler 13Y tilted relative to the surface. The anisotropic filler 13Y tilted easily contacts the anisotropic filler 13 oriented in the thickness direction, and easily improves the thermal conductivity in the thickness direction.
[0060] In the present embodiment, the thermally conductive sheet 10 further includes a non-anisotropic filler 14. When the thermally conductive sheet 10 includes the non-anisotropic filler 14, the thermal conductivity is further improved.
[0061] <Polymer matrix>
[0062] The polymer matrix 12 used in the thermally conductive sheet 10 is a polymer compound such as an elastomer or rubber, and is preferably formed by curing a liquid polymer composition (curable polymer composition) composed of a mixed system such as a main agent and a curing agent. The curable polymer composition may be, for example, a composition composed of an uncrosslinked rubber and a crosslinking agent, or a composition containing a monomer, a prepolymer, etc. and a curing agent. In addition, the curing reaction may be room temperature curing or thermal curing.
[0063] The polymer matrix formed by the curable polymer composition can be exemplified by polysiloxane rubber. In the case of polysiloxane rubber, as the polymer matrix (curable polymer composition), it is preferred to use an addition reaction curing type polysiloxane. In addition, more specifically, as the curable polymer composition, a curable polymer composition comprising an alkenyl-containing organopolysiloxane and a hydrogen-containing organopolysiloxane can be used.
[0064] As rubber, in addition to the above, various synthetic rubbers can also be used, and specific examples include acrylic rubber, nitrile rubber, isoprene rubber, polyurethane rubber, ethylene-propylene rubber, styrene-butadiene rubber, butadiene rubber, fluororubber, butyl rubber, etc. When these rubbers are used, the synthetic rubber may be cross-linked in the thermally conductive sheet or may be in an uncross-linked (i.e., uncured) state.
[0065] When crosslinked (ie, cured), as described above, the polymer matrix may be a matrix obtained by curing a curable polymer composition composed of an uncrosslinked rubber made of these synthetic rubbers and a crosslinking agent.
[0066] In addition, as the elastomer, thermoplastic elastomers such as polyester thermoplastic elastomers and polyurethane thermoplastic elastomers, and thermosetting elastomers formed by curing a mixed liquid polymer composition composed of a main agent and a curing agent can also be used. For example, a polyurethane elastomer formed by curing a polymer composition containing a polymer having a hydroxyl group and an isocyanate can be exemplified.
[0067] Among the above, silicone rubber, particularly addition reaction curing type silicone, is preferably used, for example, because the polymer matrix after curing is particularly soft and the filling property of the thermal conductive filler is good.
[0068] In addition, the polymer composition used to form the polymer matrix may be a composition consisting of a single polymer compound component, or may be a composition consisting of a polymer compound and a plasticizer. When synthetic rubber is used, a plasticizer is preferably used, and by including a plasticizer, the flexibility of the polymer matrix when not cross-linked can be improved.
[0069] Plasticizers can use plasticizers compatible with polymer compounds, specifically, preferably ester plasticizers and silicone oils. Specific examples of ester plasticizers include phthalates, adipates, trimellitates, phosphates, sebacates, azelates, maleates, benzoates, etc. As silicone oils, polydimethylsiloxanes can be mentioned.
[0070] The content of the plasticizer relative to the polymer compound is calculated by mass ratio, and the plasticizer / polymer compound is preferably 20 / 80 to 60 / 40, and more preferably 30 / 70 to 55 / 45. By setting the mass ratio of the plasticizer / polymer compound to 60 / 40 or less, it is easy to hold the filler by the polymer compound. In addition, by setting it to 20 / 80 or more, the flexibility of the polymer matrix becomes sufficient.
[0071] The content of the polymer matrix, when expressed as a volume-based filling rate (volume filling rate), is preferably 20 to 50% by volume, more preferably 25 to 45% by volume, based on the total amount of the thermally conductive sheet.
[0072] (additive)
[0073] In the thermally conductive sheet 10, various additives may be further blended into the polymer matrix 12 within a range that does not impair the function of the thermally conductive sheet 10. Examples of the additives include at least one selected from the group consisting of a dispersant, a coupling agent, an adhesive, a flame retardant, an antioxidant, a colorant, an anti-settling agent, and the like. In addition, when the curable polymer composition is crosslinked or cured as described above, a crosslinking accelerator or a curing accelerator may be blended as an additive to accelerate the crosslinking or curing.
[0074] <Anisotropic filler>
[0075] The anisotropic filler 13 mixed in the polymer matrix 12 is a filler having anisotropy in shape and is an oriented filler. The anisotropic filler 13 is a thermally conductive filler. Examples of the anisotropic filler 13 include fiber materials, flaky materials, and the like. The anisotropic filler 13 is a material with a high aspect ratio, specifically, a material with an aspect ratio greater than 2, and the aspect ratio is preferably greater than 5. By making the aspect ratio greater than 2, it is easy to orient the anisotropic filler 13 in the thickness direction, and it is easy to improve the thermal conductivity of the thermally conductive sheet 10.
[0076] The upper limit of the aspect ratio is not particularly limited, but is 100 for practical purposes.
[0077] The aspect ratio is the ratio of the length in the long axis direction to the length in the short axis direction of the anisotropic filler 13, and in a fiber material it means fiber length / fiber diameter, and in a flaky material it means the length in the long axis direction / thickness of the flaky material.
[0078] From the viewpoint of improving thermal conductivity and facilitating the placement of the anisotropic filler 13 in a tilted manner on the surfaces 10A and 10B, the anisotropic filler 13 is preferably a fiber material.
[0079] The content of the anisotropic filler 13 in the thermally conductive sheet is preferably 30 to 300 parts by mass, more preferably 50 to 270 parts by mass, relative to 100 parts by mass of the polymer matrix. In addition, the content of the anisotropic filler 13, when expressed as a volume-based filling rate (volume filling rate), is preferably 5 to 35% by volume, more preferably 8 to 30% by volume, relative to the total amount of the thermally conductive sheet.
[0080] When the content of the anisotropic filler 13 is 30 parts by mass or more, thermal conductivity is easily improved, and when it is 300 parts by mass or less, the viscosity of the mixed composition described below is easily appropriate, and the orientation of the anisotropic filler 13 is improved.
[0081] When the anisotropic filler 13 is a fiber material, the average fiber length is preferably 50 to 500 μm, more preferably 70 to 350 μm. If the average fiber length is 50 μm or more, the anisotropic fillers are in proper contact with each other inside the thermal conductive sheet 10, thereby ensuring a heat transfer path. In addition, if the average fiber length of the anisotropic filler 13 is long, it is easy to be arranged in a tilted manner near the surface, but through a specific manufacturing method described later, it can be oriented in the thickness direction at a high ratio near the surface.
[0082] On the other hand, when the average fiber length is 500 μm or less, the volume of the anisotropic filler becomes low, and the polymer matrix can be filled with a high amount of the anisotropic filler.
[0083] The average fiber length can be calculated by observing the anisotropic filler under a microscope. More specifically, for example, the fiber lengths of 50 arbitrary anisotropic fillers can be measured using an electron microscope or an optical microscope, and the average value (arithmetic mean) can be taken as the average fiber length.
[0084] In addition, it is preferable that the average fiber length of the fiber material is smaller than the thickness of the thermally conductive sheet 10 . By being smaller than the thickness, the fiber material becomes less likely to protrude from the surfaces 10A and 10B of the thermally conductive sheet 10 .
[0085] In addition, when the anisotropic filler 13 is a flaky material, the average particle size is preferably 10 to 400 μm, and more preferably 15 to 200 μm. In addition, it is particularly preferably 15 to 130 μm. By setting the average particle size to be 10 μm or more, the anisotropic fillers 13 in the thermally conductive sheet 10 are easily in contact with each other, and the heat transfer path can be ensured. In addition, the anisotropic filler 13 is easily arranged in a tilted manner on the surface of the thermally conductive sheet 10, but through the specific manufacturing method described later, it can be oriented in the thickness direction at a high ratio near the surface, and the thermal conductivity of the thermally conductive sheet 10 becomes good. On the other hand, if the average particle size is set to 400 μm or less, the volume of the thermally conductive sheet 10 becomes low, and the anisotropic filler 13 can be highly filled in the polymer matrix 12.
[0086] The average particle size of the flaky material can be obtained by observing the anisotropic filler with a microscope and calculating the major axis. More specifically, for example, the major axes of 50 arbitrary anisotropic fillers can be measured using an electron microscope or an optical microscope, and the average (arithmetic mean) can be used as the average particle size.
[0087] The anisotropic filler 13 may be a known material having thermal conductivity, but preferably has diamagnetic properties so as to enable magnetic field orientation as described later.
[0088] Specific examples of the anisotropic filler 13 include: carbon-based materials represented by carbon fibers or flaky carbon powders, metal materials represented by metal fibers, metal oxides, boron nitrides, metal nitrides, metal carbides, metal hydroxides, and the like. Among them, carbon-based materials are preferred because of their low specific gravity and good dispersibility in the polymer matrix 12, and graphitized carbon materials with high thermal conductivity are more preferred. Graphitized carbon materials have diamagnetic properties because graphite planes are aligned in a specified direction. In addition, boron nitride and the like also have diamagnetic properties because crystal planes are aligned in a specified direction. In addition, the anisotropic filler 13 is particularly preferably carbon fiber.
[0089] In addition, the anisotropic filler 13 is not particularly limited, but the thermal conductivity along the direction having anisotropy (i.e., the long axis direction) is generally 60 W / m·K or more, preferably 400 W / m·K or more. The upper limit of the thermal conductivity of the anisotropic filler 13 is not particularly limited, but is, for example, 2000 W / m·K or less. The thermal conductivity is measured by the laser flash method.
[0090] The anisotropic filler 13 may be used alone or in combination of two or more. For example, as the anisotropic filler 13, an anisotropic filler 13 having at least two different average particle sizes or average fiber lengths may be used. It is believed that if anisotropic fillers of different sizes are used, the relatively small anisotropic filler enters between the relatively large anisotropic filler, and the anisotropic filler can be densely filled into the polymer matrix, and the heat conduction efficiency can be improved.
[0091] The carbon fibers used as the anisotropic filler 13 are preferably graphitized carbon fibers. In addition, the flaky carbon powder is preferably flaky graphite powder. Among them, the anisotropic filler 13 is more preferably graphitized carbon fibers.
[0092] In the case of graphitized carbon fibers, the crystal planes of graphite are continuous in the fiber axial direction, and have high thermal conductivity in the fiber axial direction. Therefore, by aligning the fiber axial direction with a specified direction, the thermal conductivity in a specific direction can be improved. In addition, in the case of flaky graphite powder, the crystal planes of graphite are continuous in the in-plane direction of the flaky surface, and have high thermal conductivity in the in-plane direction. Therefore, by aligning the flaky surface in a specified direction, the thermal conductivity in a specific direction can be improved. Graphitized carbon fibers and flaky graphite powders preferably have a high degree of graphitization.
[0093] As the graphitized carbon materials such as the above-mentioned graphitized carbon fibers and flaky graphite powder, graphitized carbon materials obtained by graphitizing the following raw materials can be used. For example, condensed polycyclic hydrocarbon compounds such as naphthalene, PAN (polyacrylonitrile), condensed heterocyclic compounds such as asphalt, etc. can be listed, but graphitized mesophase asphalt, polyimide, and polybenzazole with high graphitization degree are particularly preferably used. For example, by using mesophase asphalt, the asphalt is oriented along the fiber axis using its anisotropy in the spinning process described later, and a graphitized carbon fiber having excellent thermal conductivity in the fiber axis can be obtained.
[0094] The use of mesophase pitch in graphitized carbon fiber is not particularly limited as long as it can be spun, and the mesophase pitch can be used alone or in combination with other raw materials. However, from the perspective of high thermal conductivity, spinnability and quality stability, it is most preferred to use mesophase pitch alone, that is, graphitized carbon fiber with a mesophase pitch content of 100%.
[0095] The graphitized carbon fibers can be: graphitized carbon fibers that are graphitized after being subjected to the treatments of spinning, infusibility, and carbonization in sequence and then pulverized or cut into a predetermined particle size, and graphitized carbon fibers that are graphitized after being pulverized or cut after carbonization. In the case of pulverization or cutting before graphitization, polycondensation reaction and cyclization reaction become easy to proceed in the surface newly exposed on the surface due to pulverization during graphitization treatment, so that graphitized carbon fibers that have increased graphitization degree and further improved thermal conductivity can be obtained. On the other hand, in the case of graphitizing the spun carbon fibers and then pulverizing them, the graphitized carbon fibers are rigid and easy to pulverize, and carbon fiber powder with a narrow fiber length distribution can be obtained by pulverizing them in a short time.
[0096] The average fiber length of the graphitized carbon fiber is preferably 50 to 500 μm, more preferably 70 to 350 μm, as described above. In addition, as described above, the aspect ratio of the graphitized carbon fiber is greater than 2, preferably greater than 5. The thermal conductivity of the graphitized carbon fiber is not particularly limited, but the thermal conductivity in the fiber axial direction is preferably 400 W / m·K or more, more preferably 800 W / m·K or more.
[0097] The carbon fibers used as the anisotropic filler 13 are preferably covered with an insulating layer.
[0098] By using carbon fibers covered with an insulating layer, the electrical insulation of the thermally conductive sheet is improved. The thickness of the insulating layer is not particularly limited, but is preferably 100 to 400 nm, more preferably 100 to 200 nm. The insulating layer contains silicon dioxide as a substance that exerts electrical insulation. The insulating layer may be an insulating layer composed only of silicon dioxide, but may also contain aluminum oxide, boron nitride, silicon nitride, etc. in addition to silicon dioxide.
[0099] The anisotropic filler 13 is a material oriented in the thickness direction as described above, but it is not necessary for the major axis direction to be strictly parallel to the thickness direction, and even if the major axis direction is slightly inclined relative to the thickness direction, it is considered to be oriented in the thickness direction. Specifically, an anisotropic filler whose major axis direction is inclined less than 20° relative to the thickness direction is also considered to be an anisotropic filler 13 oriented in the thickness direction, and if such anisotropic filler 13 is a majority in the thermal conductive sheet 10 (for example, more than 60%, preferably more than 80% relative to the total amount of anisotropic filler), it is considered to be oriented in the thickness direction.
[0100] <Non-anisotropic filler>
[0101] The non-anisotropic filler 14 is a thermally conductive filler contained in the thermally conductive sheet 10 separately from the anisotropic filler 13, and is a material that imparts thermal conductivity to the thermally conductive sheet 10 together with the anisotropic filler 13. In the present embodiment, by filling the non-anisotropic filler 14, the viscosity increase is suppressed in the stage before the sheet is solidified, and the dispersibility becomes good. In addition, when the anisotropic filler 13 is increased, for example, it is difficult to increase the contact area between the fillers, but by filling the non-anisotropic filler 14 between them, a heat transfer path can be formed, and a thermally conductive sheet 10 with high thermal conductivity can be obtained.
[0102] The non-anisotropic filler 14 is a filler having substantially no anisotropy in shape and is a filler that does not orient in a predetermined direction even under an environment where the anisotropic filler 13 is oriented in a predetermined direction, such as under the generation of magnetic lines of force or under shear force as described later.
[0103] The non-anisotropic filler 14 has an aspect ratio of 2 or less, preferably 1.5 or less. In this embodiment, by including the non-anisotropic filler 14 having such a low aspect ratio, the filler having thermal conductivity can be appropriately interposed between the gaps of the anisotropic filler 13, and a thermally conductive sheet 10 with high thermal conductivity can be obtained. In addition, by setting the aspect ratio to 2 or less, the viscosity of the mixed composition described later can be prevented from increasing, and high filling can be achieved.
[0104] Specific examples of the anisotropic filler 14 include metals, metal oxides, metal nitrides, metal hydroxides, carbon materials, oxides, nitrides, carbides of elements other than metals, etc. The anisotropic filler 14 may be in the form of spheres or irregular powders.
[0105] In the non-anisotropic filler 14, examples of metals include aluminum, copper, nickel, etc., examples of metal oxides include aluminum oxide represented by aluminum oxide (alumina), magnesium oxide, zinc oxide, etc., and examples of metal nitrides include aluminum nitride, etc. Examples of metal hydroxides include aluminum hydroxide. In addition, examples of carbon materials include spherical graphite, etc. Examples of oxides, nitrides, and carbides of elements other than metals include quartz, boron nitride, silicon carbide, etc.
[0106] The non-anisotropic filler 14 is preferably selected from alumina, aluminum, zinc oxide, boron nitride, and aluminum nitride. In particular, alumina is preferred from the viewpoint of filling properties and thermal conductivity.
[0107] The anisotropic filler 14 may be made of one of the above-mentioned materials alone or in combination of two or more.
[0108] The average particle size of the non-anisotropic filler 14 is preferably 0.1 to 50 μm, more preferably 0.5 to 35 μm. In addition, it is particularly preferably 1 to 15 μm. By setting the average particle size to be 50 μm or less, it becomes difficult to cause adverse conditions such as disturbing the orientation of the anisotropic filler 13. In addition, by setting the average particle size to be greater than 0.1 μm, the specific surface area of the non-anisotropic filler 14 will not be larger than required, and even if a large amount is added, the viscosity of the mixed composition is difficult to increase, and it is easy to highly fill the non-anisotropic filler 14.
[0109] Regarding the non-anisotropic filler 14 , for example, a non-anisotropic filler 14 having at least two kinds of average grain sizes different from each other may be used as the non-anisotropic filler 14 .
[0110] The average particle size of the anisotropic filler 14 can be measured by observation using an electron microscope, etc. More specifically, for example, the particle sizes of 50 random anisotropic fillers can be measured using an electron microscope or an optical microscope, and the average value (arithmetic mean) can be taken as the average particle size.
[0111] The content of the anisotropic filler 14 is preferably in the range of 200 to 800 parts by mass, more preferably in the range of 300 to 700 parts by mass, based on 100 parts by mass of the polymer matrix.
[0112] When the content of the anisotropic filler 14 is expressed as a filling rate based on volume (volume filling rate), it is preferably 30 to 60% by volume, and more preferably 40 to 55% by volume, based on the total volume of the thermally conductive sheet.
[0113] When the non-anisotropic filler 14 is set to 200 parts by mass or more, the amount of the non-anisotropic filler 14 interposed between the anisotropic fillers 13 becomes sufficient, and the thermal conductivity becomes good. On the other hand, when it is set to 800 parts by mass or less, the effect of improving the thermal conductivity corresponding to the content can be obtained, and the thermal conduction of the anisotropic filler 13 is not hindered by the non-anisotropic filler 14. Furthermore, when it is set to be within the range of 300 to 700 parts by mass, the thermal conductivity of the thermal conductive sheet 10 is excellent, and the viscosity of the mixed composition is more appropriate.
[0114] The ratio of the volume filling rate of the non-anisotropic filler 14 to the volume filling rate of the anisotropic filler 13 is preferably 2 to 5, and more preferably 2 to 3. By setting the range of the volume filling rate ratio to be within the above range, the non-anisotropic filler 14 can be appropriately filled between the anisotropic fillers 13, and a highly efficient heat transfer path can be formed, thereby improving the thermal conductivity of the thermally conductive sheet 10.
[0115] <Thermal conductive sheet>
[0116] The thermal conductivity of the thermally conductive sheet 10 in the thickness direction is preferably 6 W / m·K or more, more preferably 8 W / m·K or more, and further preferably 13 W / m·K or more. By setting it to be above these lower limits, the thermal conductivity of the thermally conductive sheet 10 in the thickness direction can be excellent. The upper limit is not particularly limited, and the thermal conductivity of the thermally conductive sheet 10 in the thickness direction is, for example, 50 W / m·K or less. In addition, the thermal conductivity is measured by a method based on ASTM D5470-06.
[0117] The thermal resistance value of the thermal conductive sheet 10 in the sheet thickness direction is preferably less than 3.0°C / W, more preferably less than 2.5°C / W, and further preferably less than 2.0°C / W. By setting the thermal resistance value to a certain value or less, the thermal conductive sheet 10 can easily transfer heat from the heating element to the heat sink. The smaller the thermal resistance value, the better, but it is usually 0.1°C / W or more. The thermal resistance value can be measured by the method described in the examples.
[0118] The thickness of the thermally conductive sheet may be in the range of 0.1 to 5 mm, but is not necessarily limited to this range because the thickness of the thermally conductive sheet can be appropriately changed depending on the shape and application of the electronic device on which the thermally conductive sheet is mounted.
[0119] The thermally conductive sheet 10 can be used inside electronic devices, etc. Specifically, the thermally conductive sheet 10 is interposed between a heat generating body and a heat sink, and conducts the heat generated by the heat generating body to transfer it to the heat sink, and dissipates the heat from the heat sink. Here, as the heat generating body, various electronic components such as CPU, power amplifier, and power supply used inside electronic devices can be listed. In addition, the heat sink can be a heat sink, a heat pump, and a metal housing of an electronic device. Both surfaces 10A and 10B of the thermally conductive sheet 10 are respectively in close contact with the heat generating body and the heat sink, and are compressed for use.
[0120] <Method for producing thermally conductive sheet>
[0121] The thermally conductive sheet of the present embodiment is not particularly limited, but can be produced, for example, by a method including the following steps (A) and (B).
[0122] Step (A): a step of sandwiching the mixed composition between two release materials to obtain a laminated body;
[0123] Step (B): A step of orienting the anisotropic filler in one direction which is the thickness direction in the thermally conductive sheet.
[0124] Hereinafter, each step will be described in more detail.
[0125] [Step (A)]
[0126] Process (A) is a process of obtaining a laminate by sandwiching a mixed composition with two pieces of peeling materials. The mixed composition comprises an anisotropic filler, a non-anisotropic filler and a curable polymer composition that becomes a raw material of a polymer matrix, and can be obtained by mixing the above-mentioned components. At this time, various additives such as flame retardants can also be combined as needed. When mixing, known mixing mechanisms such as mixers, mixing rolls, kneaders, extruders, etc. can be used. The mixed composition is usually in a slurry state, and an organic solvent can also be used to adjust the viscosity.
[0127] Next, the obtained mixed composition is applied to a release material. From the viewpoint of uniformly applying the mixed composition to the release material, a doctor blade method or a die coating method is preferably used. After the application, another release material is placed on the mixed composition.
[0128] Next, the mixed composition is compressed to a desired thickness while being sandwiched between two release materials using a press machine, etc., to obtain a laminate. The amount of the mixed composition applied and the compression pressure may be appropriately set in consideration of the size and thickness of the resulting thermally conductive sheet.
[0129] The release material is not particularly limited, but is preferably a release material made of a resin, and among these, a polyethylene terephthalate (PET) film is more preferred, and a PET film subjected to a release treatment with a fluororesin is further preferred.
[0130] The curable polymer composition in the mixed composition sandwiched between the two release materials tends to preferentially move toward the surface of the release materials due to the surface tension of the release materials, and conversely, the anisotropic filler becomes difficult to be arranged near the release materials. Therefore, it is believed that the obtained thermally conductive sheet is a thermally conductive sheet in which the anisotropic filler is not exposed on the surface.
[0131] In the step (A), the anisotropic filler is randomly (irregularly) dispersed in the mixed composition sandwiched between the release materials.
[0132] [Process (B)]
[0133] Step (B) is a step of orienting the anisotropic filler in the thermally conductive sheet along one direction that becomes the thickness direction. As a method for orienting it, a magnetic field orientation method is preferably applied. In the magnetic field orientation method, the laminate obtained in step (A) is placed in a magnetic field, the anisotropic filler is oriented along the magnetic field, and then the curable polymer composition is cured.
[0134] In the magnetic field orientation method, as a magnetic field line generating source for applying magnetic field lines, superconducting magnets, permanent magnets, electromagnets, etc. can be listed, but in terms of being able to generate a magnetic field with a high magnetic flux density, superconducting magnets are preferred. The magnetic flux density of the magnetic field generated from these magnetic field line generating sources is preferably 1 to 30 Tesla. If the magnetic flux density is set to 1 Tesla or more, the above-mentioned anisotropic filler material composed of carbon materials and the like can be easily oriented. In addition, by setting it to 30 Tesla or less, it can be manufactured practically.
[0135] In addition, from the viewpoint of easily applying the magnetic field orientation method to adjust the proportion of the anisotropic filler arranged in a tilted manner to the desired range, the viscosity of the mixed composition is preferably set to 450Pa·s or less, and more preferably to 300Pa·s or less. The viscosity of the mixed composition is preferably set to 10Pa·s or more. As a result, the anisotropic filler and the non-anisotropic filler become difficult to settle. Furthermore, the so-called viscosity is the viscosity measured at a rotational speed of 10rpm at 25°C using a rotational viscometer (Brucker Field Viscometer DV-E, Spindle SC4-14). However, in the case of using anisotropic fillers, non-anisotropic fillers that are difficult to settle, or in combination with additives such as anti-settling agents, the viscosity of the mixed composition can also be set to less than 10Pa·s.
[0136] By placing the laminate in a magnetic field, the anisotropic filler is oriented in the thickness direction, but near the interface between the mixed composition and the release material, that is, in the portion that eventually becomes the surface of the thermally conductive sheet, the presence of the release material makes it difficult for the anisotropic filler to be oriented in the thickness direction of the laminate, and there is a tendency for the anisotropic filler to be arranged in a tilted manner to increase. Therefore, from the perspective of making the proportion of the anisotropic filler arranged in a tilted manner within the desired range and improving the thermal conductivity of the obtained thermally conductive sheet, it is preferred to give vibration to the laminate from the outside. The vibration is given to the anisotropic filler through the curable polymer composition and the non-anisotropic filler. As a result, the anisotropic filler becomes easy to be oriented in the thickness direction, and the proportion of the anisotropic filler arranged in a tilted manner can be made within the desired range.
[0137] In the present application, by adjusting the time, frequency, acceleration, amplitude, etc. of the vibration, the intensity of the vibration can be changed, thereby adjusting the proportion of the anisotropic filling material configured in a tilted manner. If the vibration imparted is strong, the proportion of the anisotropic filling material oriented in the thickness direction increases, and the proportion of the anisotropic filling material configured in a tilted manner decreases. On the contrary, if the vibration imparted is weak, the proportion of the anisotropic filling material oriented in the thickness direction decreases, and the proportion of the anisotropic filling material configured in a tilted manner increases.
[0138] The vibration can be imparted while applying the magnetic field orientation method, or before or after the magnetic field orientation method, but from the viewpoint of making the ratio of the anisotropic filler material arranged in a tilted manner into a desired range, it is preferably imparted while applying the magnetic field orientation method. The method of imparting vibration is not particularly limited, but, for example, a vibration device that uses compressed air to impart vibration can be used.
[0139] From the viewpoint of making the proportion of the anisotropic filler configured in a tilted manner into the desired range by magnetic field orientation method and vibration, the viscosity of the mixed composition is preferably set to 450Pa·s or less, and more preferably set to 300Pa·s or less. By setting the viscosity to a certain value or less in this way, the fluidity becomes good, and it becomes easy to orient the anisotropic filler in the thickness direction by magnetic field orientation method and vibration, and there will be no undesirable situation such as excessive time consumption in orientation. The viscosity of the mixed composition is preferably set to 10Pa·s or more. As a result, anisotropic fillers and non-anisotropic fillers become difficult to settle.
[0140] However, when an anisotropic filler or a non-anisotropic filler that is difficult to settle is used, or when an additive such as an anti-settling agent is used in combination, the viscosity of the mixed composition may be less than 10 Pa·s.
[0141] The curing of the curable polymer composition can be performed by heating, for example, at a temperature of about 50 to 150° C. The heating time is, for example, about 10 minutes to 3 hours.
[0142] By curing, a thermally conductive sheet sandwiched between two release materials can be obtained.
[0143] In the above description, the anisotropic filler 13 is not exposed on both surfaces 10A and 10B of the thermally conductive sheet 10. However, in the present invention, the thermally conductive sheet 10 may have the anisotropic filler 13 exposed on one or both of the above surfaces 10A and 10B.
[0144] In order to obtain such a thermally conductive sheet, a method other than the above-mentioned production method, for example, a flow orientation method in which shear is applied to the mixed composition to orient the anisotropic filler, etc. may be applied.
[0145] However, the thermally conductive sheet 10 in which the anisotropic filler is not exposed on the surface of the thermally conductive sheet is preferred because the thermal conductivity in the thickness direction can be improved, the surface adhesiveness can be improved, and the physical property balance is excellent.
[0146] [Second embodiment]
[0147] Next, use Figure 2 A thermally conductive sheet according to a second embodiment of the present invention will be described.
[0148] In the first embodiment, the thermally conductive sheet 10 contains the non-anisotropic filler 14 as a filler in addition to the anisotropic filler 13. However, the thermally conductive sheet 20 of this embodiment includes the non-anisotropic filler 14 as a filler. Figure 2 That is, in the thermally conductive sheet of the second embodiment, only carbon fibers may be used as fillers, for example.
[0149] The other configurations of the thermally conductive sheet 20 according to the second embodiment are the same as those of the thermally conductive sheet 10 according to the first embodiment described above, except that the thermally conductive sheet 20 does not contain a non-anisotropic filler, and thus descriptions thereof are omitted.
[0150] In this embodiment, similarly to the first embodiment, the anisotropic filler 13 on the surface is arranged to tilt at a predetermined ratio, thereby improving the thermal conductivity in the thickness direction.
[0151] Example
[0152] Hereinafter, the present invention will be described in more detail using examples, but the present invention is not limited to these examples at all.
[0153] In the present example, the physical properties of the thermally conductive sheet were evaluated by the following methods.
[0154] [Thermal conductivity]
[0155] The thermal conductivity in the thickness direction of the thermally conductive sheet was measured by a method based on ASTM D5470-06.
[0156] [Proportion of anisotropic filler material arranged in a pouring manner]
[0157] One surface of the thermal conductive sheet was observed using an optical microscope "Digital Microscope VHX2000" (manufactured by Keyence Corporation) at a magnification of 200 times and an illumination of 2000 lux based on the JIS Z9110 illumination standard to obtain an observation image. In the observation image, the total number of anisotropic fillers (A) and the number of anisotropic fillers arranged in a pouring manner (B) were visually counted in a measurement area corresponding to 600 to 800 mm × 800 to 1000 mm of the thermal conductive sheet by the method described in the manual, and B / A×100 was calculated. This operation was repeated 100 times in a manner that each became a separate measurement area on one surface of the thermal conductive sheet, and the average value was calculated as the ratio of the anisotropic filler arranged in a pouring manner.
[0158] [Thermal resistance]
[0159] Thermal resistance value use Figure 3 The thermal resistance measuring machine as shown in the figure was used and the measurement was carried out using the method shown below. Specifically, for each sample, a sample S with a size of 30mm×30mm was made for this test. Then, each sample S was attached to a copper block 22 with a measuring surface of 25.4mm×25.4mm and a side covered with an insulating material 21, clamped with an upper copper block 23, and a load was applied using a force sensor (load sensor: load cell) 26, so that the thickness was set to 90.0% of the original thickness. Here, the lower copper block 22 was in contact with the heater 24. In addition, the upper copper block 23 was covered with an insulating material 21 and connected to a heat sink 25 with a fan. Next, the heater 24 was heated with a calorific value of 25W, and 10 minutes after the temperature became roughly stable, the temperature (θ j0 ), the temperature of the copper block 22 below (θ j1 ) and the heat generated by the heater (Q), the thermal resistance value of each sample was calculated using the following formula (1).
[0160] Thermal resistance = (θ j1 -θ j0 ) / Q···Formula (1)
[0161] In formula (1), θ j1 is the temperature of the copper block 22 below, θ j0 is the temperature of the upper copper block 23, and Q is the calorific value.
[0162] [Tilt-type rolling ball adhesion test]
[0163] The thermally conductive sheets manufactured in the examples and comparative examples were adjusted to a size of 20 to 25 mm in width and 50 mm in length to serve as samples. A flat plate (aluminum plate) that was sufficiently larger than the sample was prepared, and the sample was attached to the flat plate in such a manner that the surface to be the object of the rolling ball adhesion test became the surface so that no large height difference was generated. Then, the flat plate to which the sample was attached was set at an inclination angle of 30°.
[0164] Next, the steel ball was placed at the uppermost portion of the sample, and the time until it reached the lowermost portion of the sample (i.e., the time for the steel ball to move the length of the sample 50 mm) was measured, and the adhesion was evaluated using the following five stages. In addition, as the steel ball, a steel ball of SUJ2, a high carbon chromium bearing steel material specified in JIS G 4805, and a weight of 5.4 to 5.5 g was used.
[0165] (evaluate)
[0166] 1: Pass without stopping at all.
[0167] 2: The arrival time is within 1 second, but there is a moment of cessation of movement at the beginning or end of the test.
[0168] 3: The arrival time is greater than 1 second and less than 5 seconds.
[0169] 4: The arrival time is greater than 5 seconds and less than 13 seconds.
[0170] 5: Arrival time is greater than 13 seconds.
[0171] [Example 1]
[0172] A mixed composition was obtained by mixing alkenyl-containing organopolysiloxane and hydrogen-containing organopolysiloxane (total 100 parts by mass, volume filling rate 30% by volume) as a polymer matrix (polymer composition), 130 parts by mass (volume filling rate 18% by volume) of graphitized carbon fibers (average fiber length 100 μm, aspect ratio 10, thermal conductivity 500 W / m·K) as an anisotropic filler, 250 parts by mass (volume filling rate 20% by volume) of alumina powder (spherical, average particle size 10 μm, aspect ratio 1.0) as a non-anisotropic filler, and 250 parts by mass (volume filling rate 32% by volume) of aluminum hydroxide powder (amorphous, average particle size 8 μm) as a non-anisotropic filler. The viscosity of the mixed composition was 40 Pa·s.
[0173] Next, two release materials made of PET films subjected to release treatment with fluororesin were prepared, and the mixed composition was applied to one release material. The other release material was then pressed against the mixed composition and compressed to a thickness of 2 mm to obtain a laminate.
[0174] Next, the laminate was subjected to an 8 Tesla magnetic field in the thickness direction and vibrated by compressed air of a vibrator (vibration intensity was "ultra-weak") to orient the graphitized carbon fibers in the thickness direction, and then heated at 80°C for 60 minutes to solidify the matrix, thereby obtaining a thermally conductive sheet sandwiched between two peeling materials. Next, the two peeling materials were peeled off to obtain a thermally conductive sheet on which the graphitized carbon fibers were not exposed. Both sides of the thermally conductive sheet had adhesive properties.
[0175] A schematic diagram of an image obtained by observing the surface of the thermally conductive sheet obtained in Example 1 with an optical microscope is shown in FIG. Figure 4 In an optical microscope, carbon fibers lying near the surface are observed at a length equal to the actual fiber length, and as the degree of inclination relative to the surface increases, they are observed at a length shorter than the actual fiber length. Figure 4 As shown in FIG. 1 , the carbon fibers 33 on the surface of the thermal conductive sheet are mostly carbon fibers 33A oriented in the thickness direction so that only the end faces of the fibers can be seen. However, a portion of the carbon fibers are carbon fibers 33X arranged in a lying manner along the surface and carbon fibers 33Y inclined relative to the surface, that is, arranged in a tilted manner. The carbon fibers 33 are shown as linear carbon fibers only, but of course, slightly curved carbon fibers may also be used. The evaluation results are shown in Table 1.
[0176] [Example 2]
[0177] The same procedure as in Example 1 was followed except that the intensity of the vibration applied to the laminate was set to "weak" and stronger than that in Example 1, thereby obtaining a thermally conductive sheet having no graphitized carbon fibers exposed on the surface. Both surfaces of the thermally conductive sheet had adhesiveness. The evaluation results are shown in Table 1.
[0178] [Example 3]
[0179] A thermally conductive sheet having no graphitized carbon fibers exposed on the surface was obtained in the same manner as in Example 1 except that the intensity of the vibration applied to the laminate was set to "medium" and stronger than in Example 2. Both surfaces of the thermally conductive sheet had adhesiveness. The evaluation results are shown in Table 1.
[0180] [Example 4]
[0181] A thermally conductive sheet having no graphitized carbon fibers exposed on the surface was obtained in the same manner as in Example 1 except that the intensity of the vibration applied to the laminate was set to "strong" and stronger than in Example 3. Both surfaces of the thermally conductive sheet had adhesiveness. The evaluation results are shown in Table 1.
[0182] [Example 5]
[0183] A thermally conductive sheet having no graphitized carbon fibers exposed on the surface was obtained in the same manner as in Example 1 except that the intensity of the vibration applied to the laminate was set to "super strong" and stronger than that in Example 4. Both surfaces of the thermally conductive sheet had adhesiveness. The evaluation results are shown in Table 1.
[0184] [Example 6]
[0185] The same procedure as in Example 1 was carried out except that the laminate was not subjected to vibration, thereby obtaining a thermally conductive sheet having no graphitized carbon fibers exposed on the surface. Both surfaces of the thermally conductive sheet had adhesiveness. The evaluation results are shown in Table 1.
[0186] [Comparative Example 1]
[0187] A thermally conductive sheet having no graphitized carbon fibers exposed on the surface was obtained in the same manner as in Example 1 except that no magnetic field was applied to the laminate and no vibration was applied.
[0188] Table 1
[0189]
[0190] The results of the above examples clearly show that, by arranging the anisotropic filler material in a thermally conductive sheet so as to tilt at a predetermined ratio near the surface, the desired thermal resistance value and thermal conductivity can be obtained, and the thermal conductivity in the thickness direction can be improved. On the other hand, as shown in the comparative example, if the anisotropic filler material is arranged in a tilted manner, the desired thermal resistance value and thermal conductivity cannot be obtained, and the thermal conductivity in the thickness direction cannot be sufficiently improved.
[0191] Description of Reference Numerals
[0192] 10, 20 Thermally conductive sheet
[0193] 10A, 10B, 20A, 20B surface
[0194] 12 Polymer Matrix
[0195] 13A End Face
[0196] 13B Outer Surface
[0197] 13, 13X, 13Y anisotropic filling materials
[0198] 14 Non-anisotropic filling materials
[0199] 21 Insulation materials
[0200] 22 Copper block below
[0201] 23 The copper block above
[0202] 24 Heater
[0203] 25 Heat sink
[0204] 26 Force sensor
[0205] S specimen
[0206] θ j0 The temperature of the copper block above
[0207] θ j1 The temperature of the copper block below
Claims
1. A thermally conductive sheet comprising a polymer matrix and an anisotropic filler, wherein the anisotropic filler is oriented in a thickness direction. The anisotropic filler is disposed so as to be poured at a ratio of 1 to 45% on both surfaces of the thermally conductive sheet observed through an optical microscope. The anisotropic filler is not exposed on the surface of the thermally conductive sheet. The ratio of the anisotropic filler disposed in a tilted manner on the surface of the thermally conductive sheet is larger than that on other parts of the surface.
2. The thermally conductive sheet according to claim 1, The anisotropic filling material is a fiber material.
3. The thermally conductive sheet according to claim 2, The fiber material is carbon fiber.
4. The thermally conductive sheet according to claim 2, The average fiber length of the fiber material is 50 to 500 μm.
5. The thermally conductive sheet according to claim 1 or 2, Non-anisotropic fill materials are also included.
6. The thermally conductive sheet according to claim 5, The non-anisotropic filler is at least one selected from the group consisting of aluminum oxide, aluminum, zinc oxide, boron nitride, and aluminum nitride.
7. The thermally conductive sheet according to claim 5, The ratio of the volume filling rate of the non-anisotropic filling material to the volume filling rate of the anisotropic filling material is 2-5.
8. The thermally conductive sheet according to claim 1 or 2, At least a portion of the anisotropic filling material arranged in a poured manner in the surface is arranged to be inclined with respect to the surface.
9. The thermally conductive sheet according to claim 1 or 2, The polymer matrix is addition reaction curing type polysiloxane.
10. The thermally conductive sheet according to claim 1 or 2, The thermally conductive sheet has a thickness of 0.1 to 5 mm.
11. The thermally conductive sheet according to claim 1 or 2, The thermal conductivity of the thermally conductive sheet in the thickness direction is 6 w / m·K or more.
12. The thermally conductive sheet according to claim 3, The carbon fibers are covered with an insulating layer.
13. The thermally conductive sheet according to claim 12, The insulating layer includes silicon dioxide.
Citation Information
Patent Citations
Method for manufacturing thermally conductive sheet, and thermally conductive sheet
JP2011231242A
Thermally conductive resin molded product
JP2018014534A
Electromagnetic wave absorption thermal conductive sheet, method of manufacturing the same, and semiconductor device
JP2018056315A
Thermally conductive sheet, method for producing same, and semiconductor device
CN105283952A
Insulated coated carbon fiber, method for manufacturing insulated coated carbon fiber, carbon-fiber-containing composition, and heat-conducting sheet
CN107849803A