A highly sensitive and highly selective triethylamine gas-sensitive material and a preparation method thereof
By loading Pt nanoparticles with less than 2nm on the porous ZnO nanobelt, combined with the chloroplatinic acid reduction and calcination steps, a highly sensitive and highly selective triethylamine gas-sensitive material was prepared, which solved the low sensitivity and poor selectivity of existing sensors. The problem of this achieves efficient detection of triethylamine.
Patent Information
- Application Number
- CN202110155880.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-23
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-04-23
AI Technical Summary
The existing triethylamine gas-sensitive sensors have low sensitivity and poor selectivity, making it difficult to achieve high sensitivity and high selectivity detection. The loading of precious metal nanoparticles is prone to fall off on the surface of oxide nano-sensitive materials, affecting the stability of gas-sensitive performance.
Highly sensitive and highly selective triethylamine gas-sensitive materials are prepared by loading Pt nanoparticles with particle size less than 2nm on the porous ZnO nanobelt, and chloroplatinic acid reduction and calcining steps, using Pt nanoparticles and porous ZnO nanoparticles. The synergistic sensitization mechanism of the structure achieves high selective identification of triethylamine.
The sensitivity and selectivity of triethylamine gas-sensitive sensors are significantly improved. The small size and uniform distribution of Pt nanoparticles ensure high purity and stability, solving the problem of poor sensor selectivity.
Smart Images

Figure CN112964759B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nanomaterials, and in particular to a highly sensitive and highly selective triethylamine gas-sensitive material and a preparation method thereof. Background Art
[0002] Triethylamine, as a highly volatile organic compound, is flammable and explosive, which can easily cause harm to people's lives. Long-term exposure to triethylamine can cause headaches, pulmonary edema, gastroenteritis and other health problems. In addition, studies have shown that species such as fish and shellfish can release triethylamine, and its concentration gradually increases as the freshness of the fish decreases. Therefore, triethylamine can be used as a marker for monitoring the freshness of fish. Although many researchers have reported on triethylamine detection over the years, there are still some problems such as low sensitivity and poor selectivity that limit their application. Semiconductor-based metal oxide gas sensors have been widely studied around the world due to their high gas response, good portability and low manufacturing cost.
[0003] Among the numerous semiconductor gas sensors, ZnO, as a typical n-type semiconductor, has unique properties required for an ideal gas sensor, such as a wide band gap of 3.37 eV, a large exciton binding energy of 60 meV, high electron mobility, photoelectric response, and thermal stability. At the same time, ZnO has the advantages of low cost, non-toxicity, easy preparation, and suitability for mass production. In addition, ZnO is a typical sensitive material, and its conductivity mainly depends on the electron concentration in the sensitive material. When ZnO is exposed to air, oxygen molecules are adsorbed on the surface of ZnO and obtain certain electrons from the sensitive material to form highly active oxygen anions, thereby forming an electron depletion layer in the sensitive material accompanied by an increase in resistance. When reducing gas is added, oxygen anions interact with these gas molecules and release the captured electrons back to the sensitive material, resulting in a decrease in the sensor resistance. Therefore, the change in sensor resistance realizes gas sensing detection. However, the inherent cross-sensitivity of gas-sensitive materials has always been a difficulty faced by the research of gas sensors.
[0004] Loading catalytically active precious metal nanoparticles has become one of the effective means to improve the gas sensing performance of semiconductor oxides. It can catalytically reduce the reaction energy barrier of triethylamine on the surface of oxide nanosensitive materials and enhance its sensitivity. Based on the synergistic sensitization mechanism of precious metal nanoparticles and porous nanostructures, it is possible to achieve selective recognition of triethylamine. Conventional precious metal nanoparticle loading mostly adopts post-chemical modification method, which makes it easy to fall off from the surface of oxide nanosensitive materials, and the particle size and loading coverage are difficult to control, affecting the stability of gas sensing performance. Therefore, it is difficult to construct stable, highly sensitive and highly selective nanosensor devices and develop new detection methods to achieve highly sensitive and highly selective detection of triethylamine. Summary of the invention
[0005] Based on the technical problems existing in the background technology, the present invention proposes a highly sensitive and highly selective triethylamine gas-sensitive material and a preparation method thereof. The gas-sensitive material achieves highly selective and highly sensitive detection of triethylamine by loading extremely small-sized Pt nanoparticles on porous ZnO nanobelts.
[0006] The invention provides a highly sensitive and highly selective triethylamine gas-sensitive material, which comprises Pt nanoparticles with a particle size less than 2nm and a porous ZnO nanobelt with the Pt nanoparticles uniformly loaded on the surface.
[0007] Preferably, the loading amount of the Pt nanoparticles is 0.5-3% of the molar amount of the porous ZnO nanobelts, preferably 1%.
[0008] The invention also provides a method for preparing a triethylamine gas-sensitive material with high sensitivity and high selectivity, which comprises: subjecting chloroplatinic acid to a reduction reaction on the surface of a ZnSe·0.5N2H4 nanobelt, and then calcining the reaction to obtain the triethylamine gas-sensitive material with high sensitivity and high selectivity.
[0009] Preferably, the molar ratio of chloroplatinic acid to ZnSe·0.5N2H4 nanobelt is 0.005-0.03:1, preferably 0.01:1.
[0010] Preferably, the reduction reaction is carried out at a temperature of 10-60°C and a time of 60-180 min.
[0011] Preferably, the calcination is carried out in air at a temperature of 450-550° C. and a time of 5-30 min.
[0012] Preferably, the preparation method of the gas-sensitive material comprises: adding an aqueous solution of chloroplatinic acid to an ethanol solution of ZnSe·0.5N2H4 nanobelts, stirring and mixing, reacting at 10-60°C for 60-180 minutes, filtering, and calcining the resulting product in an air atmosphere at 450-550°C for 5-30 minutes to obtain the highly sensitive and highly selective triethylamine gas-sensitive material.
[0013] The present invention also provides a gas sensor, which comprises the above-mentioned gas-sensitive material or the gas-sensitive material prepared by the above-mentioned preparation method.
[0014] Preferably, the gas sensor is used for detecting triethylamine.
[0015] Preferably, the detection lower limit of the gas sensor for triethylamine is 1 ppm.
[0016] The invention provides a highly sensitive and highly selective triethylamine gas-sensitive material, comprising Pt nanoparticles with a particle size of less than 2 nm and a porous ZnO nanobelt with the Pt nanoparticles uniformly loaded on the surface. In the gas-sensitive material, since the Pt nanoparticles and the porous ZnO nanostructure have synergistic sensitization characteristics and the Pt particles are less than 2 nm, the catalytic performance is excellent, which is the main reason for achieving selective recognition of triethylamine.
[0017] The invention also provides a preparation method of a highly sensitive and highly selective triethylamine gas-sensitive material. The preparation method adopts a ZnSe·0.5N2H4 nanobelt as a precursor and uses ethanol as a solvent to disperse the ZnSe·0.5N2H4 well. When chloroplatinic acid is added to the ZnSe·0.5N2H4 precursor solution, since hydrazine hydrate is evenly distributed in ZnSe and has a strong reducing effect, when the chloroplatinic acid is reduced by the hydrazine hydrate, the evenly dispersed reducing agent enables the reduction product Pt to be evenly distributed and reach an extremely small size. At the same time, the Pt nanoparticles obtained after calcination are loaded on the porous ZnO and are not easy to fall off. The prepared Pt-modified porous ZnO nanobelt has high purity, does not contain other morphological features, and has a relatively even pore size distribution, so the sensitivity of the sensor is greatly improved.
[0018] In fact, it is found through testing that the triethylamine gas-sensitive material of the present invention has significantly improved the sensitivity and selectivity of the gas sensor compared to ZnO, and the synergistic sensitization mechanism of the noble metal nanoparticles and the porous nanostructure achieves high sensitivity and high selectivity detection of triethylamine. In addition, the present invention also controls the size and distribution density of Pt nanoparticles by controlling the amount of chloroplatinic acid added, and finally effectively solves the problem of poor selectivity of the gas sensor for triethylamine. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 Scanning electron microscope images of the gas-sensitive material of the present invention: (a), (b), (c), (d), (e), and (f) are scanning electron microscope images of Pt-loaded porous ZnO nanobelts with an amount of 0.5 at%, 1 at%, 1.5 at%, 2 at%, 3 at%, and 5 at%, respectively.
[0020] Figure 2 Transmission electron microscope images of the gas-sensitive material of the present invention: (a) is a transmission electron microscope image of the gas-sensitive material obtained in Example 1; (b) is a structural diagram of a single nanorod of the gas-sensitive material obtained in Example 1, and the inset is the HRTEM of Figure (b); (c) is a mapping image of a single nanorod in Figure (b); (d) is an X-ray single crystal powder diffraction image of the gas-sensitive material obtained in Example 7.
[0021] Figure 3The results of the sensitivity test of the gas-sensitive material of the present invention to triethylamine when used in a gas sensor are shown in the figure: (a) is a sensitivity response test graph of the gas-sensitive material obtained in Examples 1-4 and the ZnO nanobelt to 25 ppm triethylamine; (b) is a bar graph of the sensitivity response of the gas-sensitive material and the ZnO nanobelt obtained in Example 1 to 25 ppm triethylamine, methanol, ethanol, isopropanol, acetone, benzene, toluene and formaldehyde, respectively;
[0022] Figure 4 This is a test result diagram of the sensitivity response of the gas-sensitive material obtained in Example 1 of the present invention to triethylamine of different concentrations when used in a gas sensor;
[0023] Figure 5 This is a bar graph showing the sensitivity responses of the gas-sensitive material obtained in Example 1 of the present invention and the Au / ZnO nanobelt obtained in Comparative Example 2 to 100 ppm triethylamine. DETAILED DESCRIPTION
[0024] The technical solutions of the present invention are described in detail below through specific embodiments. However, it should be clearly stated that these embodiments are for illustration only and are not to be construed as limiting the scope of the present invention.
[0025] Example 1
[0026] A highly sensitive and highly selective triethylamine gas-sensitive material, the preparation method of which comprises the following steps:
[0027] (1) A 0.01 mol / L zinc chloride aqueous solution (0.2 mmol ZnCl2 dissolved in 20 mL ultrapure water) was added dropwise to a 0.02 mol / L selenium powder solution (0.4 mmol Se powder dissolved in 20 mL 80 wt% hydrazine hydrate solution), and the mixture was stirred for 1 h, and then hydrothermally reacted at 180°C for 12 h. After the reaction, the precipitate was centrifuged and washed 4 times with hydrazine hydrate to remove excess selenium powder, and then the precipitate was centrifuged and washed with water until neutral, and finally the precipitate was washed twice with ethanol to remove water, thereby obtaining a white ZnSe·0.5N2H4 nanobelt precursor;
[0028] (2) 0.2 mmol ZnSe·0.5N2H4 nanobelts were dissolved in 90 mL ethanol solution, stirred for 10 min, and then slowly added into 200 μL 10 mmol / L H2PtCl6 chloroplatinic acid solution. After stirring at room temperature for 120 min, the mixture was washed with water and ethanol for 5 times, and dried to obtain 1 at% Pt-loaded ZnSe·0.5N2H4 nanobelts.
[0029] (3) The Pt-loaded ZnSe·0.5N2H4 nanobelts were calcined in air at 500°C for 10 min and cooled to room temperature to obtain 1at% Pt-loaded porous ZnO nanobelts, namely the gas-sensitive material (1at% Pt / ZnO).
[0030] The gas-sensitive material prepared in Example 1 was tested by scanning electron microscopy, and the results were as follows: Figure 1 (b) As shown in the figure, due to the small size of Pt nanoparticles, the presence of Pt cannot be observed under a scanning electron microscope, but it can be seen that the morphology of the Pt-loaded porous ZnO nanobelts is a rough porous structure.
[0031] The gas-sensitive material prepared in Example 1 was analyzed by transmission electron microscopy, and the results are as follows: Figure 2 Shown by: Figure 2 (b) It can be seen that the maximum size of Pt particles is 2 nm, and the inset shows that the lattice spacing of Pt and ZnO is 0.19 nm and 0.23 nm, respectively, which matches the Pt (200) crystal plane and the ZnO (101) crystal plane; Figure 2 (c) Figure 2 (b) Mapping diagram, from the Pt element distribution diagram, it can be seen that the Pt particles are small and the distribution is dense, but the Pt particles are small and many particles cannot be observed under HRTEM.
[0032] Example 2
[0033] A highly sensitive and highly selective triethylamine gas-sensitive material, the preparation method of which comprises the following steps:
[0034] (1) A 0.01 mol / L zinc chloride aqueous solution (0.2 mmol ZnCl2 dissolved in 20 mL ultrapure water) was added dropwise to a 0.02 mol / L selenium powder solution (0.4 mmol Se powder dissolved in 20 mL 80 wt% hydrazine hydrate solution), and the mixture was stirred for 1 h, and then hydrothermally reacted at 180°C for 12 h. After the reaction, the precipitate was centrifuged and washed 4 times with hydrazine hydrate to remove excess selenium powder, and then the precipitate was centrifuged and washed with water until neutral, and finally the precipitate was washed twice with ethanol to remove water, thereby obtaining a white ZnSe·0.5N2H4 nanobelt precursor;
[0035] (2) 0.2 mmol ZnSe·0.5N2H4 nanobelts were dissolved in 90 mL ethanol solution, stirred for 10 min, and then slowly added into 100 μL 10 mmol / L H2PtCl6 chloroplatinic acid solution. After stirring at room temperature for 60 min, the mixture was washed with water and ethanol for 5 times to obtain 0.5 at% Pt-loaded ZnSe·0.5N2H4 nanobelts.
[0036] (3) The Pt-loaded ZnSe·0.5N2H4 nanobelts were calcined in air at 500°C for 10 min and cooled to room temperature to obtain 0.5 at% Pt-loaded porous ZnO nanobelts, namely the gas-sensitive material (0.5 at% Pt / ZnO).
[0037] The gas-sensitive material prepared in Example 2 was tested by scanning electron microscopy, and the results were as follows: Figure 1 (a) As shown in the figure, due to the small size of Pt nanoparticles, the presence of Pt cannot be observed under a scanning electron microscope, but it can be seen that the morphology of Pt-loaded porous ZnO nanobelts is a rough porous structure.
[0038] Example 3
[0039] A highly sensitive and highly selective triethylamine gas-sensitive material, the preparation method of which comprises the following steps:
[0040] (1) A 0.01 mol / L zinc chloride aqueous solution (0.2 mmol ZnCl2 dissolved in 20 mL ultrapure water) was added dropwise to a 0.02 mol / L selenium powder solution (0.4 mmol Se powder dissolved in 20 mL 80 wt% hydrazine hydrate solution), and the mixture was stirred for 1 h, and then hydrothermally reacted at 180°C for 12 h. After the reaction, the precipitate was centrifuged and washed 4 times with hydrazine hydrate to remove excess selenium powder, and then the precipitate was centrifuged and washed with water until neutral, and finally the precipitate was washed twice with ethanol to remove water, thereby obtaining a white ZnSe·0.5N2H4 nanobelt precursor;
[0041] (2) 0.2 mmol ZnSe·0.5N2H4 nanobelts were dissolved in 90 mL ethanol solution, stirred for 10 min, and then slowly added into 300 μL 10 mmol / L H2PtCl6 chloroplatinic acid solution. After stirring at room temperature for 150 min, the mixture was washed with water and ethanol for 5 times to obtain 1.5 at% Pt-loaded ZnSe·0.5N2H4 nanobelts.
[0042] (3) The Pt-loaded ZnSe·0.5N2H4 nanobelts were calcined in air at 500°C for 15 min and cooled to room temperature to obtain 1.5 at% Pt-loaded porous ZnO nanobelts, i.e., the gas-sensitive material (1.5 at% Pt / ZnO).
[0043] The gas-sensitive material prepared in Example 3 was tested by scanning electron microscopy, and the results were as follows: Figure 1 (c) As shown in the figure, due to the small size of Pt nanoparticles, the presence of Pt cannot be observed under a scanning electron microscope, but it can be seen that the morphology of the Pt-loaded porous ZnO nanobelts is a rough porous structure.
[0044] Example 4
[0045] A highly sensitive and highly selective triethylamine gas-sensitive material, the preparation method of which comprises the following steps:
[0046] (1) A 0.01 mol / L zinc chloride aqueous solution (0.2 mmol ZnCl2 dissolved in 20 mL ultrapure water) was added dropwise to a 0.02 mol / L selenium powder solution (0.4 mmol Se powder dissolved in 20 mL 80 wt% hydrazine hydrate solution), and the mixture was stirred for 1 h, and then hydrothermally reacted at 180°C for 12 h. After the reaction, the precipitate was centrifuged and washed 4 times with hydrazine hydrate to remove excess selenium powder, and then the precipitate was centrifuged and washed with water until neutral, and finally the precipitate was washed twice with ethanol to remove water, thereby obtaining a white ZnSe·0.5N2H4 nanobelt precursor;
[0047] (2) 0.2 mmol ZnSe·0.5N2H4 nanobelts were dissolved in 90 mL ethanol solution, stirred for 10 min, and then slowly added into 400 μL 10 mmol / L H2PtCl6 chloroplatinic acid solution. After stirring at room temperature for 150 min, the mixture was washed with water and ethanol for 5 times to obtain 2 at% Pt-loaded ZnSe·0.5N2H4 nanobelts.
[0048] (3) The Pt-loaded ZnSe·0.5N2H4 nanobelts were calcined in air at 500°C for 15 min and cooled to room temperature to obtain 2at% Pt-loaded porous ZnO nanobelts, namely the gas-sensitive material (2at% Pt / ZnO).
[0049] The gas-sensitive material prepared in Example 4 was tested by scanning electron microscopy, and the results were as follows: Figure 1 (d) As shown in the figure, due to the small size of Pt nanoparticles, the presence of Pt cannot be observed under a scanning electron microscope, but it can be seen that the morphology of the Pt-loaded porous ZnO nanobelts is a rough porous structure.
[0050] Example 5
[0051] A highly sensitive and highly selective triethylamine gas-sensitive material, the preparation method of which comprises the following steps:
[0052] (1) A 0.01 mol / L zinc chloride aqueous solution (0.2 mmol ZnCl2 dissolved in 20 mL ultrapure water) was added dropwise to a 0.02 mol / L selenium powder solution (0.4 mmol Se powder dissolved in 20 mL 80 wt% hydrazine hydrate solution), and the mixture was stirred for 1 h, and then hydrothermally reacted at 180°C for 12 h. After the reaction, the precipitate was centrifuged and washed 4 times with hydrazine hydrate to remove excess selenium powder, and then the precipitate was centrifuged and washed with water until neutral, and finally the precipitate was washed twice with ethanol to remove water, thereby obtaining a white ZnSe·0.5N2H4 nanobelt precursor;
[0053] (2) 0.2 mmol ZnSe·0.5N2H4 nanobelts were dissolved in 90 mL ethanol solution, stirred for 10 min, and then slowly added into 600 μL 10 mmol / L H2PtCl6 chloroplatinic acid solution. After stirring at room temperature for 180 min, the mixture was washed with water and ethanol for 5 times to obtain 3 at% Pt-loaded ZnSe·0.5N2H4 nanobelts.
[0054] (3) The Pt-loaded ZnSe·0.5N2H4 nanobelts were calcined in air at 500°C for 20 min and cooled to room temperature to obtain 3at% Pt-loaded porous ZnO nanobelts, namely the gas-sensitive material (3at% Pt / ZnO).
[0055] The gas-sensitive material prepared in Example 5 was tested by scanning electron microscopy, and the results were as follows: Figure 1 (e) As shown in the figure, due to the small size of Pt nanoparticles, the presence of Pt cannot be observed under a scanning electron microscope, but it can be seen that part of the structure of the Pt-loaded porous ZnO nanobelts has collapsed.
[0056] Example 6
[0057] A highly sensitive and highly selective triethylamine gas-sensitive material, the preparation method of which comprises the following steps:
[0058] (1) A 0.01 mol / L zinc chloride aqueous solution (0.2 mmol ZnCl2 dissolved in 20 mL ultrapure water) was added dropwise to a 0.02 mol / L selenium powder solution (0.4 mmol Se powder dissolved in 20 mL 80 wt% hydrazine hydrate solution), and the mixture was stirred for 1 h, and then hydrothermally reacted at 180°C for 12 h. After the reaction, the precipitate was centrifuged and washed 4 times with hydrazine hydrate to remove excess selenium powder, and then the precipitate was centrifuged and washed with water until neutral, and finally the precipitate was washed twice with ethanol to remove water, thereby obtaining a white ZnSe·0.5N2H4 nanobelt precursor;
[0059] (2) 0.2 mmol ZnSe·0.5N2H4 nanobelts were dissolved in 90 mL ethanol solution, stirred for 10 min, and then slowly added into 1000 μL 10 mmol / L H2PtCl6 chloroplatinic acid solution. After stirring at room temperature for 180 min, the mixture was washed with water and ethanol for 5 times to obtain 5 at% Pt-loaded ZnSe·0.5N2H4 nanobelts.
[0060] (3) The Pt-loaded ZnSe·0.5N2H4 nanobelts were calcined in air at 500°C for 30 min and cooled to room temperature to obtain 5at% Pt-loaded porous ZnO nanobelts, namely the gas-sensitive material (5at% Pt / ZnO).
[0061] The gas-sensitive material prepared in Example 6 was tested by scanning electron microscopy, and the results were as follows: Figure 1 (f) As shown in the figure, it can be seen that Pt-loaded porous ZnO cannot maintain a band structure.
[0062] Example 7
[0063] A highly sensitive and highly selective triethylamine gas-sensitive material, the preparation method of which comprises the following steps:
[0064] (1) A 0.01 mol / L zinc chloride aqueous solution (0.2 mmol ZnCl2 dissolved in 20 mL ultrapure water) was added dropwise to a 0.02 mol / L selenium powder solution (0.4 mmol Se powder dissolved in 20 mL 80 wt% hydrazine hydrate solution), and the mixture was stirred for 1 h, and then hydrothermally reacted at 180°C for 12 h. After the reaction, the precipitate was centrifuged and washed 4 times with hydrazine hydrate to remove excess selenium powder, and then the precipitate was centrifuged and washed with water until neutral, and finally the precipitate was washed twice with ethanol to remove water, thereby obtaining a white ZnSe·0.5N2H4 nanobelt precursor;
[0065] (2) 0.2 mmol ZnSe·0.5N2H4 nanobelts were dissolved in 90 mL ethanol solution, stirred for 10 min, and then slowly added into 2000 μL 10 mmol / L H2PtCl6 chloroplatinic acid solution. After stirring at room temperature for 180 min, the mixture was washed with water and ethanol for 5 times, and dried to obtain 10 at% Pt-loaded ZnSe·0.5N2H4 nanobelts.
[0066] (3) The Pt-loaded ZnSe·0.5N2H4 nanobelts were calcined in air at 500°C for 30 min and cooled to room temperature to obtain 10 at% Pt-loaded porous ZnO nanobelts, namely the gas-sensitive material (10 at% Pt / ZnO).
[0067] The gas-sensitive material prepared in Example 7 was subjected to X-ray single crystal powder diffraction, and the results are as follows: Figure 2 As shown in (d), the peak of the obtained product coincides with the peaks of ZnO (PDF#36-1451) and Pt (PDF#04-0802), and it can be clearly seen that the obtained product is Pt-loaded porous ZnO nanobelts.
[0068] Comparative Example 1
[0069] A porous ZnO nanobelt, the preparation method of which comprises the following steps:
[0070] (1) A 0.01 mol / L zinc chloride aqueous solution (0.2 mmol ZnCl2 dissolved in 20 mL ultrapure water) was added dropwise to a 0.02 mol / L selenium powder solution (0.4 mmol Se powder dissolved in 20 mL 80 wt% hydrazine hydrate solution), and the mixture was stirred for 1 h, and then hydrothermally reacted at 180°C for 12 h. After the reaction, the precipitate was centrifuged and washed 4 times with hydrazine hydrate to remove excess selenium powder, and then the precipitate was centrifuged and washed with water until neutral, and finally the precipitate was washed twice with ethanol to remove water, thereby obtaining a white ZnSe·0.5N2H4 nanobelt precursor;
[0071] (2) The ZnSe·0.5N2H4 nanobelt is calcined in air at 500°C for 10 min and then cooled to room temperature to obtain the porous ZnO nanobelt.
[0072] Comparative Example 2
[0073] An Au-loaded porous ZnO nanobelt, the preparation method of which comprises the following steps:
[0074] (1) A 0.01 mol / L zinc chloride aqueous solution (0.2 mmol ZnCl2 dissolved in 20 mL ultrapure water) was added dropwise to a 0.02 mol / L selenium powder solution (0.4 mmol Se powder dissolved in 20 mL 80 wt% hydrazine hydrate solution), and the mixture was stirred for 1 h, and then hydrothermally reacted at 180°C for 12 h. After the reaction, the precipitate was centrifuged and washed 4 times with hydrazine hydrate to remove excess selenium powder, and then the precipitate was centrifuged and washed with water until neutral, and finally the precipitate was washed twice with ethanol to remove water, thereby obtaining a white ZnSe·0.5N2H4 nanobelt precursor;
[0075] (2) 0.2 mmol ZnSe·0.5N2H4 nanobelts were dissolved in 90 mL ethanol solution, stirred for 10 min, and then 400 μL HAuCl4 solution with a concentration of 5 mmol / L was slowly added. After stirring at room temperature for 30 min, the nanobelts were washed with water and ethanol for 5 times to obtain 1 at% Au-loaded ZnSe·0.5N2H4 nanobelts.
[0076] (3) The Au-loaded ZnSe·0.5N2H4 nanobelts are calcined in air at 500°C for 10 min and cooled to room temperature to obtain 1at% Au-loaded porous ZnO nanobelts, namely the Au-loaded porous ZnO nanobelts (Au / ZnO nanobelts).
[0077] Performance Test:
[0078] The Pt-loaded ZnSe·0.5N2H4 nanobelts and ZnSe·0.5N2H4 nanobelts obtained in Examples 1-4 and Comparative Example 1 were washed with ethanol and then washed twice with N,N-dimethylformamide, and then dispersed in a mixed solution of N,N-dimethylformamide and chloroform in a volume ratio of 10:7, and uniformly assembled on the surface of a ceramic tube using the Langmuir-Blodgett assembly technique. After the ceramic tube was dried, the assembly was performed again, and the operation steps were performed 10 times. After the last drying, the ceramic tube was calcined in air at a calcination temperature of 500°C for 10 min, to obtain devices of 0.5at%, 1.0at%, 1.5at%, and 2.0at% Pt nanoparticles loaded porous ZnO nanobelts and devices of porous ZnO nanobelts, respectively.
[0079] The device was subjected to a gas-sensitivity test at 250-350°C with triethylamine introduced. The results were as follows: Figure 3 , 4 As shown:
[0080] Figure 3 The results of the sensitivity response test of the gas-sensitive material of the present invention to triethylamine when used in a gas sensor are shown in Figure (a). Figure (b) is a bar graph showing the sensitivity response of the gas-sensitive material obtained in Example 1 to triethylamine, methanol, ethanol, isopropanol, acetone, benzene, toluene and formaldehyde at the optimal working temperature (200°C) when the gas-sensitive material obtained in Example 1 and the ZnO nanomaterial obtained in Comparative Example 1 are used in a gas sensor. Figure 4 The figure is a test result of the sensitivity response of the gas-sensitive material obtained in Example 1 of the present invention to triethylamine of different concentrations at the optimal working temperature (200°C). Figure 3 It can be seen from Figure 4 that the gas-sensitive material of the present invention can achieve high sensitivity and high selectivity detection of triethylamine.
[0081] Furthermore, the present invention assembles the Pt-loaded porous ZnO nanobelt described in Example 1 and the Au-loaded porous ZnO nanobelt described in Comparative Example 2 according to the above method to obtain a device with 1.0 at% of Pt nanoparticles loaded on porous ZnO nanobelts and a device with 1.0 at% of Au nanoparticles loaded on porous ZnO nanobelts, respectively.
[0082] The device was subjected to a gas-sensitivity test at 200°C with triethylamine introduced. The results were as follows: Figure 5 As shown:
[0083] Figure 5 The following is a bar graph showing the sensitivity response of the gas-sensitive material (1 at% Pt / ZnO) obtained in Example 1 and the Au-loaded porous ZnO nanobelt (1 at% Au / ZnO) obtained in Comparative Example 2 to triethylamine at the optimal working temperature (200°C). Figure 5 It can be seen that the Pt-loaded porous ZnO nanobelts in Example 1 have a better response sensitivity to triethylamine than the Au-loaded porous ZnO nanobelts in the comparative example.
[0084] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A gas sensor, characterized in that: It includes triethylamine gas-sensitive material; The triethylamine gas-sensitive material comprises Pt nanoparticles with a particle size less than 2 nm and a porous ZnO nanobelt with the Pt nanoparticles uniformly loaded on the surface; The loading amount of the Pt nanoparticles is 0.5-3% of the molar amount of the porous ZnO nanobelts; The preparation method of the triethylamine gas-sensitive material comprises: performing a reduction reaction of chloroplatinic acid on the surface of a ZnSe∙0.5N2H4 nanobelt, and then calcining the surface to obtain the triethylamine gas-sensitive material; The gas sensor is used for detecting triethylamine.
2. The gas sensor according to claim 1, characterized in that: The loading amount of the Pt nanoparticles is 1% of the molar amount of the porous ZnO nanobelts.
3. The gas sensor according to claim 1, characterized in that: The molar ratio of chloroplatinic acid to ZnSe∙0.5N2H4 nanobelt is 0.005-0.03:
1.
4. The gas sensor according to claim 1, characterized in that: The molar ratio of chloroplatinic acid to ZnSe∙0.5N2H4 nanobelt is 0.01:
1.
5. The gas sensor according to claim 1, characterized in that: The temperature of the reduction reaction is 10-60°C and the time is 60-180min.
6. The gas sensor according to claim 1, characterized in that: The calcination is carried out in air at a temperature of 450-550° C. and a time of 5-30 min.
7. The gas sensor according to claim 1, characterized in that: include: The aqueous solution of chloroplatinic acid is added to the ethanol solution of ZnSe∙0.5N2H4 nanobelts, stirred and mixed, reacted at 10-60°C for 60-180min, filtered, and the obtained product is calcined in air at 450-550°C for 5-30min to obtain the triethylamine gas-sensitive material.
8. The gas sensor according to claim 1, characterized in that: The lower detection limit of the gas sensor for triethylamine is 1 ppm.