Graphene battery negative electrode material layer and preparation method thereof, lithium ion battery

By using graphene and nanometal alloy composite material layer and doped gallium nitride-based film in lithium-ion batteries, combined with the filling of sulfonated elastomer and lithium titanate, the lithium storage capacity of traditional lithium-ion batteries is solved. The problems of low and poor circulation performance achieve efficient lithium ion transmission and structural stability, and improve the energy density and service life of the battery.

CN113036107BActive Publication Date: 2024-12-03SHENZHEN POLYTECHNIC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110261667.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-10
Publication Date
2024-12-03
Estimated Expiration
2041-03-10

AI Technical Summary

Technical Problem

During the charging and discharging process, traditional lithium-ion batteries have problems such as low lithium storage, low lithium-ion transmission efficiency and poor circulation performance, especially structural collapse and corrosion caused by gas production expansion and electrolyte erosion.

Method used

Using graphene battery negative electrode material layer, including composite material layer composed of nanometal alloys and graphene, as well as element-doped gallium nitride-based film, the porosity is optimized and the filling of sulfonated elastomer and lithium titanate is formed. The structure is to improve the transmission efficiency and structural stability of lithium ions, and the negative electrode and the positive electrode are connected through a barrier layer to reduce the use of current collectors.

Benefits of technology

It improves the lithium storage and circulation performance of lithium ions, extends the service life of the battery, enhances the energy density of the battery, and avoids the problems of electrolyte corrosion and low lithium ion transmission efficiency, improving the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113036107B_ABST
    Figure CN113036107B_ABST
Patent Text Reader

Abstract

The present application relates to a graphene battery negative electrode material layer and a preparation method thereof, and a lithium-ion battery. The above-mentioned battery negative electrode material layer includes: an active layer; a first layer formed on the active layer, the first layer is a composite material layer composed of nano-metal alloy and graphene; and a second layer formed on the first layer, the second layer is a thin film containing a single substance doped gallium nitride base, the first layer and the second layer are both porous structures, the porosity of the second layer is greater than the porosity of the first layer, and the pores of the second layer are filled with a sulfonated elastomer that can form branch crosslinks with the single substance doped gallium nitride base. The lithium-ion battery prepared from the above-mentioned negative electrode material layer has high lithium ion transmission efficiency, good lithium storage capacity and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a graphene battery negative electrode material layer and a preparation method thereof, and a lithium-ion battery. Background Art

[0002] Lithium-ion battery is a rechargeable battery. Due to its advantages such as long cycle life, high energy density and high open circuit voltage, it is widely used as a power source in electronic products and new energy fields.

[0003] At present, most lithium-ion batteries use carbon as the negative electrode material. Their main working principle is the movement of lithium ions between the positive and negative electrodes. Specifically, when the battery is charged, the lithium ions generated by the positive electrode of the battery move to the negative electrode through the electrolyte. The lithium ions that reach the negative electrode will be embedded in the microporous structure of the negative electrode. When the battery is discharged, the lithium ions embedded in the negative electrode will be detached and return to the positive electrode.

[0004] However, during the charging and discharging process, traditional lithium-ion batteries have problems such as low lithium storage capacity, low lithium ion transmission efficiency, and poor cycle performance. Summary of the invention

[0005] Based on this, it is necessary to provide a new graphene battery negative electrode material layer and its preparation method, and a lithium ion battery to address the problems of low lithium storage capacity, low lithium ion transmission efficiency, and poor cycle performance of traditional lithium ion batteries.

[0006] A graphene battery negative electrode material layer comprises: an active layer; a first layer formed on the active layer, the first layer being a composite material layer composed of a nano metal alloy and graphene; and a second layer formed on the first layer, the second layer being a thin film containing a single substance doped gallium nitride base, the first layer and the second layer both being porous structures, the porosity of the second layer being greater than that of the first layer, and the pores of the second layer being filled with a sulfonated elastomer capable of forming branch crosslinks with the single substance doped gallium nitride base.

[0007] In one embodiment, the pores of the second layer are filled with lithium titanate wrapped by a sulfonated elastomer.

[0008] In one embodiment, the porosity of the first layer is 20%-28%, and the porosity of the second layer is 30%-40%.

[0009] In one embodiment, the second layer is provided with a plurality of grooves which do not penetrate through the second layer.

[0010] In one embodiment, the grooves adjacent to each other have different groove depths.

[0011] In one embodiment, a ceramic mesh is provided at the bottom of at least part of the grooves.

[0012] In one embodiment, the first layer is a nano-iron-nickel alloy layer doped with graphene sheets.

[0013] In one embodiment, the nano-iron-nickel alloy layer doped with graphene sheets contains a plurality of nano-iron-nickel alloy microspheres, and the graphene sheets are located in the gaps between the nano-iron-nickel alloy microspheres.

[0014] The present application also provides a method for preparing a negative electrode material layer of a battery, which comprises the following steps:

[0015] mixing the nanometal alloy and graphene to obtain a mixture;

[0016] attaching the mixture to an active layer and sintering to obtain a first layer solidified on the active layer;

[0017] In an inert atmosphere, a single-element doped gallium nitride-based material is spin-coated on the first layer to form a second layer on the first layer.

[0018] The present application also provides a lithium-ion battery, which includes a battery negative electrode material layer as described in any one of the present application, a barrier layer impregnated with an electrolyte, and a battery positive electrode material layer, wherein the two sides of the barrier layer are respectively located in the grooves of the battery negative electrode material layer and the battery positive electrode material layer to connect the battery negative electrode material layer and the battery positive electrode material layer.

[0019] The negative electrode material layer of the above-mentioned battery has a simple structure. The prepared composite material layer composed of nano-metal alloy and graphene and the thin film containing single-element doped gallium nitride are both porous structure layers with large specific surface area, which is conducive to the loading of lithium ions and has strong power storage capacity. In addition, the single-element doped gallium nitride-based material has a stable multi-dimensional spatial structure, which can not only improve the transmission efficiency of lithium ions, but also avoid the collapse of the skeleton structure caused by the insertion and extraction of lithium ions, thereby ensuring that the prepared lithium-ion battery has high lithium ion transmission efficiency and good lithium storage capacity and cycle performance.

[0020] Furthermore, the inventors of the present application have found through research that the poor cycle performance of traditional batteries is mainly due to the gas expansion during the charge and discharge process, and repeated charge and discharge cycles lead to battery scrapping. The existing method is to make a protective layer to prevent the negative electrode sheet from being corroded by the electrolyte. However, the dense structure of the protective layer will cause the migration rate of lithium ions and charges to decrease, which will reduce other battery performance while protecting the battery cycle performance. The present application rationally combines the first layer and the second layer composed of different materials, and optimizes the porosity of the second layer and the porosity of the first layer, which not only ensures that a certain amount of electrolyte passes through, but also does not cause excessive corrosion damage to the negative electrode sheet due to the protective effect of the two layers.

[0021] In order to further protect the negative electrode sheet from being corroded by transition metal ions (such as manganese ions, nickel ions and iron ions) in the electrolyte. The inventors fill the sulfonated elastomer in the pores of the second layer, which can selectively avoid the contact between the transition metal ions in the electrolyte and the negative electrode active material, and will not affect the entry and exit of lithium ions, which can improve the lithium ion conductivity. In addition, the vulcanized elastomer is filled in the pores of the second layer, and the sulfonic group in the vulcanized elastomer can form branch crosslinks with the elemental doped gallium nitride group, giving the second layer good structural strength, thereby resisting the structural collapse caused by the passage of a large number of lithium ions. However, the inventors found that encapsulating the negative electrode active material particles with other non-sulfonated elastic materials does not have much benefit in improving the cycle stability of lithium-ion batteries.

[0022] Furthermore, the pores of the second layer are filled with lithium titanate wrapped by sulfonated elastomer. Lithium titanate has a spinel structure, which can achieve charging without lithium precipitation under low temperature conditions. At the same time, the current will rise in temperature during the charging process, thereby increasing the temperature inside the battery cell and improving the viscosity of the electrolyte.

[0023] The lithium-ion battery structure of the present application is cleverly designed, and the two sides of the barrier layer soaked with electrolyte are respectively located in the grooves of the battery negative electrode material layer and the battery positive electrode material layer, connecting the battery negative electrode material layer and the battery positive electrode material layer. The traditional current collector is omitted to obtain a battery structure without a current collector. Since there is no current collector sheet such as aluminum copper foil, the weight of the battery cell is reduced, and the contribution of the current collector to energy is 0, which indirectly improves the energy density of the lithium-ion battery. Compared with the traditional lithium-ion battery containing a current collector, the energy density can be increased by about 20%. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a schematic diagram of the structure of a negative electrode material layer of a battery provided in Example 2 of the present application;

[0025] Figure 2 This is a schematic diagram of the structure of a negative electrode material layer of a battery provided in Example 3 of the present application;

[0026] Figure 3 This is a schematic diagram of the structure of a negative electrode material layer of a battery provided in Example 6 of the present application;

[0027] Figure 4 This is a schematic diagram of the structure of a negative electrode material layer of a battery provided in Example 7 of the present application;

[0028] Figure 5 This is a schematic diagram of the structure of a negative electrode material layer of a battery provided in Comparative Example 2 of the present application;

[0029] Figure 6Schematic diagram of the structure of a lithium-ion battery in one embodiment of the present application. DETAILED DESCRIPTION

[0030] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0032] See also Figures 1 to 4 In one embodiment of the present application, a battery negative electrode material layer 10 is provided, which includes: an active layer 101, a first layer 102 formed on the active layer 101, the first layer 102 is a composite material layer composed of nano-metal alloy and graphene, and a second layer 103 formed on the first layer 102, the second layer 103 is a material layer containing metal-doped gallium nitride, the first layer 102 and the second layer 103 are both porous structures, the porosity of the second layer 103 is greater than the porosity of the first layer 102, and the pores of the second layer 103 are filled with a sulfonated elastomer that can form branch crosslinks with the element-doped gallium nitride.

[0033] The active layer 101 is selected from a silicon layer, a silicon oxide layer or a silicon nitride layer. Further, the porosity of the active layer 101 is 10%-15%, which is conducive to the rapid passage of lithium ions. In addition, a higher body density can be ensured to help increase the battery capacity.

[0034] The first layer 102 is a composite material layer composed of nano-metal alloy and graphene. The introduction of graphene can improve the conductivity of the nano-metal alloy. The composite material layer composed of nano-metal alloy and graphene is a porous structure layer with a large specific surface area, which is conducive to the loading of lithium ions.

[0035] Furthermore, the particle diameter of the nano metal alloy is 100-200 nm, the shape is spherical, and the purity is above 99.96%.

[0036] Among them, sulfonated elastomers have high elasticity (high elastic deformation value). Elastic deformation is a deformation that can be fully recovered after the mechanical stress is released, and the recovery process is basically instantaneous (without obvious time delay). Elastomers such as vulcanized natural rubber can exhibit tensile elastic deformation from 2% to 1,000% (10 times its original length). Sulfonated elastomers can be used to wrap cathode active material particles. Wrapping means basically completely surrounding one or more particles without allowing the particles to come into direct contact with the electrolyte in the battery. The sulfonated elastomer can be selected from sulfonated forms of natural polyisoprene (e.g., cis-1,4-polyisoprene natural rubber (NR) and trans-1,4-polyisoprene rubber), synthetic polyisoprene, polybutadiene, chloroprene rubber (CR), polychloroprene (e.g., chloroprene rubber, Baypren, etc.), butyl rubber (copolymer of isobutylene and isoprene, IIR), including halogenated butyl rubber (chlorobutyl rubber (CIIR) and bromobutyl rubber (BIIR), styrene-butadiene rubber (copolymer of styrene and butadiene, SBR).

[0037] Furthermore, the first layer 102 is a nano-iron-nickel alloy layer doped with graphene sheets. Graphene sheets have better dispersion properties than ordinary graphene and are easy to be evenly dispersed in the first layer 102. Furthermore, the nano-iron-nickel alloy layer contains a plurality of nano-iron-nickel alloy microspheres, and the graphene sheets are located in the gaps between the nano-iron-nickel alloy microspheres. Due to the selection of spherical nano-iron-nickel alloy microspheres, the pores of the first layer 102 can be greatly increased after the graphene sheets and the spherical iron-nickel alloy microspheres are composited, which is conducive to the smooth passage of lithium ions in the pores, thereby improving the specific capacity of lithium ion charging and discharging and extending the performance of cycle charging.

[0038] Furthermore, the average thickness of the graphene sheets is 0.8-1.0 nm, and graphene sheets in this thickness range are more conducive to filling the gaps between the nano-iron-nickel alloy microspheres.

[0039] Furthermore, the mass ratio of the graphene sheet to the nanometal alloy is (1-1.5): (80-90). This ratio is reasonable. If too much graphene sheet is added, the mechanical properties will deteriorate. If too little graphene sheet is added, good conductivity cannot be achieved.

[0040] It can be understood that in order to further improve the dispersion performance of the graphene sheets in the first layer 102, some dispersants may be added.

[0041] Among them, the second layer 103 is a thin film containing a single element doped gallium nitride. The single element doped gallium nitride-based material can form a stable multi-dimensional space structure, which can not only improve the transmission efficiency of lithium ions, but also avoid the collapse of the skeleton structure caused by the insertion and extraction of lithium ions, thereby ensuring that the prepared lithium-ion battery has good lithium storage capacity and cycle performance. In addition, gallium nitride doped with a single element has good corrosion resistance, especially in an acidic electrolyte environment, and has good resistance, and the multi-dimensional space structure formed is stable.

[0042] Further, the single-element doped gallium nitride-based film is a metal-doped gallium nitride-based material layer. Further, the second layer 103 is a magnesium-doped gallium nitride-based film, and the mass percentage of magnesium doping in the magnesium-doped gallium nitride-based film is 2%-8%, for example, the mass percentage of magnesium doping in the magnesium-doped gallium nitride-based film is 2%, 4%, 5%, 6% or 8%. Further, the second layer 103 is an aluminum-doped gallium nitride-based film, and the mass percentage of aluminum doping in the aluminum-doped gallium nitride-based film is 1%-5%, for example: the mass percentage of aluminum doping in the aluminum-doped gallium nitride-based film is 1%, 3% or 5%. Of course, it can be understood that the single-element doped gallium nitride-based material can also be a non-metal-doped gallium nitride-based material, such as a silicon-doped gallium nitride-based material.

[0043] The applicant further discovered that if the aluminum-doped gallium nitride-based material is soaked in a sodium chloride solution, tiny pits will be formed on the surface of the aluminum-doped gallium nitride. This defect will improve the conductivity of the aluminum-doped gallium nitride-based film and increase the diffusion space of lithium ions. And this tiny defect will alleviate the volume expansion of the battery caused by gas production during charging and discharging. Furthermore, the sodium chloride solution is a 10%-30% sodium chloride solution.

[0044] Among them, the porosity of the second layer 103 is greater than the porosity of the first layer 102. That is to say, the second layer 103 is looser than the first layer 102, and the second layer is a multi-dimensional skeleton space composed of a single substance doped gallium nitride-based material, which is very conducive to the rapid passage of electrolyte, especially lithium ions. When a large amount of electrolyte penetrates the second layer 103 and reaches the first layer 102, the combination of nanometal alloy and graphene has a certain inertness, which can hinder the corrosion of the electrolyte. In addition, there is a gradient difference from loose to dense in the porosity of the second layer 103 and the first layer 102, and this design will not affect the rapid passage of lithium ions. Further, the porosity of the first layer 102 is 20%-28%, and the porosity of the second layer 103 is 30%-40%. In addition, compared with other carbon nanotubes, zirconium oxide, carbon, etc., the selection of graphene can reduce impedance and improve battery cycle performance while playing an anti-corrosion role.

[0045] In one embodiment, the second layer 103 is provided with a groove 110 that does not penetrate the second layer 103. That is, the groove depth of the groove 110 is less than the thickness of the second layer 103. Thus, the lithium ion loading capacity of the second layer 103 is increased. Furthermore, the groove depths of the adjacent grooves 110 are different, and the irregular groove depth will not cause a short circuit phenomenon after the positive electrode is combined later. More preferably, it is arranged in a regular gradient, for example, see Figure 2 , the groove depth of the central area of ​​the second layer 103 decreases gradually toward the edge area of ​​the second layer 103. In addition, another purpose of the second layer 103 being provided with the groove 110 that does not penetrate the second layer 103 is to facilitate direct plugging of the positive electrode protrusion corresponding to the positive electrode material layer coated with the barrier, thereby reducing the space of the battery and making the electrode structure more compact.

[0046] In one embodiment, at least part of the groove bottom is provided with a ceramic mesh, and the mesh ceramic structure does not affect the flow of electrolyte, especially lithium ions, and can also isolate electrons to prevent short circuits between positive / negative plates when assembled with the positive electrode.

[0047] In one embodiment, the upper surface of the second layer 103 is a rough surface with uneven surfaces, which is more conducive to the rapid penetration of lithium ions into the second layer 103 and loading.

[0048] In addition, the inventors have also found that if a groove 110 is opened at the edge of the second layer 103, lithium deposition will be reduced. If there is too much lithium deposition at the edge, the safety performance will be reduced after multiple cycles of use.

[0049] It is understandable that the grooves may be formed by etching liquid or laser physical etching.

[0050] The present application also provides a method for preparing a negative electrode material layer of a battery, which comprises the following steps:

[0051] S1. Mixing the nano-metal alloy and graphene to obtain a mixture.

[0052] S2, attaching the mixture to the active layer 101, and sintering to obtain the first layer 102 solidified on the active layer 101, wherein the method of attaching the mixture to the active layer 101 can be a coating method and / or an electrostatic spraying method.

[0053] In an inert atmosphere, a single-element doped gallium nitride-based material is spin-coated on the first layer 102 to form a second layer 103 on the first layer 102. Further, the spin-coating condition is a vacuum degree of 0.5*10 -7Torr, the argon flow rate is 5ppm. Further, the pores of the second layer are filled with sulfonated elastomer, which can be directly pressurized or SBS dissolved in toluene is added with benzophenone and TAA to prepare a mixed solution, which is filled in the pores of the second layer 103, and heated for 24 hours under ultraviolet light and a power of 80-120W at room temperature. During heating and subsequent use, the sulfonated elastomer and the element-doped gallium nitride base will slowly form branch crosslinks.

[0054] Combination Figure 6 As shown, the present application also provides a lithium-ion battery, comprising a battery negative electrode material layer 10 as described in any one of the present application, a barrier layer 20 impregnated with electrolyte and a battery positive electrode material layer 30, wherein both sides of the barrier layer 20 are respectively located in the grooves of the battery negative electrode material layer 10 and the battery positive electrode material layer 30 to connect the battery negative electrode material layer 10 and the battery positive electrode material layer 30.

[0055] The above-mentioned lithium-ion battery structure is cleverly designed. The two sides of the barrier layer are respectively located in the grooves of the battery negative electrode material layer and the battery positive electrode material layer, connecting the battery negative electrode material layer and the battery positive electrode material layer, eliminating the traditional current collector, and obtaining a battery structure without a current collector. Since there is no current collector sheet such as aluminum copper foil, the weight of the battery cell is reduced, and the contribution of the current collector to energy is 0, which indirectly improves the energy density of the lithium-ion battery. Compared with the traditional lithium-ion battery containing a current collector, the energy density can be increased by about 20%.

[0056] In order to make the purpose and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0057] Example 1

[0058] A method for preparing a negative electrode material layer of a battery comprises the following steps:

[0059] (1) 1.5 parts of graphene and 85 parts of nano-iron-nickel alloy microspheres with a diameter of 120 nm were mixed, added into 300 parts of N-methylpyrrolidone solution, and stirred under ultrasonic conditions.

[0060] (2) The mixed solution obtained in (1) is coated on a silicon oxide layer with a porosity of 15%, coated at 3500 r / min for 1.5 hours, and then sintered at 100°C. By controlling the coating speed and time, a first layer with a porosity of 20% is formed on the silicon oxide layer.

[0061] (3) Spin coating an organic alcohol solution containing aluminum-doped gallium nitride material on the first layer 102, wherein the mass percentage of aluminum doping in the aluminum-doped gallium nitride material is 4%, and the spin coating conditions are: vacuum degree 0.5*10 -7 Torr, argon flow rate is 5ppm, spin coating and sintering treatment is carried out for 1h, and the second layer with a porosity of 30% is formed on the first layer by controlling the spin coating conditions and sintering time. Benzophenone (BZP, 0.112g; 0.83mmol) and TAA (4.01mL; 0.124mol) are added to SBS (1.000g) dissolved in toluene (200mL) to prepare a mixed solution, which is filled in the pores of the second layer, and heated at room temperature under 300nm ultraviolet light and 100W power for 24h to obtain a sulfonated elastomer that forms branch crosslinks with a single-element doped gallium nitride base.

[0062] Example 2

[0063] A method for preparing a negative electrode material layer of a battery comprises the following steps:

[0064] (1) 1.5 parts of graphene sheets and 88 parts of nano-iron-nickel alloy microspheres with a diameter of 120 nm were mixed, added into 300 parts of N-methylpyrrolidone solution, and stirred under ultrasonic conditions.

[0065] (2) The mixed solution obtained in (1) is coated on a silicon oxide layer with a porosity of 10%, coated at 3500 r / min for 1.2 h, and then sintered at 100°C. By controlling the coating speed and time, a first layer with a porosity of 22% can be formed on the silicon oxide layer.

[0066] (3) Spin coating an organic alcohol solution containing aluminum-doped gallium nitride material on the first layer, wherein the mass percentage of aluminum doping in the aluminum-doped gallium nitride material is 6%, and the spin coating conditions are: vacuum degree 0.4*10 -7 Torr, argon flow rate is 5ppm, spin coating and sintering treatment is carried out for 1h, and by controlling the spin coating conditions and sintering time, a second layer with a porosity of 33% is formed on the first layer. Benzophenone (BZP, 0.112g; 0.83mmol) and TAA (4.01mL; 0.124mol) are added to SBS (1.000g) dissolved in toluene (200mL) to prepare a mixed solution, which is filled in the pores of the second layer, and heated at room temperature under 300nm ultraviolet light and 100W power for 24h to obtain a sulfonated elastomer that forms branch crosslinks with a single-element doped gallium nitride base.

[0067] (4) Etch a groove on the second layer to form Figure 1 Shape shown.

[0068] Example 3

[0069] A method for preparing a negative electrode material layer of a battery comprises the following steps:

[0070] (1) 1.5 parts of graphene sheets and 85 parts of nano-iron-nickel alloy microspheres with a diameter of 120 nm were mixed, added into 300 parts of N-methylpyrrolidone solution, and stirred under ultrasonic conditions.

[0071] (2) The mixed solution obtained in (1) is coated on a silicon oxide layer with a porosity of 10%. After coating at 3000 r / min for 1 hour, the mixture is sintered at 100°C. By controlling the coating speed and time, a first layer with a porosity of 25% is formed on the silicon oxide layer 101.

[0072] (3) Spin coating an organic alcohol solution containing aluminum-doped gallium nitride material on the first layer. The spin coating conditions are: vacuum degree 0.5*10 -7 Torr, argon flow rate is 8ppm, wherein the mass percentage of aluminum doping in the aluminum-doped gallium nitride material is 6%, and the spin coating is followed by sintering for 2h, and by controlling the spin coating conditions and sintering time, a second layer with a porosity of 35% is formed on the first layer. Benzophenone (BZP, 0.112g; 0.83mmol) and TAA (4.01mL; 0.124mol) are added to SBS (1.000g) dissolved in toluene (200mL) to prepare a mixed solution, which is filled in the pores of the second layer, and heated for 24h at room temperature under 300nm ultraviolet light and 100W power to obtain a sulfonated elastomer that forms branch crosslinks with a single substance doped gallium nitride base.

[0073] (4) Etch a groove on the second layer to form Figure 2 Shape shown.

[0074] Example 4

[0075] A method for preparing a negative electrode material layer of a battery, wherein the preparation method is substantially the same as that of Example 3, except that, in step (1), 1 part of a graphene sheet is mixed with 90 parts of nano-iron-nickel alloy microspheres with a diameter of 120 nm, and then added to 290 parts of an N-methylpyrrolidone solution and stirred under ultrasonic conditions.

[0076] Example 5

[0077] A method for preparing a negative electrode material layer of a battery, wherein the preparation method is substantially the same as that of Example 3, except that the aluminum-doped gallium nitride-based material is soaked in a 15% sodium chloride solution for 2 hours, dried, and then dissolved in an organic alcohol solution.

[0078] Example 6

[0079] A method for preparing a negative electrode material layer of a battery, wherein the preparation method is substantially the same as that of Example 3, except that in step (3), an organic alcohol solution containing silicon-doped gallium nitride material is spin-coated on the first layer. In step (4), a groove is etched on the second layer to form Figure 3 Shape shown.

[0080] Example 7

[0081] A method for preparing a negative electrode material layer of a battery, wherein the preparation method is substantially the same as that of Example 3, except that in step (4), a groove is etched on the second layer to form Figure 4 After step (4), the method further includes etching the surface of the second layer to form a rough surface on the surface of the second layer.

[0082] Comparative Example 1

[0083] A method for preparing a negative electrode material layer of a battery, wherein the preparation method is substantially the same as that of Example 3, except that in step (2), the sulfonated elastomer is not prepared in the pores of the second layer.

[0084] Comparative Example 2

[0085] A method for preparing a negative electrode material layer of a battery, wherein the preparation method is substantially the same as that of Example 3, except that an organic alcohol solution containing aluminum-doped gallium nitride material is directly spin-coated on the silicon oxide layer, and the spin-coating conditions are: vacuum degree 0.5*10 -7 Torr, the argon flow rate is 8 ppm, wherein the mass percentage of aluminum doping in the aluminum-doped gallium nitride material is 6%, and the spin coating is followed by sintering for 2 hours. By controlling the spin coating conditions and sintering time, a second layer with a porosity of 35% is formed.

[0086] (4) Etch the second layer as follows Figure 5 Grooves shown.

[0087] Comparative Example 3

[0088] A method for preparing a negative electrode material layer of a battery, wherein the preparation method is substantially the same as that of Example 3, except that step (3) and step (4) are omitted.

[0089] Comparative Example 4

[0090] A method for preparing a negative electrode material layer of a battery, wherein the preparation method is substantially the same as that of Example 3, except that the aluminum-doped gallium nitride material is replaced by a gallium nitride material.

[0091] Comparative Example 5

[0092] A method for preparing a negative electrode material layer for a battery is generally the same as that of Example 3, except that in step (2), the coating speed and time are controlled to form a first layer with a porosity of 30% on the silicon oxide layer 101.

[0093] In step (3), a second layer having a porosity of 25% was formed on the first layer.

[0094] Effect verification

[0095] The negative electrode material layer prepared in each embodiment and comparative example is made into a negative electrode sheet of a lithium ion battery, lithium iron phosphate is used as the positive electrode sheet, PET coated with ceramic particles is used as a composite diaphragm, the electrolyte is lithium hexafluorophosphate, and the solvent is 15% ethylene carbonate, 20% propylene carbonate, 60% dimethyl carbonate, 2.5% propylene chloride carbonate (film former) and 2.5% ethyl acetate (surfactant) by mass percentage. The pole pieces are assembled into batteries, and the charging cut-off voltage of each lithium ion secondary battery is 4.5V. The batteries prepared in each embodiment and comparative example are tested for electrical performance, wherein the volume expansion rate is the volume expansion rate of storage at 60°C for 100 days, and the test results are shown in Table 1.

[0096] In addition, the present application also examines the capacity recovery at 25°C to determine whether lithium deposition occurs during the low-temperature charging process of the lithium battery. The judgment standard is that after 400 cycles, the capacity recovery is greater than 97% and no lithium deposition occurs. If the capacity recovery is less than 96%, lithium deposition occurs. Battery low-temperature cycle test: At -25°C, the lithium-ion battery prepared in the embodiment and the comparative example is placed for 6 hours, then charged to 4.0V at 0.2C current and left to stand for 1 hour. Discharged to 2.5V at 0.2C current, left to stand for 1 hour, cycled 800 times, and the test results are shown in Table 2.

[0097] Table 1

[0098]

[0099] Table 2

[0100]

[0101] Among them, the material selection of the first layer in comparative example 1 is different from the combination of the present application, that is, the conventional combination of graphene sheets and aluminum oxide, the first layer of the present application is not included in comparative example 2, the second layer of the present application is not included in comparative example 3, and the second layer of comparative example 4 is non-doped gallium nitride. It can be seen from Table 1 that the charging capacity and discharge capacity ratios in the embodiments are significantly greater than those in the comparative examples, and the embodiments have relatively high input and output characteristics. Among them, embodiments 5 and 7 are the most excellent.

[0102] In addition, in Example 5, since the aluminum-doped gallium nitride-based material is immersed in a sodium chloride solution, tiny pits are formed on the surface of the aluminum-doped gallium nitride, which reduces the volume expansion caused by gas production. The volume expansion rate is significantly lower than that of the comparative example. Under long-term storage, the volume expansion rate is only 21%.

[0103] From the test results in Table 2, it can be seen that at -25°C, after 400 cycles at 0.2C current 4.0V, in the worst Example 6, the room temperature capacity recovery rate is still above 97.5%, while the battery sample in Comparative Example 2 is only 77.4%, and after 800 cycles, it is less than 50%. This verifies that the low-temperature charging performance of the present application is excellent, and effectively avoids the occurrence of lithium deposition at the edge of lithium-ion batteries.

[0104] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0105] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.

Claims

1. A graphene battery negative electrode material layer, characterized in that: include: Active layer; A first layer formed on the active layer, wherein the first layer is a composite material layer composed of nano-iron-nickel alloy and graphene, and the introduction of graphene can improve the electrical conductivity of the nano-iron-nickel alloy; as well as A second layer formed on the first layer, the second layer is an aluminum-doped gallium nitride-based film, the first layer and the second layer are both porous structures, the porosity of the second layer is greater than the porosity of the first layer, and the pores of the second layer are filled with a sulfonated elastomer that can form branch crosslinks with the aluminum-doped gallium nitride base; The porosity of the first layer is 20%-28%, and the porosity of the second layer is 30%-40%.

2. The graphene battery negative electrode material layer according to claim 1, characterized in that: The pores of the second layer are filled with lithium titanate wrapped by a sulfonated elastomer.

3. The graphene battery negative electrode material layer according to claim 1 or 2, characterized in that: The second layer is provided with a plurality of grooves which do not penetrate the second layer.

4. The graphene battery negative electrode material layer according to claim 3, characterized in that: The grooves adjacent to each other have different groove depths.

5. The graphene battery negative electrode material layer according to claim 3, characterized in that: A ceramic mesh is provided at the bottom of at least part of the grooves.

6. The graphene battery negative electrode material layer according to claim 1 or 2, characterized in that: The first layer is a nano-iron-nickel alloy layer doped with graphene sheets.

7. The graphene battery negative electrode material layer according to claim 6, characterized in that: The nano-iron-nickel alloy layer doped with graphene sheets contains a plurality of nano-iron-nickel alloy microspheres, and the graphene sheets are located in the gaps between the nano-iron-nickel alloy microspheres.

8. A method for preparing a graphene battery negative electrode material layer, characterized in that: The steps include: mixing nano iron-nickel alloy and graphene to obtain a mixture; attaching the mixture to an active layer and sintering to obtain a first layer solidified on the active layer; The method of attaching the mixture to the active layer is a coating method; In an inert atmosphere, spin-coating an aluminum-doped gallium nitride-based material on the first layer to form a second layer on the first layer; The porosity of the first layer is 20%-28%, and the porosity of the second layer is 30%-40%; The pores of the second layer are filled with a sulfonated elastomer.

9. A lithium ion battery, characterized in that: It comprises the graphene battery negative electrode material layer as described in any one of claims 1 to 7, a barrier layer impregnated with an electrolyte, and a battery positive electrode material layer, wherein the two sides of the barrier layer are respectively located in the grooves of the battery negative electrode material layer and the battery positive electrode material layer to connect the battery negative electrode material layer and the battery positive electrode material layer.