Alkali-soluble photosensitive resin with condensed ring naphthalene structure and composition and preparation method thereof
Through the modification and preparation of the fused ring naphthalene structure epoxy resin and the preparation of composition, the problem of plug-in ink being prone to cracking at high temperatures is solved, the high temperature resistance and solder resistance of the ink are achieved, and the high precision needs of the circuit board factory are met. .
Patent Information
- Application Number
- CN202110706848.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-06-24
AI Technical Summary
The existing plug-in ink is prone to cracking during high temperature and SMT, and cannot have the dual properties of cracking resistance and solder-resistance oil at the same time, which cannot meet the high precision needs of circuit board factories.
Using a condensed ring naphthalene structure epoxy resin, alkali-soluble photosensitive resin and its composition are prepared by modification, and low thermal expansion coefficient and acid anhydride reaction are used to prepare inks that can withstand high temperatures and are not easy to crack, and combined with photosensitizers and light Polymerize the monomer and filler to form a suitable ink composition.
It achieves the effect that ink is not easy to crack at high temperatures, and has solder resistance, which improves the process capability of the circuit board factory and is suitable for a variety of on-site conditions.
Smart Images

Figure CN113311664B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of printed circuit board ink preparation, and in particular to an alkali-soluble photosensitive resin with a condensed ring naphthalene structure, a composition thereof and a preparation method thereof. Background Art
[0002] With the increasing precision of circuit boards, the number of layers of circuit boards is increasing. Many conductions between layers need to be connected by hole rings, and many conduction holes need to be protected by plugging holes to avoid damage during circuit board surface treatment or SMT operation. At present, most circuit board factories improve the plugging effect by on-site process improvement, but this can only play a temporary effect. CN1396218A discloses reducing cavitation or cracking caused by solvent volatilization in the system by preparing solvent-free plugging ink, but it is rarely used in actual production, because if the solvent-free plugging ink is really to be industrialized, a large amount of photosensitive monomer needs to be added as a diluent to reduce the viscosity of the system, and the addition of a large amount of photosensitive monomer is bound to greatly reduce the toughness of the system, and it is more likely to crack after being heated, so it cannot fundamentally solve the problem of plugging ink being easy to crack when heated. There are also conventional epoxy resins such as o-cresol or bisphenol A that are used to make plugging inks. These resins can achieve the effect of plugging holes, but there is also the risk of cracking after tin spraying (thermal shock) or SMT after plugging holes, or the problem of cracking at the plugging position due to long parking time after the plugging operation.
[0003] In actual production, most users will combine plugging oil and surface oil at one time to reduce the process, thereby reducing labor and production costs. Plug oil alone cannot meet the needs of most users, so it is necessary to develop an ink that has the dual properties of anti-cracking plugging oil and solder mask surface oil. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides an alkali-soluble photosensitive resin having a condensed ring naphthalene structure, a composition thereof and a preparation method thereof. The present invention utilizes the low thermal expansion coefficient of the epoxy resin having a condensed ring naphthalene structure, and simultaneously modifies the epoxy resin having a condensed ring naphthalene structure to prepare an alkali-soluble photosensitive resin and a composition thereof. The prepared ink can be used for both plugging and printing, can withstand high temperatures and is not prone to cracking.
[0005] The technical solution of the present invention is as follows:
[0006] An alkali-soluble photosensitive resin having a condensed-ring naphthalene structure, wherein the preparation method of the alkali-soluble photosensitive resin comprises the following steps:
[0007] (1) adding a diluent into a reaction kettle, heating it, and then sequentially adding an epoxy resin with a condensed ring naphthalene structure, a catalyst and a polymerization inhibitor, stirring to obtain an initial product;
[0008] (2) heating to a first reaction temperature, stirring and dispersing, and then adding an unsaturated carboxylic acid to the initial product prepared in step (1) to react and obtain an intermediate having an unsaturated double bond;
[0009] (3) adding a diluent to the intermediate having an unsaturated double bond prepared in step (2), lowering the temperature to a second reaction temperature, and adding an acid anhydride to react to obtain a carboxyl-containing intermediate;
[0010] (4) adding a polymerization inhibitor and a diluent to the carboxyl-containing intermediate prepared in step (3), cooling the mixture to 60-70° C., and filtering the mixture to obtain an alkali-soluble photosensitive resin having a condensed ring naphthalene structure.
[0011] Furthermore, the diluents in steps (1), (3) and (4) are all diethylene glycol ethyl ether acetate; and the inhibitors in steps (1) and (4) are all one or more of HQ, THQ, MEHQ and BHT.
[0012] Furthermore, in step (1), the heating refers to heating to 95-100° C.; the epoxy resin with a condensed ring naphthalene structure is purchased from DIC Corporation of Japan, and the model is one or more of HP-4032, HP-4032D, HP-4710, HP-4770, HP-5000, HP-7200, and HP-7200H; the epoxy resin with a condensed ring naphthalene structure can also be purchased from Nippon Kayaku Co., Ltd., and the model is one or more of NC-7000L and NC-7300L.
[0013] Furthermore, in step (1), the catalyst is one or more of triphenylphosphine and benzylamine; the mass ratio of the diluent to the epoxy resin with a condensed naphthalene structure is (0.5-0.6):1; the mass ratio of the catalyst to the epoxy resin with a condensed naphthalene structure is (0.003-0.005):1; the mass ratio of the inhibitor to the epoxy resin with a condensed naphthalene structure is (0.006-0.01):1; the stirring speed is 150-200 r / min, and the time is 30-40 min.
[0014] Furthermore, in step (2), the first reaction temperature is 110±5°C; the stirring speed is 150-200 r / min, and the time is 12-16h; the unsaturated carboxylic acid is one or more of acrylic acid, methacrylic acid, cinnamic acid, methylcinnamic acid, methylcinnamic acid isomers, oleic acid, and elaidic acid; the molar ratio of the carboxyl group in the unsaturated carboxylic acid to the epoxy group of the epoxy resin with a condensed ring naphthalene structure is (1.01-1.05):1; the unsaturated carboxylic acid is added by dropwise addition at a dropwise addition speed of 50-100 drops / min; and the reaction conditions are: controlling the reaction temperature to 110±5°C and reacting for 12-16h.
[0015] Furthermore, in step (3), the mass ratio of the diluent to the epoxy resin with a condensed naphthalene structure is (0.2-0.7):1; the second reaction temperature is 95-100°C; the acid anhydride is one or more of tetrahydrophthalic anhydride, tetrahydrophthalic anhydride derivatives, hexahydrophthalic anhydride, hexahydrophthalic anhydride derivatives, maleic anhydride, and maleic anhydride derivatives; the molar ratio of the acid anhydride to the epoxy group of the epoxy resin with a condensed naphthalene structure is (0.34-0.9):1; and the reaction conditions are: controlling the reaction temperature to 100±5°C and reacting for 4-6h.
[0016] Furthermore, in step (4), the mass ratio of the diluent to the epoxy resin with a condensed naphthalene structure is (0.1-0.6):1; the mass ratio of the inhibitor to the epoxy resin with a condensed naphthalene structure is (0.002-0.004):1; the double bond equivalent of the alkali-soluble photosensitive resin with a condensed naphthalene structure is CEW=550-785, and the solid content is 50-70wt%.
[0017] A composition containing the alkali-soluble photosensitive resin, the composition comprising a main agent and a hardener; the main agent comprises the following components in parts by weight: 30-70 parts of the alkali-soluble photosensitive resin with a condensed ring naphthalene structure, 2-10 parts of a photosensitizer, 1-3 parts of a photopolymerizable monomer, 10-30 parts of a filler, 0.5-2 parts of a defoaming agent, and 1-5 parts of a diluent; the hardener comprises the following components in parts by weight: 5-20 parts of an epoxy resin with a condensed ring naphthalene structure, 1-4 parts of a latent curing agent, and 1-5 parts of a diluent; the mass ratio of the main agent to the hardener is (7-9):(1-3).
[0018] Further, the photosensitizer is purchased from IGM RESINS, and the model is one or more of IRGACURE 907, IRGACURE 369, IRGACURE 184, IRGACURE ITX-P, IRGACURE TPO, IRGACURE 819, and IRGACURE 784; the photopolymerizable monomer is purchased from Changxing Materials Industry Co., Ltd., and the model is EM 235, EM 241, EM 242, EM2380, EM265, One or more of EM266 and EM267; the filler is crystalline silicon powder produced by Sibelco (Shanghai) Mining Co., Ltd., model A8; the defoamer is an organosilicon defoamer purchased from Shin-Etsu Chemical Co., Ltd. of Japan, model KS-66; the diluent is diethylene glycol ethyl ether acetate purchased from Shanghai Tichem Industrial Co., Ltd.; the epoxy resin with a condensed ring naphthalene structure is purchased from DIC Co., Ltd. of Japan, model HP-4032, HP-4032D, HP-4710, HP-4770, HP-5000, HP-7200, HP-7200H or more; the epoxy resin with a condensed ring naphthalene structure can also be purchased from Nippon Kayaku Co., Ltd., model NC-7000L, NC-7300L or one or more; the latent curing agent is melamine purchased from Nanjing Meikai Technology Co., Ltd. or Shikoku Chemical Industry Co., Ltd. of Japan, model MAVT, 2E4MZ One or more of .
[0019] A method for preparing the alkali-soluble photosensitive resin composition, the method comprising the following steps:
[0020] (1) Preparation of the main agent: 30-70 parts by weight of an alkali-soluble photosensitive resin having a condensed ring naphthalene structure, 2-10 parts of a photosensitizer, 1-3 parts of a photopolymerizable monomer, 10-30 parts of a filler, 0.5-2 parts of a defoaming agent, and 1-5 parts of a diluent are mixed and dispersed, and then ground until the main agent particles have a diameter of less than 25 μm, and then used for later use;
[0021] (2) Preparation of hardener: 5 to 20 parts by weight of epoxy resin having a condensed naphthalene structure, 1 to 4 parts of a latent hardener, and 1 to 5 parts of a diluent are mixed and dispersed, and then ground until the particle diameter of the hardener is less than 25 μm, and set aside;
[0022] (3) mixing the main agent prepared in step (1) and the hardener prepared in step (2) in a mass ratio of (7-9): (1-3) and stirring to obtain an alkali-soluble photosensitive resin composition;
[0023] Furthermore, the dispersing speeds in step (1) and step (2) are both 1500-3000 r / min, and the dispersing time is both 15-30 min; the grinding is carried out in a three-roll mill; the stirring speed in step (3) is 1500-3000 r / min, and the time is 15-30 min.
[0024] The beneficial technical effects of the present invention are:
[0025] (1) The present invention utilizes the low thermal expansion coefficient of the epoxy resin with a condensed naphthalene structure, and simultaneously modifies the epoxy resin with a condensed naphthalene structure to prepare an alkali-soluble photosensitive resin and a composition thereof. The prepared ink can be used for both plugging and printing, and can withstand high temperatures (such as tin spraying, SMT) and is not easy to crack, which is incomparable to o-cresol-formaldehyde type, bisphenol A type or bisphenol F type epoxy resin; at the same time, it can also be used as a solder mask ink, which is a performance that a single plugging oil cannot have.
[0026] (2) The alkali-soluble photosensitive resin with polycyclic naphthalene structure for continuous plug-in printing and its composition prepared by the present invention can greatly improve the process capability of the circuit board factory.
[0027] (3) The present invention prepares an ink capable of realizing integrated plugging and printing by strictly controlling the acid value and double bond equivalent of the alkali-soluble photosensitive resin with a condensed ring naphthalene structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The test result of high temperature heating of the ink in the hole after the alkali-soluble photosensitive resin composition with a condensed ring naphthalene structure prepared in Example 1 of the present invention was subjected to a plug-and-strip printing operation.
[0029] Figure 2 The test result of the high temperature heating of the ink in the hole after the plug-and-print operation of the alkali-soluble photosensitive resin composition prepared in Comparative Example 1 of the present invention is shown. DETAILED DESCRIPTION
[0030] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments.
[0031] Example 1
[0032] An alkali-soluble photosensitive resin having a condensed ring naphthalene structure, wherein the preparation method thereof comprises the following steps:
[0033] First, 1.500 kg of diluent diethylene glycol ethyl ether acetate (DCAC), purchased from Shanghai Tichem Industrial Co., Ltd., was poured into a reactor and heated to 95°C, and 3.000 kg of condensed ring naphthalene epoxy resin HP-7200 (epoxy equivalent 273 g / eq.) produced by DIC of Japan, 0.018 kg of inhibitor HQ, purchased from Changzhou Yurong Chemical Co., Ltd., and 0.009 kg of catalyst triphenylphosphine (TPP), purchased from Suzhou Jinyuan Fine Chemical Co., Ltd., were poured into the reactor, and the initial product was obtained by stirring at 150 r / min for 40 min.
[0034] Then the temperature was raised to 105° C., and stirring and dispersion was continued at 200 r / min for 14 h. 0.799 kg of acrylic acid was added dropwise at 50 drops / min for reaction. The temperature of the reaction process was controlled at 110° C., and the reaction was carried out for 14 h to obtain an intermediate with an unsaturated double bond.
[0035] Then, 0.600 kg of diluent DCAC was added dropwise to the intermediate having an unsaturated double bond. When the temperature dropped to 95° C., 0.568 kg of tetrahydrophthalic anhydride was added for reaction. The reaction temperature was controlled at 100° C. and the reaction was carried out for 4 hours to obtain a carboxyl-containing intermediate.
[0036] Finally, 0.009 kg of inhibitor HQ and 0.687 kg of diluent DCAC were poured into the carboxyl-containing intermediate, and the temperature was cooled to 70°C by adding cooling water. After the reaction was completed, the material was filtered to obtain an alkali-soluble photosensitive resin having a condensed ring naphthalene structure. The synthesized alkali-soluble photosensitive resin having a condensed ring naphthalene structure had an acid value of 30 mgKOH / g, a double bond equivalent of CEW=650, and a solid content of 61%.
[0037] An alkali-soluble photosensitive resin composition having a condensed ring naphthalene structure, wherein the preparation method thereof comprises the following steps:
[0038] Preparation of the main agent: Weigh 30 parts of the alkali-soluble photosensitive resin prepared in Example 1, 10 parts of a composition of photosensitizer IRGACURE 907 and IRGACURE ITX-P purchased from IGM RESINS (the mass ratio of IRGACURE 907 to IRGACURE ITX-P is 3:1), 3 parts of a photopolymerizable monomer purchased from Changxing Materials Industry Co., Ltd., model EM265, 30 parts of crystalline silica powder A8 produced by Sibelco (Shanghai) Mining Co., Ltd., 0.5 parts of a defoamer purchased from Shin-Etsu Chemical Co., Ltd., model KS-66, and 4 parts of a diluent DCAC purchased from Shanghai Tichem Industrial Co., Ltd., mix and disperse at 1500 r / min for 30 min, and grind with a three-roll mill until the main agent particle diameter is less than 25 μm.
[0039] Preparation of hardener: 14.5 parts of polycyclic naphthalene resin HP4032, purchased from DIC Corporation of Japan, 4 parts of latent curing agent melamine, purchased from Nanjing Meikai Technology Co., Ltd., and 4 parts of diluent DCAC, purchased from Shanghai Tichem Industrial Co., Ltd., were mixed and dispersed at 1500 r / min for 30 min, and ground with a three-roll mill until the hardener particle diameter was less than 25 μm.
[0040] The main agent and the hardener prepared above were mixed in a mass ratio of 7:3, and then stirred and dispersed at 1500 r / min for 30 minutes to obtain an alkali-soluble resin composition having a condensed ring naphthalene structure.
[0041] Example 2
[0042] A method for preparing an alkali-soluble photosensitive resin with a condensed-ring naphthalene structure comprises the following steps:
[0043] First, 1.630 kg of diluent diethylene glycol ethyl ether acetate (DCAC), purchased from Shanghai Tichem Industrial Co., Ltd., was poured into a reactor and heated to 96°C, and 3.000 kg of condensed ring naphthalene epoxy resin HP-4710 (epoxy equivalent 170 g / eq.) produced by Japan DIC, 0.03 kg of inhibitor THQ, purchased from Changzhou Yurong Chemical Co., Ltd., and 0.015 kg of catalyst benzylamine, purchased from Suzhou Jinyuan Fine Chemical Co., Ltd., were poured into the reactor, and the initial product was obtained by stirring at 175 r / min for 35 min.
[0044] Then the temperature was raised to 110° C., and stirring and dispersing was continued at 175 r / min for 12 h. 1.328 kg of acrylic acid was added dropwise at 100 drops / min for reaction. The temperature of the reaction process was controlled at 105° C., and the reaction was carried out for 14 h to obtain an intermediate with an unsaturated double bond.
[0045] Then, 0.600 kg of diluent DCAC was added dropwise to the intermediate having an unsaturated double bond. When the temperature dropped to 100° C., 2.636 kg of methyltetrahydrophthalic anhydride was added for reaction. The reaction temperature was controlled at 105° C. and the reaction was carried out for 5 hours to obtain a carboxyl-containing intermediate.
[0046] Finally, 0.012 kg of polymerization inhibitor BHT and 1.14 kg of diluent DCAC were poured into the carboxyl-containing intermediate, and cooling water was added to cool the mixture to 65°C. After the reaction was completed, the material was filtered to obtain an alkali-soluble photosensitive resin having a condensed ring naphthalene structure. The synthesized alkali-soluble photosensitive resin having a condensed ring naphthalene structure had an acid value of 90 mgKOH / g, a double bond equivalent of CEW=550, and a solid content of 67%.
[0047] An alkali-soluble photosensitive resin composition having a condensed ring naphthalene structure, wherein the preparation method thereof comprises the following steps:
[0048] Preparation of the main agent: Weigh 40 parts of the alkali-soluble photosensitive resin prepared in Example 2, 8 parts of a composition of photosensitizers IRGACURE TPO and IRGACURE ITX-P purchased from IGM RESINS (the mass ratio of IRGACURE TPO: IRGACURE ITX-P is 3:1), 2 parts of photopolymerizable monomers purchased from Changxing Materials Industry Co., Ltd., model EM242, 21 parts of crystalline silica powder A8 produced by Sibelco (Shanghai) Mining Co., Ltd., 1 part of defoamer purchased from Shin-Etsu Chemical Co., Ltd., model KS-66, and 2 parts of diluent DCAC purchased from Shanghai Tichem Industrial Co., Ltd., mix and disperse at 2000 r / min for 20 min, and grind with a three-roll mill until the main agent particles have a diameter of less than 25 μm.
[0049] Preparation of hardener: 20 parts of polycyclic naphthalene resin HP4032D purchased from DIC Corporation of Japan, 4 parts of latent curing agent MAVT purchased from Shikoku Chemical Industry Co., Ltd. of Japan, and 2 parts of diluent DCAC purchased from Shanghai Tichem Industrial Co., Ltd. were mixed and dispersed at 2000 r / min for 20 minutes, and ground with a three-roll mill until the hardener particle diameter was less than 25 μm.
[0050] The main agent and the hardener prepared above were mixed in a mass ratio of 9:1, and then stirred and dispersed at 2000 r / min for 20 minutes to obtain an alkali-soluble resin composition having a condensed ring naphthalene structure.
[0051] Example 3
[0052] A method for preparing an alkali-soluble photosensitive resin with a condensed-ring naphthalene structure comprises the following steps:
[0053] First, 1.800 kg of diluent diethylene glycol ethyl ether acetate (DCAC), purchased from Shanghai Tichem Industrial Co., Ltd., was poured into a reactor and heated to 100°C, and 3.000 kg of condensed ring naphthalene epoxy resin HP-5000 (epoxy equivalent 250 g / eq.) produced by Japan DIC, 0.023 kg of inhibitor MEHQ, purchased from Changzhou Yurong Chemical Co., Ltd., and 0.014 kg of catalyst TPP, purchased from Suzhou Jinyuan Fine Chemical Co., Ltd., were poured into the reactor, and the initial product was obtained by stirring at 200 r / min for 30 min.
[0054] Then the temperature was raised to 115° C., and stirring and dispersion was continued at 200 r / min for 16 h. 0.907 kg of acrylic acid was added dropwise at 80 drops / min for reaction. The temperature of the reaction process was controlled at 115° C., and the reaction was carried out for 15 h to obtain an intermediate with an unsaturated double bond.
[0055] Then, 1.200 kg of diluent DCAC was added dropwise to the intermediate having unsaturated double bonds. When the temperature dropped to 98° C., 1.459 kg of methylhexahydrophthalic anhydride was added for reaction. The reaction temperature was controlled at 95° C. and the reaction was carried out for 6 hours to obtain a carboxyl-containing intermediate.
[0056] Finally, 0.006 kg of polymerization inhibitor BHT and 0.300 kg of diluent DCAC were poured into the carboxyl-containing intermediate, and cooling water was added to cool the mixture to 60°C. After the reaction was completed, the material was filtered to obtain an alkali-soluble photosensitive resin having a condensed ring naphthalene structure. The synthesized alkali-soluble photosensitive resin having a condensed ring naphthalene structure had an acid value of 60 mgKOH / g, a double bond equivalent of CEW=690, and a solid content of 62%.
[0057] An alkali-soluble photosensitive resin composition having a condensed ring naphthalene structure, wherein the preparation method thereof comprises the following steps:
[0058] Preparation of the main agent: Weigh 50 parts of the alkali-soluble photosensitive resin prepared in Example 3, 6 parts of a composition of photosensitizers IRGACURE TPO and IRGACURE 819 purchased from IGM RESINS (the mass ratio of IRGACURE TPO: IRGACURE 819 is 3:1), 1 part of a photopolymerizable monomer purchased from Changxing Materials Industry Co., Ltd., model EM265, 19 parts of crystalline silica powder A8 produced by Sibelco (Shanghai) Mining Co., Ltd., 1 part of a defoamer purchased from Shin-Etsu Chemical Co., Ltd., model KS-66, and 5 parts of a diluent DCAC purchased from Shanghai Tichem Industrial Co., Ltd., mix and disperse at 3000 r / min for 15 min, and grind with a three-roll mill until the main agent particle diameter is less than 25 μm.
[0059] Preparation of hardener: 10 parts of polycyclic naphthalene resin HP4710 purchased from DIC Corporation of Japan, 3 parts of latent curing agent 2E4MZ purchased from Shikoku Chemical Industry Co., Ltd. of Japan, and 5 parts of diluent DCAC purchased from Shanghai Tichem Industrial Co., Ltd. were mixed and dispersed at 3000 r / min for 15 min, and ground with a three-roll mill until the hardener particle diameter was less than 25 μm.
[0060] The main agent and the hardener prepared above were mixed in a mass ratio of 8:2, and then stirred and dispersed at 3000 r / min for 15 minutes to obtain an alkali-soluble resin composition having a condensed ring naphthalene structure.
[0061] Example 4
[0062] An alkali-soluble photosensitive resin with a condensed-ring naphthalene structure, the preparation method of which comprises the following steps:
[0063] First, 1.800 kg of diluent diethylene glycol ethyl ether acetate (DCAC), purchased from Shanghai Tichem Industrial Co., Ltd., was poured into a reactor and heated to 95°C, and 3.000 kg of Nippon Chemical Industry's polycyclic naphthalene epoxy resin NC-7300L (epoxy equivalent 210 g / eq.), 0.023 kg of inhibitor BHT, purchased from Changzhou Yurong Chemical Co., Ltd., and 0.014 kg of catalyst TPP, purchased from Suzhou Jinyuan Fine Chemical Co., Ltd., were poured into the reactor, and the initial product was obtained by stirring at 150 r / min for 40 min.
[0064] Then the temperature was raised to 105° C., and stirring and dispersion was continued at 150 r / min for 13 h. 1.247 kg of methacrylic acid was added dropwise at 50 drops / min for reaction. The temperature of the reaction process was controlled at 112° C., and the reaction was carried out for 16 h to obtain an intermediate with an unsaturated double bond.
[0065] Then, 2.1 kg of diluent DCAC was added dropwise to the intermediate having an unsaturated double bond. When the temperature dropped to 100° C., 1.4 kg of hexahydrophthalic anhydride was added for reaction. The reaction temperature was controlled at 105° C. and the reaction was carried out for 4 hours to obtain a carboxyl-containing intermediate.
[0066] Finally, 0.010 kg of polymerization inhibitor BHT and 1.8 kg of diluent DCAC were poured into the carboxyl-containing intermediate, and cooling water was added to cool the mixture to 70°C. After the reaction was completed, the material was filtered to obtain an alkali-soluble photosensitive resin having a condensed ring naphthalene structure. The synthesized alkali-soluble photosensitive resin having a condensed ring naphthalene structure had an acid value of 46 mgKOH / g, a double bond equivalent of CEW=785, and a solid content of 50%.
[0067] An alkali-soluble photosensitive resin composition having a condensed ring naphthalene structure, wherein the preparation method thereof comprises the following steps:
[0068] Preparation of the main agent: Weigh 60 parts of the alkali-soluble photosensitive resin prepared in Example 4, 4 parts of a composition of photosensitizers IRGACURE TPO and IRGACURE 819 purchased from IGM RESINS (the mass ratio of IRGACURE TPO: IRGACURE 819 is 1:1), 3 parts of photopolymerizable monomers purchased from Changxing Materials Industry Co., Ltd., model EM2380, 23.5 parts of crystalline silica powder A8 produced by Sibelco (Shanghai) Mining Co., Ltd., 1.5 parts of defoaming agent purchased from Shin-Etsu Chemical Co., Ltd., model KS-66, and 1 part of diluent DCAC purchased from Shanghai Tichem Industrial Co., Ltd., mix and disperse at 1500r / min for 30min, and grind with a three-roll mill until the main agent particles have a diameter of less than 25μm.
[0069] Preparation of hardener: 5 parts of polycyclic naphthalene resin NC-7300L purchased from Nippon Kayaku, 1 part of latent curing agent 2E4MZ purchased from Shikoku Chemical Industry Co., Ltd., Japan, and 1 part of diluent DCAC purchased from Shanghai Tichem Industrial Co., Ltd. were mixed and dispersed at 1500 r / min for 30 min, and ground with a three-roll mill until the hardener particle diameter was less than 25 μm.
[0070] The main agent and the hardener prepared above were mixed in a mass ratio of 7.5:2.5, and then stirred and dispersed at 1500 r / min for 30 minutes to obtain an alkali-soluble resin composition having a condensed ring naphthalene structure.
[0071] Example 5
[0072] An alkali-soluble photosensitive resin with a condensed-ring naphthalene structure, the preparation method of which comprises the following steps:
[0073] First, 1.750 kg of diluent diethylene glycol ethyl ether acetate (DCAC), purchased from Shanghai Tichem Industrial Co., Ltd., was poured into a reactor and heated to 100°C, and 3.000 kg of condensed ring naphthalene epoxy resin NC-7000L (epoxy equivalent 225 g / eq.) produced by Nippon Chemical Industry Co., Ltd., 0.020 kg of inhibitor BHT, 0.010 kg of inhibitor MEHQ, purchased from Changzhou Yurong Chemical Co., Ltd., and 0.014 kg of catalyst benzylamine, purchased from Suzhou Jinyuan Fine Chemical Co., Ltd., were poured into the reactor and stirred at 200 r / min for 30 min to obtain the initial product.
[0074] Then the temperature was raised to 105° C., and stirring and dispersion was continued at 200 r / min for 12 h. 2.05 kg of cinnamic acid was added at 60 drops / min for reaction. The temperature of the reaction process was controlled at 100° C., and the reaction was carried out for 13 h to obtain an intermediate with an unsaturated double bond.
[0075] Then, 0.60 kg of diluent DCAC was added dropwise to the intermediate having an unsaturated double bond. When the temperature dropped to 100° C., 1.17 kg of maleic anhydride was added for reaction. The reaction temperature was controlled at 100° C. and the reaction was carried out for 6 hours to obtain a carboxyl-containing intermediate.
[0076] Finally, 0.010 kg of polymerization inhibitor BHT and 0.34 kg of diluent DCAC were poured into the carboxyl-containing intermediate, and cooling water was added to cool the mixture to 60°C. After the reaction was completed, the material was filtered to obtain an alkali-soluble photosensitive resin having a condensed ring naphthalene structure. The synthesized alkali-soluble photosensitive resin having a condensed ring naphthalene structure had an acid value of 78 mgKOH / g, a double bond equivalent of CEW=647, and a solid content of 70%.
[0077] An alkali-soluble photosensitive resin composition having a condensed ring naphthalene structure, wherein the preparation method thereof comprises the following steps:
[0078] Preparation of the main agent: Weigh 70 parts of the alkali-soluble photosensitive resin prepared in Example 5, 2 parts of a composition of photosensitizers IRGACURE TPO / IRGACURE 819 and IRGACURE 784 purchased from IGM RESINS (the mass ratio of IRGACURE TPO, IRGACURE 819 and IRGACURE 784 is 3.1:0.1), 3 parts of a photopolymerizable monomer purchased from Changxing Materials Industry Co., Ltd., model EM265, 10 parts of crystalline silica powder A8 produced by Sibelco (Shanghai) Mining Co., Ltd., 2 parts of a defoamer purchased from Shin-Etsu Chemical Co., Ltd., model KS-66, and 2 parts of a diluent DCAC purchased from Shanghai Tichem Industrial Co., Ltd., mix and disperse at 2000 r / min for 30 min, and grind with a three-roll mill until the main agent particles have a diameter of less than 25 μm.
[0079] Preparation of hardener: 9 parts of polycyclic naphthalene resin HP5000 purchased from DIC Corporation of Japan, 1 part of latent curing agent 2E4MZ purchased from Shikoku Chemical Industry Co., Ltd. of Japan, and 1 part of diluent DCAC purchased from Shanghai Tichem Industrial Co., Ltd. were mixed and dispersed at 2000 r / min for 30 min, and ground with a three-roll mill until the hardener particle diameter was less than 25 μm.
[0080] The main agent and the hardener prepared above were mixed in a mass ratio of 8.5:1.5, and then stirred and dispersed at 2000 r / min for 30 minutes to obtain an alkali-soluble resin composition having a condensed ring naphthalene structure.
[0081] Comparative Example 1
[0082] An alkali-soluble photosensitive resin composition, the preparation method of which comprises the following steps:
[0083] Preparation of the main agent: 30 parts of alkali-soluble photosensitive resin CCP-4959HW with o-cresol structure produced by Huayao (Wuxi) Chemical, 10 parts of a composition of photosensitizers IRGACURE 907 and IRGACURE ITX-P purchased from IGM RESINS (the mass ratio of IRGACURE 907 to IRGACURE ITX-P is 3:1), 3 parts of photopolymer monomer EM265 purchased from Changxing Materials Industry Co., Ltd., 30 parts of crystalline silica powder A8 produced by Sibelco (Shanghai) Mining Co., Ltd., 0.5 parts of defoamer purchased from Shin-Etsu Chemical Co., Ltd. of Japan, model KS-66 and 4 parts of diluent diethylene glycol ethyl ether acetate (DCAC) were mixed and dispersed at 1500r / min for 30min, and ground with a three-roll mill until the diameter of the main agent particles was less than 25μm.
[0084] Preparation of hardener: 14.5 parts of bisphenol F type Nan Ya resin NPEF-170, 4 parts of latent curing agent melamine and 4 parts of diluent DCAC, purchased from Shanghai Tichem Industrial Co., Ltd., were mixed and dispersed at 1500 r / min for 30 minutes, and ground with a three-roll mill until the hardener particle diameter was less than 25 μm.
[0085] The main agent and the hardener prepared above were mixed in a mass ratio of 7:3, and then stirred and dispersed at 1500 r / min for 30 minutes to obtain an alkali-soluble resin composition having a condensed ring naphthalene structure.
[0086] Comparative Example 2
[0087] An alkali-soluble photosensitive resin composition, the preparation method of which comprises the following steps:
[0088] Preparation of the main agent: 30 parts of alkali-soluble photosensitive resin PR-400CP with bisphenol A structure produced by Shanghai Showa Polymer, 10 parts of a composition of photosensitizers IRGACURE 907 and IRGACURE ITX-P purchased from IGM RESINS (the mass ratio of IRGACURE907 to IRGACURE ITX-P is 3:1), 3 parts of photopolymer monomer EM265, 30 parts of crystalline silica powder A8, 0.5 parts of defoamer KS-66 and 4 parts of diluent diethylene glycol ethyl ether acetate (DCAC) are mixed and dispersed at 1500r / min for 30min, and ground with a three-roll mill until the diameter of the main agent particles is less than 25μm.
[0089] Preparation of hardener: 14.5 parts of bisphenol F type Nan Ya resin NPEF-170, 4 parts of latent curing agent melamine and 4 parts of diluent DCAC were mixed and dispersed at 1500 r / min for 30 minutes, and ground with a three-roll mill until the hardener particle diameter was less than 25 μm.
[0090] The main agent and the hardener prepared above were mixed in a mass ratio of 7:3, and then stirred and dispersed at 1500 r / min for 30 minutes to obtain an alkali-soluble resin composition having a condensed ring naphthalene structure.
[0091] Test example:
[0092] Table 1 shows the performance changes of the prepared resin composition when the double bond equivalent and acid value of the alkali-soluble photosensitive resin with a condensed ring naphthalene structure prepared by the present application are changed. It can be seen from Table 1 that the acid value of the alkali-soluble photosensitive resin with a condensed ring naphthalene structure prepared by the present application is controlled at 30-90 mgKOH / g. If the acid value is too low (< 30 mgKOH / g), it is easy to develop uncleanly and cannot be used; if the acid value is too high (> 90 mgKOH / g), the circuit board will have too much side etching after development, and it is easy to lose oil after surface treatment, and the performance requirements cannot be met. The double bond equivalent of the alkali-soluble photosensitive resin with a condensed ring naphthalene structure prepared by the present application is controlled between 550 and 785. If the double bond equivalent is too low (< 550), the cross-linking reaction is too fast, the shrinkage is too large, and the plugging ink is easy to crack; if the double bond equivalent is too high (> 785), the cross-linking reaction is insufficient, and the plugging and printing are easy to lose oil, and the performance requirements cannot be met.
[0093] Table 1
[0094]
[0095] The alkali-soluble resin compositions having a fused ring structure prepared in Examples 1 to 5 and the alkali-soluble resin compositions prepared in Comparative Examples 1 to 2 were respectively printed on a printed circuit board by screen printing and strip printing, pre-baked at 75° C. for 45 min, dried, and exposed using a Taiwan Zhisheng high-pressure mercury lamp exposure machine (UVE-M720) with a power setting of 7 KW and an energy control range of 200 to 400 mJ / cm 2After developing with 1wt% sodium carbonate solution, heat curing at 150℃ for 60min, a finished circuit board containing solder mask and plugging ink was prepared, and then the finished circuit board was subjected to a thermal shock test at 288℃*10sec*1-3cycle to observe whether the plugging ink cracked. The heat-cured circuit board was parked for 24h and 48h and then subjected to a thermal shock test (288℃*10sec*3cycle) to observe whether the plugging ink cracked; at the same time, a terminal SMT furnace 1-3cycle test was simulated to observe whether the plugging ink cracked. The test results are shown in Table 2. As shown in Table 2, the thermal shock test of the ink at the plug hole position after the plugging tape printing of Comparative Examples 1 to 2 is OK at 288℃*10sec*1cycle, and the test of IR furnace 1cycle is OK, which can meet the use of some processes of some circuit board factories, but many circuit board factories need 2 or even 3 rework thermal shocks, and the terminal patch SMT will also involve rework and furnace 2 or even 3 times, at this time, Comparative Examples 1 to 2 cannot meet the requirements; in addition, after the solder mask is produced in most circuit board processes, there will be parking time before the thermal shock due to production scheduling, and Comparative Examples 1 to 2 cannot meet the parking requirements, and can only be baked and sprayed (thermal shock) operations, and the applicability is very narrow, and most customers cannot use it. The resin composition prepared by using Examples 1 to 5 of the present invention can meet the requirement that the ink at the plug hole position after the plugging tape printing on the circuit board site does not crack, and can not only be printed with plugging tape, but also meet the use of customers with different on-site conditions, and the applicability is very wide.
[0096] Table 2
[0097]
[0098] Note: If there is no cracking of ink at the plug hole position in the above test, it will be judged as OK, and if there is cracking, it will be judged as NG.
[0099] The alkali-soluble resin composition with a condensed ring structure prepared in Example 1 was subjected to a thermal shock test after thermal curing. The results of the plugging ink test were as follows: Figure 1 The resin prepared in comparative example 1 has the following effect on the ink plugging after the thermal shock test: Figure 2 As shown. Figure 1 The two bright edges in the picture are the edges of the circuit board hole rings. There are no cavitation cracking problems in the holes. The test results are OK, and there is no cracking in the ink at the plugging position. Figure 2 The test results of the high temperature heating of the ink in the hole after the plug printing operation of the alkali-soluble photosensitive resin composition prepared in Comparative Example 1 of the present invention. The two bright edges in the picture are the edges of the circuit board hole ring, and the dark cracks in the hole are caused by cavitation cracking and other problems. The test result is NG, and the plug ink is cracked.
[0100] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A composition containing an alkali-soluble photosensitive resin, characterized in that: The composition comprises a main agent and a hardener; the main agent comprises the following components in parts by weight: 30-70 parts of an alkali-soluble photosensitive resin having a condensed ring naphthalene structure, 2-10 parts of a photosensitizer, 1-3 parts of a photopolymerizable monomer, 10-30 parts of a filler, 0.5-2 parts of a defoaming agent, and 1-5 parts of a diluent; the hardener comprises the following components in parts by weight: 5-20 parts of an epoxy resin having a condensed ring naphthalene structure, 1-4 parts of a latent curing agent, and 1-5 parts of a diluent; the mass ratio of the main agent to the hardener is (7-9):(1-3); The preparation method of the alkali-soluble photosensitive resin having a condensed-ring naphthalene structure comprises the following steps: (1) adding a diluent into a reaction kettle, heating it, and then sequentially adding an epoxy resin having a condensed ring naphthalene structure, a catalyst, and a polymerization inhibitor, stirring to obtain an initial product; (2) heating to a first reaction temperature, stirring and dispersing, and then adding an unsaturated carboxylic acid to the initial product prepared in step (1) to react and obtain an intermediate having an unsaturated double bond; (3) adding a diluent to the intermediate having an unsaturated double bond prepared in step (2), lowering the temperature to a second reaction temperature, and adding an acid anhydride to react to obtain a carboxyl-containing intermediate; (4) adding a polymerization inhibitor and a diluent to the carboxyl-containing intermediate prepared in step (3), cooling the mixture to 60-70° C., and filtering the mixture to obtain an alkali-soluble photosensitive resin having a condensed ring naphthalene structure; The double bond equivalent of the alkali-soluble photosensitive resin having a condensed-ring naphthalene structure is CEW=550-785, and the solid content is 50-70wt%.
2. The composition containing an alkali-soluble photosensitive resin according to claim 1, characterized in that: The diluents in steps (1), (3) and (4) are all diethylene glycol ethyl ether acetate; the inhibitors in steps (1) and (4) are all one or more of HQ, THQ, MEHQ and BHT.
3. The alkali-soluble photosensitive resin according to claim 1, characterized in that: In step (1), the heating refers to heating to 95-100° C.; the epoxy resin with a condensed naphthalene structure is purchased from DIC Corporation of Japan, and the model is one or more of HP-4032, HP-4032D, HP-4710, HP-4770, HP-5000, HP-7200, and HP-7200H; or, the epoxy resin with a condensed naphthalene structure is purchased from Nippon Kayaku Co., Ltd., and the model is one or more of NC-7000L and NC-7300L.
4. The composition containing an alkali-soluble photosensitive resin according to claim 1, characterized in that: In step (1), the catalyst is one or more of triphenylphosphine and benzylamine; the mass ratio of the diluent to the epoxy resin with a condensed ring naphthalene structure is (0.5-0.6):1; the mass ratio of the catalyst to the epoxy resin with a condensed ring naphthalene structure is (0.003-0.005):1; the mass ratio of the inhibitor to the epoxy resin with a condensed ring naphthalene structure is (0.006-0.01):1; the stirring speed is 150-200 r / min, and the time is 30-40 min.
5. The composition containing an alkali-soluble photosensitive resin according to claim 1, characterized in that: In step (2), the first reaction temperature is 110±5°C; the stirring speed is 150-200 r / min, and the time is 12-16h; the unsaturated carboxylic acid is one or more of acrylic acid, methacrylic acid, cinnamic acid, methylcinnamic acid, methylcinnamic acid isomers, oleic acid, and elaidic acid; the molar ratio of the carboxyl group in the unsaturated carboxylic acid to the epoxy group of the epoxy resin with a condensed ring naphthalene structure is (1.01-1.05):1; the unsaturated carboxylic acid is added by dropwise addition, and the dropwise addition speed is 50-100 drops / min; the reaction conditions are: controlling the reaction temperature to 110±5°C and reacting for 12-16h.
6. The composition containing an alkali-soluble photosensitive resin according to claim 1, characterized in that: In step (3), the mass ratio of the diluent to the epoxy resin with a condensed ring naphthalene structure is (0.2-0.7):1; the second reaction temperature is 95-100°C; the acid anhydride is one or more of tetrahydrophthalic anhydride, hexahydrophthalic anhydride, and maleic anhydride; the molar ratio of the acid anhydride to the epoxy group of the epoxy resin with a condensed ring naphthalene structure is (0.34-0.9):1; the reaction conditions are: controlling the reaction temperature to 100±5°C and reacting for 4-6h.
7. The composition containing an alkali-soluble photosensitive resin according to claim 1, characterized in that: In step (4), the mass ratio of the diluent to the epoxy resin with a condensed naphthalene structure is (0.1-0.6):1; the mass ratio of the polymerization inhibitor to the epoxy resin with a condensed naphthalene structure is (0.002-0.004):
1.
8. The composition containing an alkali-soluble photosensitive resin according to claim 1, characterized in that: The photosensitizer is purchased from IGM RESINS, and the model is one or more of IRGACURE 907, IRGACURE 369, IRGACURE 184, IRGACURE ITX-P, IRGACURE TPO, IRGACURE 819, and IRGACURE 784; the photopolymerizable monomer is purchased from Changxing Materials Industry Co., Ltd., and the model is one or more of EM 235, EM 241, EM 242, EM2380, EM265, EM266, and EM267; the filler is crystalline silicon micropowder produced by Sibelco (Shanghai) Mining Co., Ltd., and the model is A8; the defoamer is an organosilicon defoamer purchased from Shin-Etsu Chemical Co., Ltd. of Japan, and the model is KS-66; the diluent is diethylene glycol ethyl ether acetate purchased from Shanghai Tichem Industrial Co., Ltd.; the epoxy resin with a condensed ring naphthalene structure is purchased from DIC Corporation of Japan, and the model is HP-4032 , HP-4032D, HP-4710, HP-4770, HP-5000, HP-7200, HP-7200H or one or more thereof; or, the epoxy resin with condensed ring naphthalene structure is purchased from Nippon Kayaku Co., Ltd., and the model is one or more of NC-7000L and NC-7300L; the latent curing agent is purchased from melamine of Nanjing Meikai Technology Co., Ltd. or Japan Shikoku Chemical Industry Co., Ltd., and the model is one or more of MAVT and 2E4MZ.
9. A method for preparing a composition containing an alkali-soluble photosensitive resin according to claim 1, characterized in that: The preparation method comprises the following steps: (1) Preparation of the main agent: according to weight, 30-70 parts of alkali-soluble photosensitive resin with condensed ring naphthalene structure, 2-10 parts of photosensitizer, 1-3 parts of photopolymerizable monomer, 10-30 parts of filler, 0.5-2 parts of defoamer and 1-5 parts of diluent are mixed and dispersed, and then ground until the particle diameter of the main agent is less than 25 μm, and set aside; (2) Preparation of hardener: Mix and disperse 5-20 parts of epoxy resin with condensed ring naphthalene structure, 1-4 parts of latent curing agent and 1-5 parts of diluent by weight, grind until the curing agent particles have a diameter of less than 25 μm, and set aside; (3) mixing the main agent prepared in step (1) and the hardener prepared in step (2) in a mass ratio of (7-9):(1-3), and stirring to obtain an alkali-soluble photosensitive resin composition; The dispersing speeds in step (1) and step (2) are both 1500-3000 r / min, and the dispersing time is both 15-30 min; the grinding is performed in a three-roll mill; the stirring speed in step (3) is 1500-3000 r / min, and the time is 15-30 min.