A Cap layer etching optimization method
By performing ohmic contact photolithography and dry etching on the Cap layer of the VCSEL chip, it is ensured that the metal is in close contact with the edge of the photoresist, which solves the gap problem during metal deposition and improves the optoelectronic characteristics and reliability of the chip.
Patent Information
- Application Number
- CN202110793446.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-14
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-07-14
AI Technical Summary
During the preparation process of the VCSEL chip, the Cap layer layer and the edge of the optical film cannot be closely attached during metal deposition, causing the SN830 solution to etch the Cap layer layer during cleaning, affecting the optoelectronic characteristics and reliability of the chip.
By performing ohmic contact photolithography on the Cap layer of the epitaxial wafer, the photoresist edge has an inclination angle, and dry etching and ohmic contact metal deposition are used to ensure that the metal is in close contact with the photoresist edge and avoid the SN830 solution from entering the gap. .
It achieves a close fit between metal and photoresist, avoids etching of the Cap layer, improves the performance and reliability of the chip, and increases the selection ratio and flexibility in controlling the etching angle.
Smart Images

Figure CN113675722B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chip preparation, and in particular to a Cap layer etching optimization method. Background Art
[0002] VCSEL chips are made by using epitaxial wafers as the base wafer and carrying out corresponding process flow on the epitaxial wafers. The epitaxial wafers are composed of Cap layer, P-DBR, N-DBR, oxide layer, quantum well and substrate. Damage to any layer will affect the reliability or optoelectronic properties of the chip.
[0003] During the preparation of VCSEL chips, after the optical film deposition, photolithography, etching and metal deposition steps are performed on the Cap layer of the epitaxial wafer, the epitaxial wafer needs to be cleaned with SN830 solution to remove the photoresist remaining on the epitaxial wafer. Among them, the photolithography process is to remove part of the photoresist to expose the optical film; the etching step is to remove the optical film at the photolithography position so that the metal after the metal deposition step is in direct contact with the Cap layer. However, during the metal deposition step, the edge metal deposited on the Cap layer cannot fit tightly with the optical film, and there will be a certain gap (such as Figure 1 When the residual photoresist is cleaned with SN830 solution, the SN830 solution can easily penetrate into the Cap layer from the gap, dissolve part of the Cap layer, and cause certain damage to the Cap layer, which ultimately affects the optoelectronic properties and reliability of the chip.
[0004] Therefore, it is urgent to solve the problem that the edge of the optical film cannot fit tightly with the metal during metal deposition, and to find a method to protect the Cap layer from being etched. Summary of the invention
[0005] In view of the above technical problems, the present invention provides a Cap layer etching optimization method, which can make the metal of the chip perfectly fit with the edge of the optical film during metal deposition, thereby avoiding the etching of the Cap layer by the SN830 solution.
[0006] In order to achieve the above object, the technical solution of the present invention is:
[0007] A method for optimizing Cap layer etching includes the following steps:
[0008] S1, prepare the epitaxial wafer with full structure;
[0009] S2, performing warpage compensation processing on the N surface of the epitaxial wafer;
[0010] S3, depositing a layer of optical film on the Cap layer of the P surface of the epitaxial wafer;
[0011] S4, performing ohmic contact photolithography on the epitaxial wafer with the optical film deposited thereon, so that the edge of the photoresist has a tilt angle;
[0012] S5, etching away the optical film outside the coverage of the photoresist by dry etching;
[0013] S6, performing ohmic contact metal deposition, depositing the metal in the etched area, so that the deposited metal is in close contact with the inclination angle of the edge of the photoresist and the Cap layer;
[0014] S7. Use SN830 solution to remove the photoresist.
[0015] With the above solution, since the metal slowly changes from liquid to solid during metal deposition, the edge of the photoresist is tilted to a certain extent, and the liquid metal is deposited downward along the tilt. After the metal solidifies, it will fit tightly with the photoresist without any gaps.
[0016] Further, in step S4, the method of ohmic contact lithography for making the photoresist edge have a tilt angle is as follows:
[0017] S41, using a spin coater to perform a coating process on the epitaxial wafer, so that the thickness of the photoresist is at least 3 um;
[0018] S42, using an exposure machine to perform exposure, wherein the exposure parameters are exposure dose 2500 and focal length 0;
[0019] S43, developing the exposed epitaxial wafer using a developer.
[0020] By adopting the above scheme, in order to make the photoresist have a certain angle after exposure, the coating process is first optimized to ensure a thickness of 3um to ensure that 3000 angstroms are reached during dry etching in step S5; then, by changing the exposure parameters, such as exposure dose, focal length, etc., the photoresist edge tilt effect is achieved.
[0021] Furthermore, in step S4, the method of ohmic contact lithography for making the photoresist edge have a tilt angle is as follows:
[0022] S411, using a spin coater to quickly spin-coat photoresist on the epitaxial wafer at a high rotation speed, so that the photoresist is quickly spread;
[0023] S412, leaving the epitaxial wafer after spin coating a layer of photoresist to stand for 10 seconds;
[0024] S413, using a spin coater to slowly rotate the epitaxial wafer at a low speed to make the photoresist on the epitaxial wafer uniform.
[0025] Using the above scheme, first rotate at high speed to quickly spread the photoresist, and then stand still for 10 seconds to ensure the thickness of the photoresist. The photoresist cannot be too thin, and then rotate slowly to make the thickness of the photoresist on the entire wafer uniform.
[0026] Furthermore, the high speed in step S41 is 3500-4000 r / s.
[0027] Furthermore, the low speed in step S43 is 800-1200 r / s.
[0028] Furthermore, the inclination angle of the edge of the photoresist is 70-80 degrees.
[0029] Furthermore, the warpage compensation method is to grow a layer of stress film, the material of the stress film is SiO2, SiN X or SiO X N y .
[0030] Furthermore, the material of the optical film is a dielectric formed by one or a combination of several of Si, N, O, Al, F, and Mg.
[0031] Furthermore, the metal material used for the metal deposition is one or more of gold, titanium, silver, copper, chromium, manganese and germanium.
[0032] Furthermore, the full-structure epitaxial wafer includes a Cap layer, a P-DBR layer, an oxide layer, a quantum well layer, an N-DBR layer and a substrate from the P surface to the N surface, wherein the substrate is a GaAs single crystal substrate.
[0033] Beneficial effects: The present invention optimizes the photolithography process steps so that the edge of the photoresist after exposure has a certain inclination angle, and the liquid metal is deposited along the inclination angle, so that the deposited metal and the photoresist are closely fitted, avoiding the occurrence of gaps that cause the SN830 solution to enter the gaps and cause etching of the Cap layer, thereby increasing the selectivity, facilitating the control of the etching angle, improving the yield of the chip and protecting the performance of the chip to a great extent. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a SEM image taken when there is a gap between the photoresist and the metal.
[0035] Figure 2 Schematic diagram of the epitaxial wafer structure after glue coating.
[0036] Figure 3 Schematic diagram of the epitaxial wafer structure after ohmic contact lithography.
[0037] Figure 4Schematic diagram of the epitaxial wafer structure after metal deposition.
[0038] Figure 5 Schematic diagram of the epitaxial wafer structure after removing the photoresist.
[0039] Figure 6 The figure is a SEM picture of the epitaxial wafer after using the method of the present invention.
[0040] Among them, 1-epitaxial wafer, 2-stress film, 3-cap layer, 4-optical film, 5-photoresist, 6-metal. DETAILED DESCRIPTION
[0041] The embodiments of the present invention will be further described below in conjunction with the accompanying drawings.
[0042] Example: Figure 2-5 As shown, a method for optimizing etching of Cap layer 3 comprises the following steps:
[0043] S1. Prepare a fully structured epitaxial wafer 1; the fully structured epitaxial wafer 1 includes a Cap layer 3, a P-DBR layer, an oxide layer, a quantum well layer, an N-DBR layer and a substrate from the P side to the N side, wherein the substrate is a GaAs single crystal substrate.
[0044] S2, performing warpage compensation processing on the N surface of the epitaxial wafer 1; the warpage compensation method is to grow a layer of stress film 2, the material of the stress film 2 is SiO2, SiN X or SiO X N y The stress film 2 is used to compensate for the warping of the epitaxial wafer, making the epitaxial wafer 1 flat, which is beneficial to the steps of photolithography, metal deposition, etc.
[0045] S3. Depositing an optical film 4 on the Cap layer 3 of the P surface of the epitaxial wafer 1; the material of the optical film is a combination of one or more dielectrics formed by Si, N, O, Al, F, and Mg, and the thickness of the optical film 4 is 3000 angstroms.
[0046] S4, performing ohmic contact photolithography on the epitaxial wafer 1 with the optical film 4 deposited thereon, so that the edge of the photoresist 5 has a tilt angle of 70-80 degrees.
[0047] The method of ohmic contact lithography for making the edge of the photoresist 5 have a tilt angle is as follows:
[0048] S41, using a spin coater to perform a coating process on the epitaxial wafer 1, so that the thickness of the photoresist 5 is at least 3 um;
[0049] The glue coating process steps are as follows:
[0050] S411, using a spin coater to quickly spin-coat the photoresist 5 on the epitaxial wafer 1 at a high speed, so that the photoresist 5 is quickly spread; the high speed is 4000 r / s;
[0051] S412, leaving the epitaxial wafer 1 after spin coating a layer of photoresist 5 to stand for 10 seconds;
[0052] S413, using a spin coater to slowly rotate the epitaxial wafer 1 at a low speed to make the photoresist 5 on the epitaxial wafer 1 uniform; the low speed is 1000 r / s.
[0053] S42, using an exposure machine to perform exposure, the exposure parameters of which are exposure dose 2500 and focal length 0.
[0054] S43, developing the exposed epitaxial wafer 1 using a developer.
[0055] S5 , etching away the optical film 4 outside the coverage of the photoresist 5 by dry etching.
[0056] S6, performing ohmic contact metal deposition, depositing metal 6 in the etched area, so that the deposited metal is in close contact with the inclination angle of the edge of the photoresist 5 and the Cap layer 3; the material of the metal 6 used for the metal deposition is one or more of gold, titanium, silver, copper, chromium, manganese, and germanium.
[0057] S7. Use SN830 solution to remove the photoresist 5.
[0058] In this embodiment, the SN830 solution is used to remove the photoresist 5 with very ideal effect.
[0059] The dry etching is a technology that uses plasma to etch thin films. The chemical activity of these gases in the plasma is much stronger than that in normal conditions. According to the different materials to be etched, by selecting the appropriate gas, it can react with the material faster to achieve the purpose of etching and removal; the electric field can also be used to guide and accelerate the plasma so that it has a certain energy. When it bombards the surface of the etched object, it will knock out the atoms of the etched material, thereby achieving the purpose of etching by physical energy transfer. Therefore, dry etching is the result of a balance between the physical and chemical processes on the surface of the wafer. In this embodiment, the thickness of the dry etching is 3000 angstroms, which just etches the optical film 4 to ensure that the Cap layer is not etched. The electrode pattern formed by dry etching is annular, and the CD value of the annular electrode is about 3.
[0060] Exposure dose focal length CD angle 3000 -1 3 90 2800 -0.5 3.1 84 2500 0 3.15 77
[0061] It can be seen that under the conditions of exposure dose of 2500 and focal length of 0, the angle of epitaxial wafer 1 measured by SEM is 77 degrees, and the CD value of the ring electrode is 3.15, which is also within the normal range. Figure 6 As shown, at this angle, the deposited metal can cover the optical film 4 well, and no phenomenon of the SN830 solution etching the Cap layer 3 is found in the SEM image.
[0062] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention is described in detail with reference to the preferred embodiments, a person skilled in the art should understand that the technical solutions of the invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solutions of the present invention, which should be included in the scope of the claims of the present invention. The techniques, shapes, and structural parts not described in detail in the present invention are all well-known technologies.
Claims
1. A Cap layer etching optimization method, Features: The following steps are involved: S1, prepare the epitaxial wafer with full structure; S2, performing warpage compensation processing on the N surface of the epitaxial wafer; S3, depositing a layer of optical film on the Cap layer of the P surface of the epitaxial wafer; S4, performing ohmic contact photolithography on the epitaxial wafer with the optical film deposited thereon, so that the edge of the photoresist has a tilt angle; S5, etching away the optical film outside the coverage of the photoresist by dry etching; S6, performing ohmic contact metal deposition, depositing the metal in the etched area, so that the deposited metal is in close contact with the inclination angle of the edge of the photoresist and the caplayer layer; S7, removing the photoresist using SN830 solution; In step S4, the method of ohmic contact lithography for making the edge of the photoresist have a tilt angle is as follows: S41, using a spin coater to perform a coating process on the epitaxial wafer, so that the thickness of the photoresist is at least 3 um; S42, using an exposure machine to perform exposure, wherein the exposure parameters are exposure dose 2500 and focal length 0; S43, developing the exposed epitaxial wafer using a developer; In step S6, the liquid metal is deposited downward along the inclination angle of the edge of the photoresist, and the metal is closely attached to the photoresist after solidification.
2. A caplayer layer etching optimization method according to claim 1, Features: The gluing process steps in step S41 are as follows: S411, using a spin coater to quickly spin-coat photoresist on the epitaxial wafer at a high rotation speed, so that the photoresist is quickly spread; S412, leaving the epitaxial wafer after spin coating a layer of photoresist to stand for 10 seconds; S413, using a spin coater to slowly rotate the epitaxial wafer at a low speed to make the photoresist on the epitaxial wafer uniform.
3. A caplayer layer etching optimization method according to claim 2, Features: The high speed in step S411 is 3500-4000 r / s.
4. A caplayer layer etching optimization method according to claim 2, Features: The low speed in step S413 is 800-1200 r / s.
5. A caplayer layer etching optimization method according to claim 2, Features: The inclination angle of the edge of the photoresist is 70 to 80 degrees.
6. A caplayer layer etching optimization method according to claim 1, Features: The warpage compensation method is to grow a layer of stress film, the material of which is SiO 2 、SiN X or SiO X N y .
7. A caplayer layer etching optimization method according to claim 1, Features: The material of the optical film is one or a combination of dielectrics formed by Si, N, O, Al, F, and Mg.
8. A method for optimizing Cap layer etching according to any one of claims 1 to 7, Features: The metal material used for the metal deposition is one or more of gold, titanium, silver, copper, chromium, manganese and germanium.
9. A method for optimizing Cap layer etching according to any one of claims 1 to 7, Features: The full-structure epitaxial wafer comprises a Cap layer, a P-DBR layer, an oxide layer, a quantum well layer, an N-DBR layer and a substrate from the P surface to the N surface, wherein the substrate is a GaAs single crystal substrate.
Citation Information
Patent Citations
Alignment film for liquid crystals obtainable by direct particle beam deposition
US20110007255A1
Semiconductor device and manufacturing method thereof
US20130009219A1