A molybdenum phosphide-based polycrystalline block and its preparation method and application

Through solid phase reaction and pressurized sintering simplified processes, molybdenum phosphide-based polycrystalline blocks are prepared, which solves the problems of complex processes and high costs in the prior art, and achieves efficient electrocatalytic performance and environmentally friendly self-supporting working electrodes.

CN113649035BActive Publication Date: 2024-11-12WUHAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010349462.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-04-28
Publication Date
2024-11-12
Estimated Expiration
2040-04-28

AI Technical Summary

Technical Problem

The prior art has complicated processes when preparing non-precious metal catalysts. High-temperature phosphating treatment requires toxic gases, and the prepared MoP materials require conductive adhesives to combine with working electrodes, which is costly and affects environmental protection.

Method used

The single raw materials are used to directly prepare molybdenum phosphide-based polycrystalline blocks through solid phase reaction and pressurized sintering, simplifying the process, reducing costs, and realizing self-supporting working electrodes.

Benefits of technology

The prepared molybdenum phosphide-based polycrystalline block has excellent electrocatalytic properties. When the current density is 10mAcm-2, the overpotentials of the hydrogen evolution and oxygen evolution process reach 205mV and 213mV respectively. It has a high conductivity and is suitable for large-scale production and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113649035B_ABST
    Figure CN113649035B_ABST
Patent Text Reader

Abstract

The present invention discloses a molybdenum phosphide-based polycrystalline block and a preparation method and application thereof, the method comprising: using a single substance as a raw material, preparing a MoP 1‑y Or Mo 1‑x A x P 1‑y B y , weigh and mix the reactants in a stoichiometric ratio to obtain reactants; wherein A is a doping element at the Mo lattice position, including one or more of Nb, Fe, Co, and Ni elements, B is a doping element at the P lattice position, including one or more of S, Se, and Te elements, x and y are the contents of the doping elements, x=0-0.06, y=0-0.07; then a polycrystalline powder product is obtained by solid phase reaction under vacuum or inert conditions, and then pressure sintering is performed. The present invention directly prepares the product from single-element raw materials through two steps of solid phase reaction and pressure sintering, has no by-products, has simple equipment and process, is environmentally friendly, and has low cost. It can be directly used as a working electrode for electrocatalytic hydrogen and oxygen evolution without subsequent treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water electrolysis and electrocatalytic hydrogen evolution in the chlor-alkali industry, and in particular to a molybdenum phosphide-based polycrystalline block and a preparation method and application thereof. Background Art

[0002] Hydrogen energy has significant advantages such as cleanliness, zero emission, and high combustion calorific value. Its energy density is as high as 142500KJ / mol, which is three times the energy density of gasoline (46100KJ / mol). It is the next generation of new energy. Hydrogen is an extremely important industrial raw material. It is widely used in petrochemical, electronic industry, metallurgical industry, food processing, new energy vehicles, aerospace, medical and other fields. Its uses are extremely broad. At present, the industrial production of hydrogen mainly includes hydrogen production from fossil raw materials reforming, hydrogen production from methane / methanol catalytic thermal decomposition, hydrogen production from biomass, and hydrogen production from water electrolysis. Hydrogen production from fossil raw materials reforming and hydrogen production from methane / methanol catalytic thermal decomposition are the main ways of large-scale hydrogen production. Their disadvantages are that they consume fossil raw materials and emit greenhouse gas CO2; the efficiency of hydrogen production from biomass is relatively low. Relatively speaking, water electrolysis can not only produce hydrogen but also oxygen, and produce high-purity hydrogen and oxygen with important uses. It is an environmentally friendly, efficient and cost-effective preparation method; currently this method produces 5% of high-purity hydrogen in industry. However, the current industrial production of hydrogen and oxygen by water electrolysis relies on expensive and extremely low reserves of precious metals as catalysts (such as Pt, Ru and Ir, etc.). Therefore, the development of efficient non-precious metal hydrogen and oxygen evolution catalysts is of great significance to the development of the water electrolysis industry.

[0003] The development of non-precious metal hydrogen and oxygen evolution catalysts has been an important topic in electrocatalysis research in recent years. One of the important goals is to obtain catalysts with low overpotential. At present, Pt / C precious metal and RuO2 / C precious metal are commercial hydrogen evolution catalysts and oxygen evolution catalysts, respectively. They have a current density of 10mAcm -2The overpotentials are ~50meV and ~300meV, respectively. In order to improve the catalytic performance of electrochemical catalysts, researchers currently generally use chemical synthesis methods based on hydrothermal synthesis to construct nanostructured catalysts, which aims to increase the surface area and expose more electrocatalytic active sites, which can effectively reduce the overpotential of hydrogen and oxygen evolution catalysts. Hexagonal MoP materials are an important class of non-precious metal electrochemical hydrogen and oxygen evolution catalysts. At present, MoP as an electrocatalytic material focuses on the preparation of nanostructured MoP and its electrocatalytic performance, but there is no report on the direct use of MoP bulk as an electrocatalytic material. For example, Chinese invention patent CN104988536B discloses "a method for preparing a high-performance molybdenum-based hydrogen evolution electrode from a phosphating molybdate precursor". This method involves cleaning the surface of a nickel foam substrate, using molybdate and the like as reactants, and in-situ growing a molybdate nano-precursor on the surface of the nickel foam by hydrothermal synthesis and high-temperature heat treatment in a reducing atmosphere. Finally, the molybdate precursor is subjected to high-temperature phosphating treatment in a H2 reducing atmosphere with phosphite, elemental phosphorus, etc. as a phosphorus source, to ultimately prepare a nanostructured high-performance molybdenum-based hydrogen evolution electrode; the highly conductive nickel foam substrate is used as the working electrode for hydrogen and oxygen evolution reactions. For example, Chinese invention patent application CN107999105A discloses "a method for preparing a molybdenum phosphide hydrogen evolution catalyst having a rod-shaped porous morphology structure". This method uses soluble ammonium molybdate and ammonium dihydrogen phosphate as starting materials and absorbent cotton as a soft film plate, obtains a molybdenum phosphide precursor through drying and high-temperature treatment, and finally obtains a molybdenum phosphide hydrogen evolution catalyst having a rod-shaped porous morphology structure through high-temperature reduction treatment; this method prepares the molybdenum phosphide hydrogen evolution catalyst as a powder, and needs to use a conductive binder to disperse MoP on a highly conductive nickel substrate, graphite carbon or other working electrode for hydrogen and oxygen evolution reactions.

[0004] The above chemical synthesis method prepares MoP materials with specific micro-nano structures mainly through solvent thermal reaction to prepare molybdenum oxide / molybdenum salt precursors, and then performs high-temperature phosphating reaction in a reducing atmosphere to prepare MoP-based materials: its synthesis process involves solvent thermal reaction, cleaning, drying, high-temperature heat treatment in a reducing atmosphere and phosphating reaction and other multi-step reactions, the process is complicated, and the controllable preparation is difficult; at the same time, high-temperature phosphating treatment requires the use of H2, PH3 and elemental phosphorus sources, and the synthesis process discharges toxic wastewater and waste residues, as well as toxic / hazardous gases such as NH3, PH3, and H2 that are not completely reacted. In addition, if the prepared MoP material is not grown in situ on the surface of the working electrode, a conductive binder must be used to achieve the combination of MoP and the working electrode before it can be finally used for hydrogen and oxygen evolution reactions. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a molybdenum phosphide-based polycrystalline block and its preparation method and application. The present invention directly prepares the molybdenum phosphide-based polycrystalline block from a single raw material through solid phase reaction and pressure sintering in two steps, without by-products, and has the advantages of simple equipment and process, low production cost, suitable for large-scale production, and environmental protection. In addition, the molybdenum phosphide-based polycrystalline block prepared by this process has excellent electrocatalytic performance: the current density is 10mAcm -2 The overpotentials of hydrogen and oxygen evolution processes are 205 mV and 213 mV, respectively; in addition, the dense molybdenum phosphide-based polycrystalline bulk has a high electrical conductivity equivalent to that of working electrodes such as metallic nickel and carbon materials, and can be directly used as a self-supporting working electrode for electrocatalytic hydrogen and oxygen evolution without subsequent treatment.

[0006] The present invention is achieved in that:

[0007] One of the purposes of the present invention is to provide a method for preparing a molybdenum phosphide-based polycrystalline block, the preparation method comprising:

[0008] Step 1: Use single substance as raw material, according to MoP 1-y Or Mo 1-x A x P 1-y B y , weighing and mixing in a stoichiometric ratio to obtain a reactant; wherein A is a doping element at a Mo lattice position, including one or more of Nb, Fe, Co, and Ni; B is a doping element at a P lattice position, including one or more of S, Se, and Te; x and y are the contents of the doping element, x=0 to 0.06, y=0 to 0.07;

[0009] Step 2: subjecting the reactants to solid phase reaction under vacuum or inert conditions to obtain Mo 1-x A x P 1-y B y Polycrystalline powdery product;

[0010] Step 3: 1-x A x P 1-y B y The polycrystalline powder product is sintered under pressure to obtain Mo 1-x A x P 1-y B y Polycrystalline bulk material.

[0011] The reason why x is controlled within the range of 0 to 0.06 and y is controlled within the range of 0 to 0.07 is to avoid affecting the intrinsic electrocatalytic properties of MoP and to obtain a highly dense sintered block. As shown in Table 1, when x is greater than 0.06 and y is greater than 0.07, Mo1-x A x P 1-y B y The density and conductivity of polycrystalline bulk may be too low, affecting its ability to serve as an in-situ working electrode for electrocatalytic reactions.

[0012] Preferably, the inert condition is a sealed container or a vacuum environment with an inert gas, and the inert gas includes H2 and Ar. A small amount of the inert gas is sufficient, and there is no limit to the amount of the inert gas, which is mainly to prevent the material from being oxidized or nitrided under high temperature conditions.

[0013] Preferably, the temperature of the solid phase reaction is 700°C to 800°C (more preferably 700°C to 750°C); the time of the solid phase reaction is 40h to 55h. The range of the solid phase reaction temperature and the solid phase reaction time is to allow the reaction between the constituent elements to proceed smoothly. As described in Experimental Example 2, if the temperature of the solid phase reaction is lower than 700°C, the reaction between the constituent elements is difficult to proceed completely.

[0014] Preferably, the pressure sintering is hot pressing sintering or plasma sintering.

[0015] Preferably, the process of pressure sintering is: sintering temperature is 850℃~950℃, sintering pressure is 40MPa~80MPa, and sintering time is 10min~60min. According to the Mo-P binary phase diagram, when the temperature is higher than 950℃, MoP may decompose. In theory, the higher the sintering temperature and the greater the sintering pressure, the higher the density of the sintered product. However, the sintering mold is generally made of graphite, and it is difficult to apply a pressure of more than 80MPa. Under the pressure sintering process, high-density Mo can be stably obtained. 1-x A x P 1-y B y Polycrystalline blocks with a density of more than 80% and an electrical conductivity higher than 1×10 6 S / m (as described in Table 1).

[0016] The second object of the present invention is to provide a molybdenum phosphide-based polycrystalline block prepared by the method.

[0017] The third object of the present invention is to provide the use of the molybdenum phosphide-based polycrystalline block as a self-supporting working electrode for electrocatalytic hydrogen and oxygen evolution.

[0018] Compared with the prior art, the present invention has the following advantages and effects:

[0019] 1. The present invention provides a method for preparing a molybdenum phosphide-based polycrystalline block. For the first time, a MoP-based polycrystalline block material is prepared by combining a solid-phase reaction with heating and sintering. It has no by-products and has the advantages of simple equipment and process, low production cost, suitability for large-scale production, and environmental protection. It mainly uses single-element Mo powder, P powder, Nb powder, Se powder, Te powder, etc., which are rich in sources and have low raw material costs.

[0020] 2. The present invention provides a molybdenum phosphide-based polycrystalline block with an electrical conductivity of 10 6 S / m level, with an electrical conductivity equivalent to that of working electrodes such as metallic nickel and carbon materials, and can be directly used as a self-supporting working electrode for electrocatalytic hydrogen and oxygen evolution without subsequent treatment.

[0021] 3. The molybdenum phosphide-based polycrystalline block provided by the present invention has excellent electrocatalytic performance: the current density is 10 mA cm -2 The overpotentials of hydrogen and oxygen evolution processes reached 205mV and 213mV respectively. The molybdenum phosphide-based polycrystalline block as a whole is used as a working electrode and catalyst, and its stability is significantly improved. It can be widely used in water electrolysis and chlor-alkali industry electrocatalytic hydrogen evolution. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Shown is the XRD spectrum of the MoP powder after solid phase reaction and plasma activated sintering in Example 1;

[0023] Figure 2 Shown is the SEM image of the MoP powder after solid phase reaction in Example 1;

[0024] Figure 3 Shown is a cross-sectional SEM image of the MoP plasma activated sintered block in Example 1;

[0025] Figure 4 The figure shows the hydrogen evolution overpotential of the MoP polycrystalline bulk in an alkaline environment (1M KOH) in Example 1; the hydrogen evolution overpotential of the Pt / C electrode under the same conditions is listed for comparison;

[0026] Figure 5 The figure shows the oxygen evolution overpotential of the MoP polycrystalline bulk in an alkaline environment (1M KOH) in Example 1; the oxygen evolution overpotential of the RuO2 / Ni electrode under the same conditions is listed for comparison;

[0027] Figure 6 Shown is the MoP in Examples 1-5 1-y (y=0~0.07) Powder XRD pattern of sintered polycrystalline block;

[0028] Figure 7 Mo in Examples 6-8 is shown 1-x Nb xPowder XRD pattern of sintered polycrystalline block of P (x = 0 ~ 0.06);

[0029] Figure 8 Shown is the MoP in Examples 9-10 1-y Se y (y=0~0.02) Powder XRD pattern of sintered polycrystalline block;

[0030] Fig. 9 Shown is the MoP in Examples 11-12 1-y Te y (y=0~0.02) Powder XRD spectrum of sintered polycrystalline block.

[0031] Fig.10 Shown are the powder XRD spectra of MoP after solid phase reaction at different temperatures in Experimental Example 2. DETAILED DESCRIPTION

[0032] Example 1

[0033] This embodiment provides a method for preparing a MoP polycrystalline block by solid phase reaction combined with plasma activated sintering, which comprises the following steps:

[0034] 1) Using Mo powder and P powder with a purity of 99.9% as raw materials, weighing and grinding and mixing them uniformly according to the MoP stoichiometric ratio to obtain a reactant;

[0035] 2) The reactant obtained in step 1) is pressed into a tablet and vacuum-sealed in a quartz glass tube, and placed in a muffle furnace for reaction at 750° C. for 48 hours to obtain a reaction product;

[0036] 3) The polycrystalline powder product obtained in step 2) is further ground and refined, and then a dense polycrystalline product is obtained by plasma activated sintering at 950° C., 80 MPa and heat preservation for 10 min;

[0037] 4) The surface of the plasma activated sintered MoP polycrystalline block can be directly used for electrochemical hydrogen and oxygen evolution experiments after being polished with 800 mesh sandpaper.

[0038] Figure 1 Shown is the XRD spectrum of MoP powder after solid phase reaction and plasma activated sintering; Figure 2 and Figure 3 The following are the SEM images of the cross section of MoP solid phase reaction powder and plasma activated sintered block, respectively, showing the cross section morphology and dense microstructure of the prepared MoP polycrystalline block; Figure 4 and Figure 5The figures show the overpotentials of hydrogen evolution and oxygen evolution of MoP polycrystalline bulk in alkaline environment (1M KOH, PH=14). The overpotential of hydrogen evolution on Pt / C electrode is 115mV, and the overpotential of oxygen evolution on RuO2 / Ni electrode is 319mV under the same conditions.

[0039] The MoP polycrystalline bulk sintered by plasma activation has a dense structure and a room temperature conductivity of up to 6.74×10 6 S / m (as shown in Table 1), which is comparable to the conductivity of existing working electrodes such as metal nickel and carbon materials. MoP polycrystalline bulk has excellent electrochemical performance, with hydrogen and oxygen evolution overpotentials of 205mV and 213mV@10mAcm, respectively. -2 , can be directly used for electrochemical hydrogen and oxygen evolution without subsequent treatment.

[0040] Example 2

[0041] This embodiment provides a MoP 1-y A method for preparing a polycrystalline block by solid phase reaction combined with plasma activated sintering comprises the following steps:

[0042] 1) Using 99.9% pure Mo powder and P powder as raw materials, according to MoP 1-y (y=0.01) stoichiometric ratio is weighed and ground and mixed to obtain the reactants;

[0043] 2) The reactant obtained in step 1) is pressed into a tablet and vacuum-sealed in a quartz glass tube, and placed in a muffle furnace for reaction at 750° C. for 48 hours to obtain a reaction product;

[0044] 3) The polycrystalline powder product obtained in step 2) is further ground and refined, and then a dense polycrystalline product is obtained by plasma activated sintering at 950° C., 80 MPa and heat preservation for 10 min;

[0045] 4) Plasma activated sintering of MoP 0.99 The surface of the polycrystalline block can be directly used for electrochemical hydrogen and oxygen evolution experiments after being polished with sandpaper.

[0046] Example 3

[0047] This embodiment provides a MoP 1-y Preparation method of polycrystalline block by solid phase reaction combined with plasma activated sintering, according to MoP 0.97 (y=0.03) stoichiometric ratio, and the remaining steps are the same as in Example 2.

[0048] Example 4

[0049] This embodiment provides a MoP 1-y Preparation method of polycrystalline block by solid phase reaction combined with plasma activated sintering, according to MoP0.95 (y=0.05) stoichiometric ratio, and the remaining steps are the same as in Example 2.

[0050] Example 5

[0051] This embodiment provides a MoP 1-y Preparation method of polycrystalline block by solid phase reaction combined with plasma activated sintering, according to MoP 0.93 (y=0.07) stoichiometric ratio, and the remaining steps are the same as in Example 2.

[0052] Example 6

[0053] This embodiment provides a Mo 1-x Nb x The method for preparing a P polycrystalline block by solid phase reaction combined with plasma activated sintering comprises the following steps:

[0054] 1) Using 99.9% pure Mo powder, Nb powder and P powder as raw materials, according to Mo 1-x Nb x P 1-y B y (x=0.02, y=0) stoichiometric ratio is weighed and ground and mixed to obtain a reactant;

[0055] 2) The reactant obtained in step 1) is pressed into a tablet and vacuum-sealed in a quartz glass tube, and placed in a muffle furnace for reaction at 750° C. for 48 hours to obtain a reaction product;

[0056] 3) The polycrystalline powder product obtained in step 2) is further ground and refined, and then a dense polycrystalline product is obtained by plasma activated sintering at 950° C., 80 MPa and heat preservation for 10 min;

[0057] 4) Plasma activated sintering Mo 1-x Nb x The surface of the P polycrystalline block can be directly used for electrochemical hydrogen and oxygen evolution experiments after being polished with sandpaper.

[0058] Example 7

[0059] In this embodiment, except for 1-x Nb x P 1-y B y (x=0.03, y=0) are weighed and ground and mixed evenly to obtain the reactants in a stoichiometric ratio, and the remaining steps are the same as in Example 6.

[0060] Example 8

[0061] In this embodiment, except for 1-x Nb x P 1-y By (x=0.06, y=0) are weighed and ground and mixed evenly to obtain the reactants in a stoichiometric ratio, and the remaining steps are the same as in Example 6.

[0062] Example 9

[0063] This embodiment provides a MoP 1-y Se y A method for preparing a polycrystalline block by solid phase reaction combined with plasma activated sintering comprises the following steps:

[0064] 1) Using 99.9% pure Mo powder, P powder and Se powder as raw materials, 1-x A x P 1-y Se y (x=0, y=0.005) stoichiometric ratio is weighed and ground and mixed to obtain the reactants;

[0065] 2) The reactant obtained in step 1) is pressed into a tablet and vacuum-sealed in a quartz glass tube, and placed in a muffle furnace for reaction at 750° C. for 48 hours to obtain a reaction product;

[0066] 3) The polycrystalline powder product obtained in step 2) is further ground and refined, and then a dense polycrystalline product is obtained by plasma activated sintering at 950° C., 80 MPa and heat preservation for 10 min;

[0067] 4) Plasma activated sintering of MoP 1-y Se y The surface of the polycrystalline block can be directly used for electrochemical hydrogen and oxygen evolution experiments after being polished with sandpaper.

[0068] Example 10

[0069] This embodiment is based on Mo 1-x A x P 1-y Se y (x=0, y=0.02) The reactants were weighed and ground and mixed evenly in a stoichiometric ratio, and the remaining steps were the same as in Example 9.

[0070] Embodiment 11

[0071] This embodiment provides a MoP 1-y Te y A method for preparing a polycrystalline block by solid phase reaction combined with plasma activated sintering comprises the following steps:

[0072] 1) Using 99.9% pure Mo powder, P powder and Te powder as raw materials, 1-x A x P 1-y Te y(x=0, y=0.005) stoichiometric ratio is weighed and ground and mixed to obtain the reactants;

[0073] 2) The reactant obtained in step 1) is pressed into a tablet and vacuum-sealed in a quartz glass tube, and placed in a muffle furnace for reaction at 750° C. for 48 hours to obtain a reaction product;

[0074] 3) The polycrystalline powder product obtained in step 2) is further ground and refined, and then a dense polycrystalline product is obtained by plasma activated sintering at 950° C., 80 MPa and heat preservation for 10 min;

[0075] 4) Plasma activated sintering of MoP 1-y Te y The surface of the polycrystalline block can be directly used for electrochemical hydrogen and oxygen evolution experiments after being polished with sandpaper.

[0076] Example 12

[0077] This embodiment is based on Mo 1-x A x P 1-y Te y (x=0, y=0.02) The reactants were weighed and ground and mixed evenly in a stoichiometric ratio, and the remaining steps were the same as in Example 11.

[0078] Experimental Example 1

[0079] The electrical conductivity and density of the molybdenum phosphide-based polycrystalline blocks prepared in Examples 1-12 are statistically shown in Table 1.

[0080] Table 1

[0081] Group Nominal composition <![CDATA[Conductivity (10 6 S / m)]]> Density Example 1 MoP 6.74 93.5% Example 2 <![CDATA[MoP 0.99 ]]> 6.64 93.3% Example 3 <![CDATA[MoP 0.97 ]]> 4.55 93.1% Example 4 <![CDATA[MoP 0.95 ]]> 4.04 90.6% Example 5 <![CDATA[MoP 0.93 ]]> 3.28 85.1% Example 6 <![CDATA[Mo 0.98 Nb 0.02 P]]> 7.22 96.1% Example 7 <![CDATA[Mo 0.97 Nb 0.03 P]]> 6.69 95.7% Example 8 <![CDATA[Mo 0.94 Nb 0.06 P]]> 6.61 94.5% Example 9 <![CDATA[MoP 0.995 With 0.005 ]]> 5.00 90.9% Example 10 <![CDATA[MoP 0.98 With 0.02 ]]> 2.29 82.0% Embodiment 11 <![CDATA[MoP 0.995 The 0.005 ]]> 5.76 91.8% Example 12 <![CDATA[MoP 0.98 The 0.02 ]]> 1.78 85.9%

[0082] From the changing trend of the doping amount affecting density and conductivity in Table 1, it can be seen that increasing the doping amount will greatly reduce the Mo 1-x A x P 1-y By polycrystalline body density and conductivity; in this embodiment, when the selected trace doping amount x = 0 ~ 0.06 and y = 0 ~ 0.07, Mo 1-x A x P 1-y B y The density of the polycrystalline block is higher than 80% and the electrical conductivity is higher than 1×10 6 S / m, it can be used as a catalyst for electrocatalytic reactions and as an in-situ working electrode without the assistance of an external working electrode. The range of x and y selected in this experimental example is Mo 1-x A x P 1-y B yThe polycrystalline block can be applied within a range of doping amounts to avoid excessively high doping amounts causing low density and conductivity and affecting its ability to serve as an in-situ working electrode.

[0083] Figure 6 MoP of Examples 1-5 1-y (y=0~0.07) Powder XRD spectrum of plasma activated sintering products. When P deficiency reaches y=0.05 or above, MoP 1-y The Mo impurity phase appears in the polycrystalline block, and its density and conductivity are significantly reduced (as shown in Table 1), but its conductivity remains at 3×10 6 S / m and above.

[0084] Figure 7 Mo of Example 6-8 1-x Nb x Powder XRD spectrum of plasma activated sintering products of P (x = 0 ~ 0.06). When Nb doping exceeds x = 0.02, Mo 1-x Nb x NbP impurity phase appears in the P polycrystalline bulk, while the overall conductivity remains unchanged (as shown in Table 1), up to 6-7×10 6 S / m.

[0085] Figure 8 MoP of Examples 9-10 1-y Se y (y=0~0.02) Powder XRD pattern of plasma activated sintering product. After Se doping, MoP 1-y Se y The polycrystalline block is a single phase, and the density and conductivity are significantly reduced (as shown in Table 1), but still as high as 2.29×10 6 S / m and above.

[0086] Fig. 9 MoP of Example 11-12 1-y Te y (y=0~0.02) Powder XRD pattern of plasma activated sintering product. After Te doping, MoP 1-y Te y The polycrystalline block is a single phase, and the density and conductivity are significantly reduced (as shown in Table 1), but still as high as 1.78×10 6 S / m and above.

[0087] Experimental Example 2 Exploration of solid phase reaction temperature

[0088] The XRD patterns of MoP powders after solid phase reaction at different temperatures (650℃, 700℃, 750℃) are shown in Figure 2. Fig.10 shown.

[0089] Depend on Fig.10It can be seen that when the solid phase reaction time is 40h to 55h, the solid phase reaction temperature is lower than 700 degrees, which will lead to incomplete reaction of Mo and P, and the product contains a large amount of MoP2 and Mo impurities. Therefore, in order to achieve complete reaction of single elements in the solid phase reaction and save energy, the present invention will Mo 1-x A x P 1-y B y The solid phase reaction temperature is controlled in the range of 700°C to 800°C.

[0090] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. Use of a molybdenum phosphide-based polycrystalline block as a self-supporting working electrode for electrocatalytic hydrogen and oxygen evolution, characterized in that: The method for preparing the molybdenum phosphide-based polycrystalline block comprises the following steps: Step 1: Use single substance as raw material, according to MoP 1-y The reactants are weighed and mixed uniformly in a stoichiometric ratio to obtain reactants; wherein y = 0 to 0.01; Step 2: subjecting the reactants to solid phase reaction under vacuum or inert conditions to obtain MoP 1-y A polycrystalline powder product; wherein the temperature of the solid phase reaction is 700°C to 800°C, and the time of the solid phase reaction is 40h to 55h; Step 3: 1-y The polycrystalline powder product is sintered under pressure to obtain MoP 1-y The polycrystalline block material is a molybdenum phosphide-based polycrystalline block; wherein the pressure sintering process is as follows: the sintering temperature is 850°C to 950°C, the sintering pressure is 40MPa to 80MPa, and the sintering time is 10min to 60min.

2. Use of a molybdenum phosphide-based polycrystalline block as a self-supporting working electrode for electrocatalytic hydrogen and oxygen evolution, characterized in that: The method for preparing the molybdenum phosphide-based polycrystalline block comprises the following steps: Step 1: Use single substance as raw material, press Mo 1-x Nb x P are weighed and mixed uniformly to obtain a reactant; wherein Nb is a doping element at the Mo lattice position, and x is 0.02 to 0.06; Step 2: subjecting the reactants to solid phase reaction under vacuum or inert conditions to obtain Mo 1-x Nb x P polycrystalline powder product; wherein the temperature of the solid phase reaction is 700°C to 800°C, and the time of the solid phase reaction is 40h to 55h; Step 3: 1-x Nb x The polycrystalline powder product of P is sintered under pressure to obtain Mo 1-x Nb x P polycrystalline block material, that is, molybdenum phosphide-based polycrystalline block; wherein the pressure sintering process is: sintering temperature is 850°C to 950°C, sintering pressure is 40MPa to 80MPa, and sintering time is 10min to 60min.

3. The use of the molybdenum phosphide-based polycrystalline block as claimed in claim 1 as a self-supporting working electrode for electrocatalytic hydrogen and oxygen evolution, characterized in that: The simple substance is in powder form, and the reactant is in powder form or is pressed into an ingot.

4. Use of the molybdenum phosphide-based polycrystalline block as claimed in claim 1 as a self-supporting working electrode for electrocatalytic hydrogen and oxygen evolution, characterized in that: The inert condition is a sealed container with an inert gas, and the inert gas includes H2 and Ar.

5. Use of the molybdenum phosphide-based polycrystalline block as claimed in claim 1 as a self-supporting working electrode for electrocatalytic hydrogen and oxygen evolution, characterized in that: The pressure sintering is selected from hot pressing sintering or plasma sintering.