Mask Blanks and Photomasks for EUV Lithography
By optimizing the multilayer film structure and processing technology of extreme ultraviolet lithography masks, the problems of pattern distortion, substrate and capping film oxidation were solved, achieving high-precision pattern transfer and resolution improvement.
Patent Information
- Application Number
- CN202011221137.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-05
- Filing Date
- 2020-11-05
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-11-05
AI Technical Summary
Existing extreme ultraviolet lithography technology suffers from problems such as pattern distortion, base phenomenon, flatness issues, and oxide coating, which affect resolution and pattern position accuracy, especially when forming patterns of 7 nanometers or smaller.
The design employs a multi-layer structure of reflective film, cover film, and absorbent film, including a stress control layer and a back conductive film. Oxidation is suppressed by electron beam treatment, the etching process is optimized to improve flatness and prevent substrate damage, and specific materials and processing techniques are used to enhance the oxidation resistance of the cover film.
It effectively improves the flatness of extreme ultraviolet lithography masks, prevents the base phenomenon and oxidation of the cover film, improves the pattern position accuracy and resolution, and ensures high-precision pattern transfer.
Smart Images

Figure CN112782931B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a blank mask and a photomask for extreme ultraviolet lithography, and more particularly, to a blank mask and a photomask for extreme ultraviolet lithography capable of implementing fine patterns of 14 nanometers or less (particularly 10 nanometers or 7 nanometers or less) using extreme ultraviolet (EUV) light of 13.5 nanometers as exposure light. Background Art
[0002] Recently, lithography technology for manufacturing semiconductors has evolved from ArF, ArFi, and multiple (MP) lithography to EUV lithography technology. EUV lithography is a technology that has attracted attention for manufacturing semiconductor devices of 10 nanometers or less, because EUV lithography can achieve solution and process simplification by using an exposure wavelength of 13.5 nanometers.
[0003] On the other hand, EUV lithography can not use the existing refractive optical system, such as lithography using KrF or ArF light, because EUV light is well absorbed by all materials and the refractive index of the material at the wavelength is close to 1. For this reason, in EUV lithography, a photomask using a reflective optical system is used.
[0004] The blank mask is a raw material of a photomask and is configured to include two thin films on a substrate to form a reflective structure: a reflective film that reflects EUV light and an absorption film that absorbs EUV light. In addition, the blank mask may include a cover film that protects the reflective film, a back conductive film for e-chucking, and the like. More specifically, the blank mask for EUV is configured to include a SiO2 film having a low thermal expansion coefficient. 2 -TiO 2 A reflective film made of Mo / Si on a low thermal expansion material (LTEM) substrate, a ruthenium (Ru)-based capping film on the reflective film, and a tantalum (Ta)-based absorption film on the capping film. The photomask formed in this way has a form in which the absorption film is patterned, and uses the principle of forming a pattern on a wafer by using the contrast difference between the reflectivity of the reflective film and the reflectivity of the absorption film.
[0005] When a pattern is formed using the EUV blank mask as described above, the following problems occur.
[0006] First, as the size of the pattern to be implemented is miniaturized, problems such as distortion of the implemented pattern profile (especially the footing of the pattern) directly affect the resolution. In particular, the footing problem occurring in the sub-resolution feature size (SFRS) CD pattern used to correct the optical proximity effect and the main pattern to be implemented has a fatal influence on the resolution.
[0007] Specifically, the tantalum (Ta)-based material that forms the absorption film pattern of the EUV blank mask is generally formed in a two-layer structure, in which the lower layer does not contain oxygen and the upper layer is formed to contain oxygen. In addition, in order to control the shielding effect, the upper layer containing oxygen has a thickness of 15 nanometers or less, and has recently been formed to have a thickness of 10 nanometers or less. Since the upper layer containing oxygen has the property of being etched with a fluorine-based etching gas, in general, the pattern profile of the absorption film and phenomena such as footing are determined by the lower layer of the absorption film. In addition, the lower layer of the absorption film is relatively thicker than the upper layer of the absorption film, and the etching radical component is relatively lower than the surface in the depth direction during etching, and therefore there is a problem of an increased probability of the footing phenomenon occurring.
[0008] Second, the following problem also occurs in the flatness of the EUV blank mask.
[0009] Generally, the flatness of an EUV blank mask can be classified into two types, namely, the flatness of an absorption film and the flatness of a cover film including a reflection film.
[0010] Regarding the flatness of the absorption film, the absorption film is the part that finally forms the pattern after film formation, and the residual stress generated during film formation is released while the pattern is formed, so the registration problem occurs during the release. Recently, due to the size of the fine pattern, the registration problem at each position has emerged as a more important problem.
[0011] However, in the case of forming a pattern on a current tantalum (Ta)-based absorption film, there is no registration problem when forming a pattern of 10 nanometers or less, but a registration problem caused by residual stress occurs when forming a pattern of 7 nanometers or less. In addition, the registration problem has a more fatal effect on EUV lithography in which the exposure light is obliquely incident at an incident angle of 6°. This is because in the EUV exposure process by reflected light, not only the residual stress on the entire surface of each mask is different, but also the residual stress in the micro region is different, and thus the pattern position varies in any portion and the shielding effect caused by the exposure light incident at an angle of 6° increases.
[0012] The problem of the flatness of the cover film including the reflective film involves the stress of the film. Since the EUV exposure light is tilted at 6° and transferred to the wafer PR through a reflection path, when the flatness of the cover film including the reflective film is high, a difference occurs between the ideal reflection path and the actual reflection path, and thus a pattern position error occurs in the transferred pattern. The flatness of the cover film is affected by at least one of the reflective film, the LTEM substrate, and the thin film under the cover film (e.g., a back conductive film formed on the rear surface of the LTEM substrate). However, the reflective film formed by forming 40 pairs of Mo / Si generally has a convex cross-sectional shape, and the back conductive film made of a chromium (Cr)-based material generally has a concave cross-sectional shape. Therefore, the convexity of the surface of the reflective film is eventually deepened, and thus the flatness is further increased. Therefore, there is a problem that the difference between the path of the actual reflected light and the path of the ideal reflected light is greater, and thus the problem of the pattern position error becomes worse.
[0013] Thirdly, the ruthenium (Ru)-based material forming the capping film causes the following problems.
[0014] Ruthenium (Ru)-based materials play a role in reducing the degree of oxidation and protecting the lower reflective film during etching. However, ruthenium (Ru)-based materials are oxidized by cleaning solutions such as ozone water and DI water, and ruthenium (Ru) of the cover film and silicon (Si) of the reflective film under the cover film are oxidized due to high energy during repeated exposure to the wafer. Therefore, damage to the cover film occurs, resulting in a decrease in reflectivity to exposure light, an increase in the incidence of defects, and an adverse effect on the thin film (absorption film, phase shift film, or the like) on the cover film. Summary of the invention
[0015] The present disclosure will provide a blank mask for extreme ultraviolet lithography, which can prevent footing of an EUV photomask pattern from occurring, improve flatness of the EUV blank mask, and prevent oxidation and defects of a capping film.
[0016] According to one aspect of the present disclosure, a blank mask for extreme ultraviolet lithography includes a reflective film, a cover film, and an absorption film sequentially formed on a transparent substrate, wherein the reflective film has a surface roughness of 0.5 nanometer Ra or less.
[0017] The reflective film can be a Mo / Si structure, Mo / B 4 C / Si / C / Mo structure and Mo / C / Si / B 4 A C / Mo structure in which multiple layers are stacked.
[0018] B in reflective film 4 At least one of C or C may be formed as a layer having a thickness of 0.1 nm to 5 nm.
[0019] The reflective film may be heat-treated at a temperature of 200°C to 500°C.
[0020] The reflective film or the cover film may be subjected to electrical neutralization treatment for suppressing formation of an oxide film by electron beam treatment after film formation.
[0021] The blank mask may further include a stress control layer disposed between the transparent substrate and the reflective film and having a concave shape.
[0022] The stress control layer may be made of a material containing at least one of the following: Cr, Ta, B, Mo, V, Co, Ag, Sb, Ti, I, Pb, Ga, Bi, Co, Sn, Te, Ni, Zr, Si, Nb, Pt, Pd, Zn, Al, Mn, Cd, Mg, Li, Se, Cu, Hf and W, or further containing at least one of oxygen (O), nitrogen (N), carbon (C), boron (B) and hydrogen (H).
[0023] The stress control layer may have a thickness of 10 nanometers to 100 nanometers.
[0024] The capping film may be made of a material containing at least one of Ru and Nb, or further containing at least one light element of oxygen (O), nitrogen (N), and carbon (C).
[0025] The absorption film may be made of a tantalum (Ta) compound having a two-layer structure in which an upper layer contains oxygen (O) and a lower layer does not contain oxygen (O).
[0026] The lower layer may be made of a material containing at least one of tantalum (Ta), tantalum nitride (TaN), tantalum carbonitride (TaCN), tantalum carbide (TaC), tantalum boride (TaB), tantalum boronitride (TaBN) and tantalum borocarbide (TaBC), or further containing hydrogen (H).
[0027] The lower layer may be formed as a continuous film having a composition ratio that varies in the thickness direction.
[0028] The absorption film may be made of a tantalum (Ta) compound having a three-layer structure.
[0029] The absorption film may be formed such that the nitrogen (N) content in the intermediate layer is higher than the nitrogen (N) content in the lower layer by 1 atomic % to 20 atomic %.
[0030] The intermediate layer of the absorber film may have a thickness of 3 nm to 40 nm.
[0031] The absorption film may have a structure of two or more layers and may be made of a tantalum (Ta) compound, and a layer below an upper layer of the absorption film may have a composition ratio of Ta:N=95 atomic %:5 atomic % to 50 atomic %:50 atomic %.
[0032] The absorption film may be made of a tantalum (Ta) compound containing boron (B), and may have a composition ratio of 40 to 90 atomic % of Ta, 5 to 20 atomic % of B, and 5 to 50 atomic % of N.
[0033] The absorption film may have a structure of two or more layers and may be made of a tantalum (Ta) compound, and an upper layer may be formed to contain 50 atomic % to 90 atomic % of oxygen (O).
[0034] The blank mask may further include a hard mask film formed on the absorption film.
[0035] The hard mask film may be made of a material containing at least one of the following: Cr, Ta, Mo, V, Co, Ag, Sb, I, Pb, Ga, Bi, Co, Sn, Te, Ni, Zr, Si, Nb, Pt, Pd, Zn, Al, Mn, Cd, Mg, Li, Se, Cu, Hf and W, or further containing at least one selected from oxygen (O), nitrogen (N), carbon (C), boron (B) and hydrogen (H).
[0036] The blank mask may further include a back conductive film disposed under the transparent substrate.
[0037] The back conductive film may have a sheet resistance of 100 ohms / □ or less.
[0038] The back conductive film may be made of a material containing at least one of the following: Cr, Ta, Mo, V, Co, Ag, Sb, I, Pb, Ga, Bi, Co, Sn, Te, Ni, Zr, Si, Nb, Pt, Pd, Zn, Al, Mn, Cd, Mg, Li, Se, Cu, Hf and W, or further containing at least one of oxygen (O), nitrogen (N), carbon (C), boron (B) and hydrogen (H).
[0039] The back conductive film may be made of chromium (Cr), a chromium (Cr) compound, or a compound in which a metal material is contained in chromium (Cr). The back conductive film may have a three-layer structure in which a first layer contacts the rear surface of the transparent substrate, a second layer is formed on the first layer, and a third layer is formed on the second layer. The first layer and the third layer may contain oxygen (O), and the second layer may not contain oxygen (O).
[0040] The first layer and the third layer may have a composition ratio in which chromium (Cr) is 20 atomic % to 70 atomic % and C, O and N are 30 atomic % to 80 atomic % in total, and the second layer may have a composition ratio of Cr:N=70 atomic %:30 atomic % to 20 atomic %:80 atomic %.
[0041] According to another aspect of the present disclosure, a photomask for extreme ultraviolet lithography is provided, the photomask being manufactured using the blank mask for extreme ultraviolet lithography having the above configuration.
[0042] According to the present disclosure, the flatness of the EUV blank mask is improved, and oxidation and defects of the cover film are prevented. In addition, footing is prevented from occurring in the pattern of the EUV photomask manufactured by this blank mask. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] The above and other aspects, features and advantages of certain embodiments of the present disclosure will become more apparent from the following detailed description taken in conjunction with the accompanying drawings.
[0044] Figure 1 is a cross-sectional view of a photomask for extreme ultraviolet lithography according to the present disclosure.
[0045] Figure 2 It is shown Figure 1 FIG. 4 is a diagram showing a specific configuration of the back conductive film.
[0046] Description of Figure Numbers
[0047] 100: blank mask;
[0048] 102: Transparent substrate;
[0049] 104: reflective film;
[0050] 106: covering film;
[0051] 108: Absorption film;
[0052] 110: conductive film;
[0053] 110-1: First floor;
[0054] 110-2: Second floor;
[0055] 110-3: Third floor. DETAILED DESCRIPTION
[0056] Figure 1 is a cross-sectional view showing a blank mask for extreme ultraviolet lithography according to the present disclosure.
[0057] refer to Figure 1 The blank mask 100 for EUV lithography according to the present disclosure includes a transparent substrate 102, and a reflective film 104, a cover film 106, and an absorption film 108 sequentially stacked on the transparent substrate 102. In addition, the blank mask 100 includes a conductive film 110 disposed on the rear surface of the transparent substrate 102.
[0058] The transparent substrate 102 is a glass substrate for a reflective blank mask using EUV exposure light of 13.5 nm, and preferably uses a substrate having a wavelength within 0±1.0×10 -7 / ℃(and preferably within 0±0.3×10 -7 The transparent substrate 102 may be made of a low thermal expansion material (LTEM) substrate having a low thermal expansion coefficient in the range of 100 Å / °C to prevent the pattern from being deformed due to heat and stress caused by the film during exposure. For this purpose, the transparent substrate 102 may be made of, for example, SiO 2 -TiO 2 Made of glass-like, multi-component glass-ceramic or similar materials.
[0059] The transparent substrate 102 needs to have high flatness in order to increase the accuracy of reflected light during exposure. The flatness is expressed as a total indicated reading (TIR) value, and the TIR of the transparent substrate 102 is 100 nm or less, preferably 50 nm or less, and more preferably 30 nm or less in an area of 132 mm2 or 142 mm2.
[0060] The reflective film 104 disposed on the transparent substrate 102 has a function of reflecting EUV exposure light, and is formed by alternately stacking 40 to 60 layers of molybdenum (Mo) and silicon (Si). The reflective film 104 requires a high reflectivity relative to a wavelength of 13.5 nanometers in order to improve image contrast. The reflection intensity of the reflective film 104 depends on the incident angle of the exposure light and the structure (thickness of each layer) of the reflective film 104 and changes. For example, when a common NA method of 0.33 is applied and the incident angle of the exposure light is 4° to 6°, it is preferred that the molybdenum (Mo) layer and the silicon (Si) layer have a thickness of 2.8 nanometers and 4.2 nanometers, respectively, and when a high NA method with an incident angle of 8° to 14° is applied, it is preferred that the molybdenum (Mo) layer and the silicon (Si) layer have a thickness of 2 nanometers to 4 nanometers and 3 nanometers to 5 nanometers, respectively.
[0061] In order to reduce diffusion between the corresponding layers when forming the molybdenum (Mo) layer and the silicon (Si) layer and to reduce the reduction of reflectivity caused by the heat treatment process during the manufacturing process, after the molybdenum (Mo) layer is formed, the reflective film 104 may be made of a material selected from B 4 At least one material of Mo / B or carbon (C) is made into a thickness of 0.1 nm to 5 nm, and preferably made into a thickness of 0.1 nm to 1 nm. In this way, in detail, the reflective film can be Mo / B 4 C / Si / C / Mo structure or Mo / C / Si / B 4 C / Mo structure is formed. However, when B 4When the thickness of C or carbon is 5 nm or more, the reflectivity of the reflective film 104 decreases, and when B 4 When the thickness of C or carbon is 0.1 nm or less, it is difficult to reduce diffusion between Mo / Si layers or reduction in reflectivity due to thermal change.
[0062] The reflective film 104 may be selectively heat-treated. The heat treatment may be performed by at least one method selected from a furnace in the range of 200° C. to 500° C., rapid thermal annealing (RTA), and a hot plate. The heat treatment is preferably performed in the temperature range of 250° C. to 300° C. to reduce the stress of the reflective film 104. On the other hand, when the reflective film 104 is formed, B4C or C may be formed to suppress the influence of reducing the reflectivity due to diffusion caused during the heat treatment.
[0063] Since the reflective film 104 is easily oxidized when molybdenum (Mo) comes into contact with the atmosphere and thus the reflectivity is reduced, the uppermost layer of the reflective film 104 is preferably formed with a silicon (Si) layer as a protective film that does not oxidize. On the other hand, even if the uppermost layer is formed with a silicon (Si) layer, an oxide film is formed on the silicon (Si) layer by high energy during repeated exposure to a wafer after manufacturing a mask, which affects the upper film or the lower film. Therefore, it is preferred to perform electrical neutralization treatment such as electronic surface treatment after the reflective film 104 is formed. In this way, surface electrons can be controlled to prevent changes in the film, such as oxidation.
[0064] The reflective film 104 has a reflectivity of 65% or more with respect to an EUV exposure wavelength of 13.5 nanometers, and a reflectivity of 65% or less with respect to a wavelength of 193 nanometers or 257 nanometers. When the surface flatness of the reflective film 104 is defined by TIR, the surface flatness has an absolute value of 1,000 nanometers or less, preferably 500 nanometers or less, and more preferably 300 nanometers or less. When the surface flatness of the reflective film 104 is poor, an error occurs in a position where EUV exposure light is reflected, and as the position error becomes higher, a position error of a critical dimension occurs. On the other hand, the reflective film 104 has a surface roughness of 0.5 nanometer Ra or less, preferably 0.3 nanometer Ra or less, and more preferably 0.1 nanometer Ra or less, so as to suppress diffuse reflection of EUV exposure light.
[0065] At the same time, despite Figure 1Although not shown in the figure, a stress control layer may be additionally formed between the transparent substrate 102 and the reflective film 104. The stress control layer may be made of a material having a concave shape. Examples of the material may include at least one material selected from the following: Cr, Ta, B, Mo, V, Co, Ag, Sb, Ti, I, Pb, Ga, Bi, Co, Sn, Te, Ni, Zr, Si, Nb, Pt, Pd, Zn, Al, Mn, Cd, Mg, Li, Se, Cu, Hf, and W, or in addition include at least one material selected from oxygen, nitrogen, carbon, boron, and hydrogen, and may preferably include a material selected from Cr, Mo, Ti, Si, and compounds thereof.
[0066] By setting the stress of the stress control layer in the following manner, the residual stress can be controlled to reduce the flatness. For example, when the reflective film 104 has a convex thickness of 800 nanometers, the transparent substrate 102 has a convex thickness of 30 nanometers, and the back conductive film 110 has a concave thickness of 200 nanometers, the stress control layer can be designed to have a concave range of 100 nanometers to 600 nanometers. In addition, when the reflective film 104 has a convex thickness of 800 nanometers, the transparent substrate 102 has a convex thickness of 30 nanometers, and the back conductive film 110 has a concave thickness of 100 nanometers, the stress control layer can be designed to have a concave range of 200 nanometers to 700 nanometers.
[0067] The thickness of the stress control layer is preferably 10 nm to 100 nm. When the stress control layer is made of a chromium-containing material, the stress control layer preferably has a range of Cr:N=100:0 to 35:65.
[0068] The stress control layer may be heat treated. The stress control layer may be heat treated by at least one method selected from a furnace in the range of 10°C to 500°C, rapid thermal annealing (RTA), and a hot plate. The heat treatment is preferably performed in the range of 250°C to 400°C.
[0069] The cover film 106 is formed on the reflective film 104 and serves to protect the reflective film 104 during the dry etching or cleaning process for pattern formation. For this purpose, the cover film 106 may be made of only ruthenium (Ru) or niobium (Nb), a ruthenium (Ru) compound or a niobium (Nb) compound, or a compound containing both ruthenium (Ru) and niobium (Nb). Specifically, the cover film 106 may be made of a material in which at least one light element material among oxygen (O), nitrogen (N) and carbon (C) is contained in ruthenium (Ru) and / or niobium (Nb). In this case, it is preferred that ruthenium () or niobium (Nb) as a main element is formed to have a content of 60 atomic % or more.
[0070] The cover film 106 has a thickness of 1 nm to 10 nm, and preferably has a thickness of 1 nm to 5 nm. When the thickness of the cover film 106 is 1 nm or less, it is difficult to protect the reflective film 104 in the etching and cleaning processes, and when the thickness is 10 nm or more, the reflectivity of the 13.5 nm exposure light is attenuated, thereby causing a problem of reducing image contrast.
[0071] The cover film 106 exhibits relatively weak characteristics to the cleaning solution (especially to ozone water and hot DI water) during the cleaning process. Therefore, in order to prevent the oxide film from being formed on the cover film 106, a process of suppressing the formation of the oxide film on the surface of the cover film 106 by electrical neutralization treatment (e.g., electron beam treatment) may be added.
[0072] The absorption film 108 may be formed by various methods, such as sputtering, chemical vapor deposition (CVD), atomic layer deposition (ALD), and ion beam deposition (IBD). Specifically, the absorption film 108 may be formed by at least one of sputtering and ion beam deposition (IBD).
[0073] The absorption film contains, for example, at least one selected from the group consisting of Cr, Ta, B, Mo, V, Co, Ag, Sb, I, Pb, Ga, Bi, Co, Sn, Te, Ni, Zr, Si, Nb, Pt, Pd, Zn, Al, Mn, Cd, Mg, Li, Se, Cu, Hf, and W, or preferably further contains at least one light element material of oxygen (O), nitrogen (N), carbon (C), boron (B), and hydrogen (H). Specifically, the absorption film 108 is preferably made of tantalum (Ta) and a compound thereof having a high extinction coefficient for exposure light.
[0074] The absorption film 108 may be formed in one or more of a single-layer structure, a multi-layer structure, a single-layer film structure, or a continuous film structure. The absorption film 108 is preferably formed in two or more layers, and more preferably in three or more layers, and the upper layer is formed to contain oxygen (O). Specifically, when the absorption film is formed in two layers, the upper layer contains a material in which at least oxygen (O) is contained in tantalum (Ta), and the lower layer is formed to not contain oxygen (O). For example, the lower layer is made of at least one material not containing oxygen (O) selected from Ta, TaN, TaCN, TaC, TaB, TaBN, and TaBC, or a material further containing a material in which hydrogen (H) is further contained in the at least one material.
[0075] On the other hand, the lower layer is preferably formed in the form of a continuous film in which the composition ratio varies in the thickness direction. Specifically, the lower layer can be formed as a continuous film in which the nitrogen (N) content gradually decreases from the surface in the depth direction. In this way, the etching rate increases in the depth direction, and thus, phenomena such as footing can be solved. On the other hand, since an over-etching method can be applied as another method for solving footing, but may cause damage to the cover film 106, it is more preferable to gradually increase the etching rate in the depth direction.
[0076] Meanwhile, when the absorption film 108 is formed in three layers, each layer of the absorption film may be formed in the form of a single-layer film other than the continuous film form as described above. For example, the intermediate layer may be formed to have a nitrogen (N) content higher than that of the lower layer. Specifically, the nitrogen content in the intermediate layer may be designed to be 1 atomic % or more than 1 atomic % greater than the nitrogen content of the lower layer, and preferably 3 atomic % or more than 3 atomic %. At this time, the difference between the nitrogen content in the intermediate layer and the nitrogen content in the lower layer is preferably 20 atomic % or less. When nitrogen is contained in tantalum (Ta), the higher the nitrogen (N) content, the lower the etching rate of the chlorine (Cl)-based gas, and therefore, when the difference in nitrogen (N) content is 20 atomic % or more, a problem of pattern profile degradation due to a large difference in etching rate occurs. In addition, when the difference is 1 atomic % or less than 1 atomic %, there is no difference in etching rate, and thus the footing is not effectively improved.
[0077] On the other hand, a bias may occur between the resist CD and the absorption film pattern CD formed by the absorption film etching process. As the etching rate increases, there is a problem that the CD changes due to side etching even if the pattern of the absorption film 108 is etched by dry etching. Therefore, in order to reduce the CD bias caused by side etching, it is preferable to etch the intermediate layer at a low etching rate. For this purpose, a method of designing the nitrogen (N) content in the intermediate layer to be relatively higher than the nitrogen (N) content of the lower layer or designing the nitrogen (N) content in the intermediate layer to be lower but designing the thickness of the intermediate layer to be thicker or the like can be used.
[0078] On the other hand, side etching is affected not only by the etching rate but also by the thickness of the intermediate layer. When the thickness of the intermediate layer is 3 nanometers or less, it is difficult to correct CD by side etching, and when the thickness of the intermediate layer is 40 nanometers or more, it is difficult to improve the footing due to the limitation of the thickness of the lower layer with a faster etching rate. Therefore, it is preferred that the thickness of the intermediate layer is 3 nanometers to 40 nanometers or less than 40 nanometers.
[0079] When the absorption film 108 is formed in two layers or three layers, the lower layer is preferably formed to have a composition ratio of Ta:N=95 atomic %:5 atomic % to 50 atomic %:50 atomic %. On the other hand, when the absorption film 108 is formed to contain boron (B), the absorption film 108 is preferably formed to have a composition ratio in which Ta is 40 atomic % to 90 atomic %, B is 5 atomic % to 20 atomic % and N is 5 atomic % to 50 atomic %.
[0080] On the other hand, the upper layer of the absorption film 108 is formed to contain oxygen (O). When the oxygen (O) content in the upper layer is low, the etching rate of the fluorine (F)-based gas decreases, and thus the etching time of the entire absorption film 108 is significantly increased. Therefore, it is preferred that the oxygen content contained in the TaON layer and the TaBON layer (which is the upper layer) is 50 atomic % to 90 atomic %.
[0081] In addition, the upper layer of the absorption film 108 is formed to have a thickness of 1 nm to 10 nm.
[0082] Although not shown, a hard mask film may be formed on the absorption film 108. The hard mask film is made of a material having a high etching selectivity to the absorption film 108 thereunder (particularly to the upper layer of the absorption film 108). Specifically, the hard mask film may be made of chromium (Cr) and a chromium (Cr) compound, and may be made of a synthetic material containing chromium (Cr). Specifically, the hard mask film may be made of a material containing at least one selected from the group consisting of Cr, Ta, Mo, V, Co, Ag, Sb, I, Pb, Ga, Bi, Co, Sn, Te, Ni, Zr, Si, Nb, Pt, Pd, Zn, Al, Mn, Cd, Mg, Li, Se, Cu, Hf, and W, or further containing at least one selected from the group consisting of oxygen (O), nitrogen (N), carbon (C), boron (B), and hydrogen (H).
[0083] The hard mask film is formed to have a thickness of 2 nm to 15 nm. When the lower layer of the absorption film 108 is etched, the hard mask film is etched and removed.
[0084] The back conductive film 110 disposed under the transparent substrate 102 is a thin film for the electronic clip and affects the flatness of the reflective film 104 thereon. Therefore, it is preferred that the back conductive film 110 is formed in a convex shape. The back conductive film 110 may be formed as a single-layer film or a multi-layer film. It is preferred that the back conductive film 110 has a sheet resistance of 100 ohms / □ or less.
[0085] For this purpose, the back conductive film may be made of a material containing at least one of Cr, Ta, Mo, V, Co, Ag, Sb, I, Pb, Ga, Bi, Co, Sn, Te, Ni, Zr, Si, Nb, Pt, Pd, Zn, Al, Mn, Cd, Mg, Li, Se, Cu, Hf, W, or further containing at least one of oxygen (O), nitrogen (N), carbon (C), boron (B), and hydrogen (H). Specifically, the back conductive film may be made of chromium (Cr), a chromium (Cr) compound, or a compound in which a metal material is contained in chromium (Cr).
[0086] Figure 2 1 is a diagram showing a specific configuration of the back-surface conductive film 110 .
[0087] The back conductive film 110 may be formed of three layers: a first layer 110-1 in contact with the back surface of the substrate 102, a second layer 110-2 formed on the first layer 110-1, and a third layer 110-3 formed on the second layer 110-2. In order to form the back conductive film 110 to have a convex shape, the first layer 110-1 in contact with the back surface of the substrate 102 is formed to contain at least oxygen (O). The second layer 110-2 may contain oxygen (O) and may not contain oxygen (O). When the second layer 110-2 is formed to not contain oxygen (O), the sheet resistance may be reduced. The third layer 110-3 preferably contains oxygen (O) in order to increase the friction with the electrostatic chuck. Specifically, when the back conductive film 110 is formed in three layers, the first layer 110-1 and the third layer 110-3 containing oxygen (O) are preferably formed to have a composition ratio in which chromium (Cr) is 20 atomic % to 70 atomic % and C, O and N are 30 atomic % to 80 atomic % in total, and the second layer is preferably formed to have a composition ratio of Cr:N=70 atomic %:30 atomic % to 20 atomic %:80 atomic %.
[0088] The resist film (not shown) disposed on the absorption film 108 or the hard mask film is composed of a chemically amplified resist for electron beams, and has a thickness of 150 nm or less, preferably 100 nm or less, and more preferably 60 nm or less. In addition, the resist film may be composed of a resist for multi-electron beams, and the resist film for multi-electron beams has an exposure dose of 50 microcoulombs / cm2 or more, and preferably 70 microcoulombs / cm2 or more.
[0089] Although not shown, an anti-charge layer may be selectively formed on the resist film to reduce the charging of electrons during electron beam exposure. The anti-charge layer may be made of, for example, a self-doped water-soluble conductive polymer. The anti-charge layer has the property of being soluble in ultrapure water and has a thickness of 5 to 60 nanometers and preferably 5 to 30 nanometers. By preventing the charging phenomenon of electrons during electron beam exposure using the anti-charge layer, thermal deformation of the resist film can be prevented, and thus high resolution can be implemented.
[0090] In the above, the present disclosure has been specifically described by the embodiments of the present disclosure, but this is only for the purpose of illustrating and explaining the present disclosure, and is not intended to limit the meaning or scope of the present disclosure described in the claims. Therefore, a person of ordinary skill in the technical field of the present disclosure may understand that various modifications and other equivalent embodiments are possible according to the embodiments. Therefore, the actual technical scope of the present disclosure should be defined by the spirit of the attached claims.
Claims
1. A blank mask for extreme ultraviolet lithography, comprising: The reflective film, the cover film and the absorption film are sequentially formed on the transparent substrate. wherein the reflective film has a surface roughness of 0.5 nanometers Ra or less; wherein the absorption film is made of a tantalum compound having a two-layer structure in which an upper layer contains oxygen and a lower layer does not contain oxygen; wherein the lower layer is formed in the form of a continuous film having a composition ratio that varies in the thickness direction; The lower layer is formed as a continuous film in which the nitrogen (N) content gradually decreases from the surface in the thickness direction.
2. The blank mask for extreme ultraviolet lithography according to claim 1, wherein the reflective film is a structure in which one of a molybdenum / silicon structure, a molybdenum / boron carbide / silicon / carbon / molybdenum structure, and a molybdenum / carbon / silicon / boron carbide / molybdenum structure is stacked in multiple layers. 3 . The blank mask for EUV lithography according to claim 2 , wherein at least one of boron carbide or carbon in the reflective film is formed in a layer having a thickness of 0.1 nm to 5 nm. 4 . The blank mask for EUV lithography according to claim 1 , wherein the reflective film is heat-treated at a temperature of 200° C. to 500° C. 5 . The blank mask for EUV lithography according to claim 1 , wherein the reflective film or the cover film is subjected to an electrical neutralization treatment for suppressing formation of an oxide film by electron beam treatment after film formation.
6. The blank mask for extreme ultraviolet lithography according to claim 1, further comprising: The stress control layer is disposed between the transparent substrate and the reflective film and has a concave shape.
7. The blank mask for extreme ultraviolet lithography according to claim 6, wherein the stress control layer is made of a material containing at least one of the following: chromium, tantalum, boron, molybdenum, vanadium, cobalt, silver, antimony, titanium, iodine, lead, gallium, bismuth, cobalt, tin, tellurium, nickel, zirconium, silicon, niobium, platinum, palladium, zinc, aluminum, manganese, cadmium, magnesium, lithium, selenium, copper, hafnium and tungsten, or further contains at least one of oxygen, nitrogen, carbon, boron and hydrogen. 8 . The blank mask for EUV lithography according to claim 6 , wherein the stress control layer has a thickness of 10 nm to 100 nm.
9. The blank mask for extreme ultraviolet lithography according to claim 1, wherein the cover film is made of a material containing at least one of ruthenium or niobium, or further contains at least one light element of oxygen, nitrogen and carbon.
10. The blank mask for extreme ultraviolet lithography according to claim 1, wherein the lower layer is made of a material containing at least one of tantalum, tantalum nitride, tantalum carbonitride, tantalum carbide, tantalum boride, tantalum boronitride and tantalum borocarbide, or further contains hydrogen.
11. The blank mask for EUV lithography according to claim 1, wherein the absorption film is made of a tantalum compound having a three-layer structure. 12 . The blank mask for EUV lithography according to claim 11 , wherein the absorption film is formed such that a nitrogen content in the middle layer is higher than a nitrogen content in the lower layer by 1 at. % to 20 at. %. 13 . The blank mask for EUV lithography according to claim 12 , wherein the intermediate layer of the absorption film has a thickness of 3 nm to 40 nm.
14. The blank mask for extreme ultraviolet lithography according to claim 1, wherein the absorption film has a structure of two or more layers and is made of a tantalum compound, and a layer below an upper layer of the absorption film has a composition ratio of tantalum:nitrogen=95at.%:5at.% to 50at.%:50at.%.
15. The blank mask for EUV lithography according to claim 1, wherein the absorption film is made of a tantalum compound containing boron and has a composition ratio of 40 at.% to 90 at.% tantalum, 5 at.% to 20 at.% boron, and 5 at.% to 50 at.% nitrogen.
16. The blank mask for EUV lithography according to claim 1, wherein the absorption film has a structure of two or more layers and is made of a tantalum compound, and an upper layer of the absorption film is formed to contain 50 at.% to 90 at.% of oxygen.
17. The blank mask for extreme ultraviolet lithography according to claim 1, further comprising: A hard mask film is formed on the absorption film.
18. The blank mask for extreme ultraviolet lithography according to claim 17, wherein the hard mask film is made of a material containing at least one of the following: chromium, tantalum, molybdenum, vanadium, cobalt, silver, antimony, iodine, lead, gallium, bismuth, cobalt, tin, tellurium, nickel, zirconium, silicon, niobium, platinum, palladium, zinc, aluminum, manganese, cadmium, magnesium, lithium, selenium, copper, hafnium and tungsten, or further contains at least one selected from oxygen, nitrogen, carbon, boron and hydrogen.
19. The blank mask for extreme ultraviolet lithography according to claim 1, further comprising: The back conductive film is arranged under the transparent substrate. 20 . The blank mask for EUV lithography according to claim 19 , wherein the back surface conductive film has a sheet resistance of 100 Ω / □ or less.
21. The blank mask for extreme ultraviolet lithography according to claim 19, wherein the back conductive film is made of a material containing at least one of the following: chromium, tantalum, molybdenum, vanadium, cobalt, silver, antimony, iodine, lead, gallium, bismuth, cobalt, tin, tellurium, nickel, zirconium, silicon, niobium, platinum, palladium, zinc, aluminum, manganese, cadmium, magnesium, lithium, selenium, copper, hafnium and tungsten, or further contains at least one of oxygen, nitrogen, carbon, boron and hydrogen.
22. A blank mask for extreme ultraviolet lithography according to claim 19, wherein the back conductive film is made of chromium, a chromium compound or a compound in which a metal material is contained in chromium, and the back conductive film has a three-layer structure, wherein a first layer is in contact with the rear surface of the transparent substrate, a second layer is formed on the first layer, and a third layer is formed on the second layer, and the first layer and the third layer contain oxygen, and the second layer does not contain oxygen.
23. The blank mask for extreme ultraviolet lithography according to claim 22, wherein the first layer and the third layer have a composition ratio in which chromium is 20 at.% to 70 at.% and carbon, oxygen and nitrogen are 30 at.% to 80 at.% in total, and the second layer has a composition ratio of chromium:nitrogen=70 at.%:30 at.% to 20 at.%:80 at.%.
24. A photomask for extreme ultraviolet lithography, manufactured using the blank mask for extreme ultraviolet lithography according to any one of claims 1 to 23.