Glass wiring substrate
By forming a conductor layer structure with recesses on the glass wiring substrate, the crack problem caused by the concentration of stress of the electrolytic copper plating layer is solved, ensuring the stability and electrical characteristics of the glass plate, while avoiding the resistance caused by the increase in the thickness of the conductor layer Getting higher problem.
Patent Information
- Application Number
- CN201980040498.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-06-19
- Filing Date
- 2019-06-10
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2039-06-10
AI Technical Summary
When the thickness of the electrolytic copper-plated conductor layer formed on the glass plate exceeds 15 μm, stress concentration is easily caused, resulting in cracks in the glass plate, and cracks may be affected by increasing the thickness of the conductor layer to suppress cracks.
By forming a conductor layer structure with a recess on the glass plate, it is ensured that the contact area between the first metal layer and the second metal layer is smaller than the upper surface area of the second metal layer, thereby reducing stress concentration and avoiding the occurrence of cracks.
The generation of cracks under the conductor layer in the glass plate is effectively suppressed, even if the thickness of the conductor layer increases, cracks will not occur, and the electrical characteristics remain stable.
Smart Images

Figure CN112335038B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a glass wiring substrate. Background Art
[0002] In recent years, electronic devices have been increasingly becoming more functional and miniaturized. Along with this, semiconductor modules mounted on electronic devices are required to be more densely packed. In order to meet such requirements, research is underway to improve the wiring density of wiring substrates used to mount semiconductor chips.
[0003] Generally, glass epoxy resin is used as a core material contained in a wiring substrate. However, in recent years, a glass wiring substrate using a glass plate as a core material has attracted attention.
[0004] Compared with the core material composed of glass epoxy resin, the glass plate can achieve higher smoothness. Therefore, it is possible to form ultra-fine wiring on the glass wiring substrate. Therefore, by using the glass wiring substrate, high-density mounting of circuit components can be achieved.
[0005] In addition, the coefficient of linear expansion (CTE) of the glass plate in the temperature range of 20°C to 260°C is substantially the same as the coefficient of linear expansion of the semiconductor chip using the silicon substrate in the temperature range of 20°C to 260°C. Therefore, by using the glass wiring substrate, it is possible to mount the semiconductor chip while suppressing the residual stress.
[0006] As can be seen from the above, the glass wiring substrate has attracted attention as one of the wiring substrates of the semiconductor module mounted in the high-performance electronic equipment.
[0007] As a conventional technology for forming wiring on a glass plate, for example, a structure of a laminated film composed of an inorganic substance containing palladium or the like, an electroless nickel phosphorus plating film, and an electrolytic copper plating film formed on a glass plate is disclosed (see, for example, Patent Document 1).
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2017-81781 Summary of the invention
[0011] [Problems to be Solved by the Invention]
[0012] When the thickness of the conductor layer including the electrolytic copper plating layer formed directly above the glass plate is 15 μm or more, there is a problem of cracks being generated in the glass plate under the conductor layer due to stress of the conductor including the electrolytic copper plating layer. In order to suppress cracks, the conductor layer in the glass wiring substrate needs to be thinner, but this may cause problems in electrical characteristics such as increased circuit resistance.
[0013] Therefore, a glass wiring substrate is desired in which cracks do not occur in the glass plate under the conductor layer even if the thickness of the conductor layer is increased. This problem of cracks is also a concern in the technology of Patent Document 1, in which the thickness of the electrolytic copper plating layer in the conductor layer composed of an inorganic substance containing palladium, a chemical nickel-phosphorus coating, and an electrolytic copper plating coating is increased, and cracks occur in the glass plate under the conductor layer mainly due to the stress of the electrolytic copper plating layer.
[0014] This is because when wiring is formed on a glass plate, the cross-sectional structure of the conductor layer composed of an inorganic substance containing palladium, a chemical nickel-phosphorus coating, and an electrolytic copper-plated coating, which is obtained by etching the unnecessary metal layer, is a rectangular cross-sectional structure. Therefore, the stress of the electrolytic copper-plated layer is easily excessively concentrated on the glass plate directly below the conductor layer, thereby causing cracks.
[0015] The cracks under the conductor layer may also be generated when titanium, copper, and electrolytic copper plating layers are sequentially stacked from the glass plate side by sputtering.
[0016] The present invention has been made in view of the above problems, and an object of the present invention is to provide a glass wiring substrate capable of preventing stress concentration on a glass plate provided with a conductor layer including an electrolytic copper plating layer, thereby suppressing the occurrence of cracks.
[0017] [Means for solving this problem]
[0018] According to one aspect of the present invention, a glass wiring substrate has:
[0019] glass plate,
[0020] a first metal layer covering at least a portion of the glass plate, and
[0021] The second metal layer covering at least a portion of the first metal layer is characterized by:
[0022] An area of the first metal layer in contact with the second metal layer is smaller than an area of the second metal layer facing the first metal layer.
[0023] [Effects of the Invention]
[0024] According to the present invention, there is provided a glass wiring substrate capable of preventing stress from being concentrated on a glass plate provided with a conductor layer including an electrolytic copper plating layer, thereby suppressing the occurrence of cracks. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] [ Figure 1 ] Figure 1 This is a perspective view schematically showing a glass wiring substrate 1 according to one embodiment of the present invention.
[0026] [ Figure 2] Figure 2 It is a cross-sectional view schematically showing a glass wiring substrate 1 according to one embodiment of the present invention.
[0027] [ Figure 3 ] Figure 3 It is shown in detail Figure 2 1 is a cross-sectional view of a glass wiring substrate 2 of a glass wiring substrate 1 according to an embodiment of the present invention.
[0028] [ Figure 4 ] Figure 4 It is a cross-sectional view schematically showing a method for manufacturing glass wiring substrate 2 according to one embodiment of the present invention.
[0029] [ Figure 5 ] Figure 5 It is a cross-sectional view schematically showing a method for manufacturing glass wiring substrate 3 according to an embodiment of the present invention. DETAILED DESCRIPTION
[0030] Hereinafter, the scheme of the present invention will be described with reference to the accompanying drawings. It should be noted that in the following description, the same symbols are used for each part having the same element or the same function, and repeated descriptions are omitted. In addition, in this specification, "up" refers to the direction away from the glass substrate, and "down" refers to the direction close to the glass substrate.
[0031] Figure 1 This is a perspective view schematically showing a glass wiring substrate 1 according to an embodiment of the present invention.
[0032] Figure 1 The glass wiring substrate 1 shown includes a glass plate 10 and a conductor layer 100 formed on the glass plate 10 .
[0033] The glass plate 10 is generally light-transmissive. The composition and ratio of the glass material constituting the glass plate 10 are not particularly limited. As the glass plate 10, for example, glass containing silicate as a main component, such as alkali-free glass, alkali glass, borosilicate glass, quartz glass, sapphire glass, and photosensitive glass, can be used. From the viewpoint of use in semiconductor packaging and semiconductor modules, it is preferable to use alkali-free glass as the glass plate 10. The content of the alkali component contained in the alkali-free glass is preferably 0.1% by mass or less.
[0034] The thickness of the glass plate 10 is preferably 1 mm or less. In view of the ease of forming the through-hole and the workability during production, the thickness of the glass plate 10 is more preferably within a range of 0.1 mm to 0.8 mm.
[0035] Examples of a method for manufacturing the glass plate 10 include a float method, a down-draw method, a fusion method, an up-draw method, and a roll-out method. The glass plate 10 can be manufactured by any method.
[0036] In the temperature range of 20°C to 260°C, the coefficient of thermal expansion (CTE) of the glass plate 10 is preferably within 0.5×10 -6 / K above 160×10 -6 / K or less, more preferably within the range of 0.8×10 -6 / K above 50×10 -6 / K or less, and more preferably within 1.0×10 -6 / K above 8.0×10 -6 / K or less. When the linear expansion coefficient of the glass plate 10 is within this range, the difference in linear expansion coefficient with the semiconductor chip using a silicon substrate mounted on the surface of the glass wiring substrate 1 tends to be small. It should be noted that the linear expansion coefficient refers to the ratio of the length change with respect to the increase in temperature.
[0037] At least one main plane of the glass plate 10 may be provided with a functional layer. Examples of the functional layer include an antireflection layer containing microparticles, an infrared shielding layer containing an infrared absorber, a strength-imparting layer containing a hard coating material, an antistatic layer containing an antistatic agent, a coloring layer containing a coloring agent, an optical filter layer containing an optical thin film, a texture control layer containing a light scattering film, and an antiglare layer. These functional layers may be formed, for example, by a surface treatment technique such as a vapor deposition method, a sputtering method, or a wet method.
[0038] The glass plate 10 may also be provided with through holes.
[0039] The shape of the cross section of the through hole parallel to the thickness direction can be a rectangle; it can also be an X-shape, that is, a shape in which the diameter of the central portion is smaller than the top diameter and the bottom diameter of the through hole; it can also be a cone, that is, a shape in which the bottom diameter is smaller than the top diameter of the through hole; it can also be an O-shape, that is, a shape in which the diameter of the central portion is larger than the top diameter and the bottom diameter of the through hole; it can also be other shapes.
[0040] The shape of the cross section of the through hole perpendicular to the thickness direction may be circular, elliptical, or polygonal.
[0041] Figure 2 is Figure 1The glass wiring substrate 1 shown is a cross-sectional view of the glass wiring substrate obtained by cutting along a plane passing through the FF line so as to be perpendicular to the longitudinal direction of the wiring formed on the glass plate 10.
[0042] like Figure 2 As shown, a conductor layer 100 is provided on the glass plate 10 on the glass main plane 10a side. The conductor layer 100 is composed of a first metal layer 60 and a second metal layer 70. The conductor layer 100 (for example) constitutes a circuit wiring or an electrode pad. The conductor layer 100 can be provided on any one surface of the glass plate 10, or on both surfaces.
[0043] The first metal layer 60 covers at least a portion of the main plane 10a of the glass plate 10. Furthermore, the second metal layer 70 covers at least a portion of the first metal layer 60. The lower surface of the second metal layer 70 is eroded and worn away near the edge of the upper surface of the first metal layer 60, and contacts the upper surface of the first metal layer 60 on the inner side thereof. It can be seen from this that the area where the first metal layer 60 contacts the second metal layer 70 is smaller than the area of the second metal layer 70 facing the first metal layer 60. In other words, the lower surface of the second metal layer 70 has an area (peripheral area) that is not in contact with the upper surface of the first metal layer 60.
[0044] Specifically, if Figure 2 As shown, the second metal layer 70 forms recesses 701 on both sides of the surface facing the first metal layer 60. The recesses 701 have depths a and b from the end of the conductor layer toward the center. Therefore, the cross-sectional shape of the conductor formed by the first metal layer 60 and the second metal layer 70 is not rectangular, but has a shape with recesses 701 (narrowed in the middle) near the bonding surface. By providing such recesses 701, the area where the first metal layer 60 and the second metal layer 70 are in contact is smaller than the area of the lower surface of the second metal layer 70 facing the upper surface of the first metal layer 60. Therefore, compared with the case where no narrowing portion is provided, the stress of the second metal layer 70 can be suppressed from concentrating on the glass main plane 10a, making it difficult to generate cracks.
[0045] The depths a and b of the recess 701 may be the same or different on both sides.
[0046] Figure 3 The glass wiring substrate 2 shown is shown in more detail Figure 2 FIG. 1 is a diagram of a glass wiring substrate 1 shown.
[0047] The conductor layer 1000 is composed of a first metal layer 600 and a second metal layer 700. In addition, the first metal layer 600 is, for example, sequentially stacked with a metal layer 200, a metal layer 300, and a metal layer 500, and has a metal inclusion 400 between the metal layer 300 and the metal layer 500. It should be noted that the number of metal layers in the first metal layer 600 is not limited to this example.
[0048] The second metal layer 700 is formed by plating. For example, copper (Cu) or an alloy containing copper can be selected as the plating for forming the second metal layer 700, but electrolytic copper plating with excellent conductivity is preferred.
[0049] The metal layer 200 and the metal layer 300 are formed by sputtering or chemical vapor deposition (CVD). For example, metals such as copper (Cu), aluminum (Al), titanium (Ti), chromium (Cr), molybdenum (Mo), tungsten (W), tantalum (Ta), gold (Au), iridium (Ir), ruthenium (Ru), palladium (Pd), and platinum (Pt) can be listed. In addition, as a conductive material, Al-Si alloys, Al-Si-Cu alloys, Al-Cu alloys, Ni-Fe alloys, indium tin oxide (ITO), indium zinc oxide (IZO), active zinc oxide (AZO), zinc oxide (ZnO), lead zirconate titanate (PZT), titanium nitride (TiN), Cu 3 N 4 , Cu alloy, or a mixture thereof.
[0050] The metal layer 200 and the metal layer 300 are preferably formed of titanium and copper, respectively, by a sputtering method.
[0051] When the metal layer 200 is made of titanium, the thickness of the titanium is preferably in the range of 0.01 μm to 0.1 μm. By setting the thickness of the titanium to be 0.01 μm or more, good adhesion to the glass can be exhibited. On the other hand, even if the thickness of the titanium is greater than 0.1 μm, the adhesion to the glass does not change, so from the perspective of productivity, it is preferred that the thickness of the titanium be 0.1 μm or less.
[0052] When the metal layer 300 is made of copper, the thickness of the copper is preferably in the range of 0.09 μm to 0.5 μm. By setting the thickness of the copper to 0.09 μm or more, the metal layer 500 described later can be formed densely without pinholes on the metal layer 300 made of copper. Therefore, the electrical characteristics are improved. On the other hand, even if the thickness of the copper is greater than 0.5 μm, no change is found in the electrical characteristics, so from the perspective of productivity, it is preferred to set the thickness of the copper to 0.5 μm or less.
[0053] The metal layer 500 is made of chemical nickel-phosphorus plating. The metal layer 500 is formed by chemical nickel-phosphorus plating at a lower etching rate than the second metal layer 700 made of electrolytic copper plating, so that when forming wiring, in the process of etching the unnecessary metal layer 500 made of chemical nickel-phosphorus plating, the second metal side made of electrolytic copper plating in contact with the first metal layer 600 is preferentially etched, thereby forming a concave portion 701 on the side of the second metal layer 700 made of electrolytic copper plating in contact with the first metal layer 600.
[0054] Therefore, the area of the second metal layer 700 formed of electrolytic copper plating in contact with the first metal layer 600 is smaller than the area of the lower surface of the second metal layer 700 facing the upper surface of the first metal layer 600 .
[0055] The chemically plated nickel-phosphorus layer may contain other components, such as sulfur (S), lead (Pb) and bismuth (Bi), in addition to nickel and phosphorus.
[0056] The chemical nickel-phosphorus plating solution contains a nickel-containing metal salt and a reducing agent. Examples of the nickel-containing metal salt include nickel sulfate, nickel chloride, or a mixture thereof. The concentration of the nickel-containing metal salt contained in the chemical nickel-phosphorus plating solution is preferably in the range of 10 g / L to 60 g / L, more preferably in the range of 15 g / L to 45 g / L, and further preferably in the range of 20 g / L to 30 g / L.
[0057] The reducing agent reduces the nickel-containing metal salt. Examples of the reducing agent include formalin, hydrazine, hypophosphorous acid, sodium hypophosphite, sodium borohydride, or a mixture thereof, but hypophosphorous acid, sodium hypophosphite, or a mixture thereof is preferably used. The concentration of the reducing agent contained in the chemical nickel-plating phosphorus solution is preferably in the range of 10 g / L to 60 g / L, more preferably in the range of 15 g / L to 45 g / L, and further preferably in the range of 20 g / L to 30 g / L.
[0058] The chemical nickel phosphorus plating solution may further contain a metal additive, an organic additive, a complexing agent, a pH adjuster, a buffer, or a mixture thereof.
[0059] The metal additive improves the stability of the electroless nickel phosphorus plating solution. The metal additive may include lead, bismuth or a mixture thereof.
[0060] The organic additive promotes the precipitation of nickel. The organic additive contains, for example, sulfur.
[0061] As the complexing agent, for example, ammonia water, sodium citrate, ethylene glycol or a mixture thereof can be cited. The concentration of the complexing agent contained in the chemical nickel phosphorus plating solution is preferably in the range of 10 g / L to 60 g / L, more preferably in the range of 10 g / L to 50 g / L, and further preferably in the range of 20 g / L to 30 g / L.
[0062] Examples of the pH adjuster include sodium hydroxide, ammonia, sulfuric acid, and mixtures thereof.
[0063] Examples of the buffer include sodium citrate, boric acid, carbonic acid, and mixtures thereof.
[0064] In addition, the chemical nickel-plating phosphorus solution may also contain ammonium chloride. The concentration of ammonium chloride contained in the chemical nickel-plating phosphorus solution is preferably in the range of 10 g / L to 60 g / L, more preferably in the range of 10 g / L to 50 g / L, and further preferably in the range of 20 g / L to 30 g / L.
[0065] When the phosphorus content in the chemical nickel-phosphorus plating film is set to 5 mass % or more and 12 mass % or less, the pH of the chemical nickel-phosphorus plating solution is preferably set in the range of 3 or more and 6 or less, and more preferably in the range of 5.0 or more and 5.5 or less. In addition, the temperature of the chemical nickel-phosphorus plating solution is preferably set in the range of (for example) 60° C. or more and 80° C. or less.
[0066] When the phosphorus content in the chemical nickel-phosphorus plating film is set to be greater than 0.5 mass % and less than 5 mass %, during the chemical plating treatment, the pH of the chemical nickel-phosphorus plating solution is preferably set in the range of greater than 7 and less than 9, and the temperature of the chemical nickel-phosphorus plating solution is preferably set in the range of (for example) greater than 30°C and less than 60°C.
[0067] The thickness of the chemically plated nickel-phosphorus layer can be obtained, for example, by X-ray fluorescence elemental analysis.
[0068] The metal inclusion 400 is between the metal layer 300 composed of copper and the metal layer 500 composed of chemically plated nickel-phosphorus. The metal inclusion 400 contains at least palladium. The metal inclusion 400 can also form a layer. The palladium in the metal inclusion 400 is used as a catalyst for forming chemically plated nickel-phosphorus. Palladium can be used alone, or in a mixture with an inorganic substance, or in a mixture with an organic substance, or further in a mixture with an organic substance and an inorganic substance.
[0069] At the interface where the second metal layer 700 formed of electrolytic copper plating contacts the metal layer 500 formed of chemical nickel-phosphorus plating, the recessed portion formed in the second metal layer 700 can be controlled by the coverage rate (the amount of palladium per unit area) of palladium contained in the metal inclusion 400. As the coverage rate of palladium increases from 0.01 μg / cm 2 Increase to 500 μg / cm 2 The contact area between the second metal layer 700 formed by electrolytic copper plating and the metal layer 500 formed by chemical nickel-phosphorus plating is reduced. That is, the depths a and b of the concave portion 701 are increased.
[0070] When palladium is used alone, the coverage of palladium contained in the metal-containing material 400 with respect to the metal layer 300 composed of copper is preferably 0.01 μg / cm 2 Above 500 μg / cm 2 The palladium coverage is less than 0.01 μg / cm 2 In the case of , the catalytic activity of palladium is weakened, and it is difficult to form the metal layer 500 composed of chemically plated nickel phosphorus, which is not preferred. In addition, the cross-sectional structure of the conductor layer 1000 is close to a rectangle, and the effect of suppressing cracks cannot be obtained.
[0071] In addition, when the metal layer 500 composed of chemically plated nickel phosphorus and the metal layer 300 composed of copper are etched during wiring formation, the metal inclusion 400 containing at least palladium is removed, but the palladium coverage is greater than 500 μg / cm 2 In the case of , when etching the metal layer 500 composed of chemically plated nickel phosphorus and the metal layer 300 composed of copper, it is difficult to remove the palladium in the metal-containing material 400, so it is not preferred. The palladium coverage is more preferably 1 μg / cm 2 Above 100 μg / cm 2 Within the following range.
[0072] The coverage of palladium in the metal-containing material 400 with respect to the copper-containing metal layer 300 can be controlled by the immersion time of the catalytic metal layer 300 in the palladium treatment solution. The palladium treatment solution can use a substance containing a palladium complex or a colloidal solution of tin and palladium.
[0073] An intermetallic compound layer derived from each metal may be formed at each interface of the metal layer 200 composed of titanium, the metal layer 300 composed of copper, the metal inclusion 400 containing at least palladium, and the metal layer 500 composed of chemically plated nickel phosphorus.
[0074] In the cross-sectional view, the contact areas of the metal layer 200 made of titanium, the metal layer 300 made of copper, and the metal layer 500 made of chemically plated nickel phosphorus may be different.
[0075] Next, refer to Figure 4 (A) to Figure 4 (G) Figure 3 An example of a method for manufacturing the glass wiring substrate 2 shown in FIG.
[0076] First, prepare the glass plate 10. Figure 4 As shown in (A), metal layers 200 and 300 are stacked in order from the glass side on the main plane 10a of the glass plate 10. Specifically, a titanium layer and a copper layer are formed as the metal layers 200 and 300 on one main plane of the glass plate 10 by sputtering.
[0077] Then, if Figure 4 As shown in (B), the metal inclusion 400 is formed on the metal layer 300, and then the metal layer 500 is formed. Specifically, as the metal inclusion 400 and the metal layer 500, a layer containing at least palladium and an electroless nickel-phosphorus plating layer are formed.
[0078] Then, if Figure 4 As shown in (C), a dry film resist is laminated on the metal layer 500 formed of electroless nickel phosphorus plated on the glass main plane 10a using a roll laminator or the like, and a resist layer RE1 having an opening RE0 is formed by photolithography.
[0079] Then, if Figure 4 As shown in FIG. 5D , a second metal layer 700 composed of electrolytic copper is formed on the metal layer 500 composed of chemically plated nickel-phosphorus by electroplating in an electrolytic copper plating solution.
[0080] Next, the resist layer RE1 is peeled off in a sodium hydroxide solution or a TMAH solution, thereby obtaining Figure 4 (E) The substrate shown.
[0081] Then, if Figure 4 As shown in (F), the metal layer 500 composed of chemically plated nickel-phosphorus and the metal layer 300 composed of copper are etched in sequence. At this time, due to the catalytic action of palladium in the metal inclusion 400, the second metal layer 700 composed of electrolytic copper plating is corroded at the periphery of the side in contact with the metal layer 500 composed of chemically plated nickel, thereby forming a concave portion 701.
[0082] Next, the metal layer 200 composed of titanium is etched to obtain Figure 4In this way, a first metal layer 600 composed of a metal layer 200 covering at least a portion of a glass plate 10, a metal layer 300, a metal inclusion 400, and a metal layer 500, and a second metal layer 700 covering at least a portion of the first metal layer are obtained, and further a glass wiring substrate is obtained in which the area of the first metal layer 600 in contact with the second metal layer 700 is smaller than the area of the second metal layer 700 facing the first metal layer 600.
[0083] According to the structure of the glass wiring substrate, stress applied to the glass directly below the second metal layer 700 composed of electrolytic copper plating can be relieved, and cracks in the glass plate 10 can be suppressed even when the thickness of the formed electrolytic copper plating layer exceeds 15 μm.
[0084] It should be noted that the present invention is not limited to the above-mentioned embodiments and modifications, and various modifications can be made without departing from the gist of the present invention.
[0085] Example
[0086] Hereinafter, examples related to the evaluation of the presence or absence of glass cracks under the conductor layer will be described in comparison with comparative examples.
[0087] [Judging whether there are glass cracks under the conductor layer]
[0088] Next, regarding the glass wiring substrates obtained in Examples 1 and 2 and Comparative Example 1, the glass plate under the conductor layer was observed by a scanning electron microscope (SEM), and the presence or absence of glass cracks was determined when the number of samples N = 10.
[0089] <Example 1>
[0090] In this embodiment, according to Figure 5 A glass wiring substrate 3 was produced in the manufacturing example.
[0091] First, if Figure 5 As shown in (A), a glass plate 11 (OA-10G, manufactured by Nippon Denki Glass Co., Ltd.) with a thickness of 300 μm is prepared, and a titanium layer 21 with a thickness of 50 nm and a copper layer 31 with a thickness of 300 nm are deposited on one surface of the glass plate 11 by sputtering.
[0092] Then, if Figure 5 As shown in (B), a palladium-containing material 41 is provided on the copper layer 31. At room temperature, Figure 5 The substrate shown in (A) was immersed in a 1 g / L palladium chloride solution for 60 seconds to form a palladium-containing material 41. At this time, the palladium coverage of the palladium-containing material 41 on the copper layer 31 was 1 μg / cm 2Furthermore, by immersing in a plating solution, an electroless nickel-phosphorus plating layer 51 with a thickness of 0.1 μm is formed on the palladium-containing material 41 .
[0093] In this manner, the first metal layer 61 composed of the titanium layer 21 , the copper layer 31 , the palladium-containing material 41 , and the chemical nickel-phosphorus plating layer 51 is provided on the glass plate 11 .
[0094] Then, if Figure 5 As shown in (C), a photosensitive dry film resist with a thickness of 56 μm is laminated on the chemical nickel phosphorus plating layer 51 using a roll laminator to form a first resist layer RE2, and an opening RE0 is provided by exposing and developing a predetermined position. The opening size of RE0 is about 500 μm×500 μm.
[0095] Then, if Figure 5 As shown in (D), the substrate is immersed in a copper sulfate plating solution, and an electrolytic copper plating layer 71 is formed at 1 ASD (current density) to a thickness of 15 μm.
[0096] Next, in Figure 5 The substrate obtained in (D) was immersed in a 5% sodium hydroxide aqueous solution at 60°C to peel off RE2, thereby obtaining Figure 5 (E) substrate.
[0097] Then, if Figure 5 As shown in (F), the chemical nickel-phosphorus plating layer 51, the palladium-containing material 41, and the copper layer 31 are etched using a mixed solution of hydrogen peroxide and sulfuric acid (pH 1, temperature 25° C.), thereby obtaining an electrolytic copper-plated layer 71 having a recessed portion 701.
[0098] Then, if Figure 5 As shown in (G), the titanium layer 21 is removed using a mixed solution of hydrogen peroxide and ammonia (pH 9, temperature 25°C).
[0099] In this manner, a first metal layer 61 consisting of a titanium layer 21, a copper layer 31, a palladium-containing substance 41, and a chemically plated nickel-phosphorus layer 51, which covers at least a portion of the glass, and an electrolytic copper-plated layer 71 constituting a second metal layer covering at least a portion of the first metal layer 61 are obtained, and further a glass wiring substrate 3 is obtained in which the contact area between the first metal layer 61 and the electrolytic copper-plated layer 71 constituting the second metal layer is smaller than the area of the electrolytic copper-plated layer 71 constituting the second metal layer toward the side of the first metal layer 61.
[0100] At this time, the area where the first metal layer 61 contacts the electrolytic copper plating layer 71 constituting the second metal layer is 24.9×10 3 μm 2On the other hand, the area of the electrolytic copper plating layer 71 constituting the second metal layer facing the first metal layer 61 is 25.0×10 3 μm 2 It should be noted that as a method for calculating the area, the glass wiring substrate 3 is cut, and its cut surface is observed with a microscope to calculate the size of the upper surface of the first metal layer 61 and the size of the lower surface of the second metal layer 71 protruding laterally from the upper surface of the first metal layer 61, and the areas are calculated respectively.
[0101] <Example 2>
[0102] In Example 2, the thickness of the electrolytic copper plating layer 71 in Example 1 was set to 25 μm. Example 2 was formed by the same manufacturing method as Example 1 except for the above.
[0103] At this time, the area where the first metal layer 61 contacts the electrolytic copper plating layer 71 constituting the second metal layer is 24.5×10 3 μm 2 The area of the electrolytic copper plating layer 71 constituting the second metal layer facing the first metal layer 61 is 25.0×10 3 μm 2 .
[0104] <Comparative Example 1>
[0105] In this comparative example 1, a glass wiring substrate was obtained by the same method as in Example 1 except that the palladium-containing material 41 and the chemical nickel-phosphorus plating layer 51 were not used and the electrolytic copper plating layer 71 constituting the second metal layer was formed on the titanium layer 21 and the copper layer 31 .
[0106] The electrolytic copper plating layer in the obtained conductor layer has no concave portion, and a conductor layer with a rectangular cross-section shape is obtained (not shown). That is, the area where the copper layer 31 constituting the first metal layer contacts the electrolytic copper plating layer 71 constituting the second metal layer, and the area of the electrolytic copper plating layer 71 constituting the second metal layer facing the copper layer 31 constituting the first metal layer are both 25.0×10 3 μm 2 .
[0107] Table 1 is a summary of the above results of Examples 1 and 2 and Comparative Example 1. It should be noted that, regarding the evaluation of glass cracks, the surface of the glass wiring substrate was examined with a microscope to determine whether there were cracks. In the evaluation in Table 1, 10 / 10OK means that 10 samples were evaluated and no cracks were generated in all 10 samples; 10 / 10NG means that 10 samples were evaluated and all 10 samples were cracked.
[0108] [Table 1]
[0109]
[0110] As shown in Table 1, in the glass wiring substrates of Examples 1 and 2, when the thickness of the electrolytic copper plating layer was set to 15 μm or 25 μm, no glass cracks were found under the conductor layer composed of the titanium layer, the copper layer, the chemical nickel-phosphorus plating layer, and the electrolytic copper plating layer. On the other hand, in the glass wiring substrate of Comparative Example 1, cracks were generated even when the thickness of the electrolytic copper plating layer was set to 15 μm. Therefore, the effect of using the palladium-containing material was confirmed.
[0111] Explanation of symbols
[0112] 1, 2, 3···Glass wiring substrate, 10, 11···Glass plate, 20, 30, 50···Metal layer, 40···Metal containing layer, 60, 61, 600···First metal layer, 70, 700···Second metal layer, 21···Titanium layer, 31···Copper layer, 41···Palladium containing, 51···Chemical nickel phosphorus plating layer, 71···Electrolytic copper plating layer, 701···Recessed portion, RE1, RE2···Anti-etching layer.
Claims
1. A glass wiring substrate, It is characterized in that have: glass plate, a first metal layer covering at least a portion of the glass plate, and a second metal layer covering at least a portion of the first metal layer, The area of the first metal layer in contact with the second metal layer is smaller than the area of the second metal layer facing the first metal layer. The first metal layer is stacked with a plurality of metals, The first metal layer is formed by laminating titanium, copper, and chemically plated nickel-phosphorus in this order from the glass plate side, and a palladium-containing substance is disposed between the copper layer and the chemically plated nickel-phosphorus layer.
2. The glass wiring substrate according to claim 1, Features: The second metal layer is an electrolytic copper plating layer.
3. The glass wiring substrate according to claim 1 or claim 2, Features: The second metal layer is corroded near the outer periphery of the surface in contact with the first metal layer.