Method for rapidly batch preparing large-area, uniform perovskite cell tin oxide electron transport layer and perovskite solar cell

Through dynamic eddy current deposition technology, the film inhomogeneity of the tin oxide electron transport layer is solved, and the preparation of large-area uniform and dense films is achieved, which improves the performance and efficiency of perovskite solar cells.

CN113725369BActive Publication Date: 2024-12-03WUHAN UNIV OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202110890418.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-04
Publication Date
2024-12-03
Estimated Expiration
2041-08-04

AI Technical Summary

Technical Problem

When the existing chemical bath deposition method prepares large-area tin oxide electron transport layer, the film thickness is uneven and the coverage is uneven, resulting in a decrease in the electron transfer rate and affecting the performance of perovskite solar cells.

Method used

Dynamic vertical or horizontal eddy current deposition technology is adopted to form a vortex at a certain rate, so that the solution moves as a whole, ensuring uniform distribution of particles during large-area deposition, improving the deposition process, and forming a uniform and dense tin oxide film.

Benefits of technology

The uniformity and density of large-area tin oxide electron transport layer are achieved, the charge transfer efficiency and device performance of perovskite solar cells are improved, and the production cost and environmental pollution are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113725369B_ABST
    Figure CN113725369B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for rapidly preparing a large-area, uniform perovskite cell tin oxide electron transport layer in batches and a perovskite solar cell. The steps are as follows: 1) inserting one or more clean substrates into a substrate rack vertically or horizontally, and treating the substrate surface with ozone or plasma; 2) placing the substrate rack together with the substrate in a tin oxide precursor solution, sealing and placing it on a heater that has reached a predetermined temperature, and starting to form an eddy current for deposition, with an eddy current speed of 0.1-1m / s; 3) immediately after the deposition is completed, taking out the substrate and placing it in cold water for ultrasonic cleaning, drying, and annealing to obtain a perovskite cell tin oxide electron transport layer. The method of the present invention is simple to operate, can be mass-produced, has low use cost, low environmental pollution, and the obtained tin oxide film is uniform and dense, and has good conductivity, permeability, and crystallinity; used for perovskite solar cells, rapid charge transmission can be achieved, and the performance of the device is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of tin oxide electron transport layer preparation, and specifically relates to a method for rapidly batch preparing large-area, uniform tin oxide electron transport layers for perovskite cells and a perovskite solar cell. Background Art

[0002] Perovskite solar cells are considered to be the most promising photovoltaic devices due to their low production cost and simple manufacturing. The typical device structure of PSC is transparent conductive electrode (such as FTO, ITO) / electron transport layer (ETL) / perovskite absorber layer / hole transport layer (HTL) / metal electrode. The electron transport layer facilitates the transport of carriers and effectively blocks holes, thereby reducing carrier recombination. Therefore, for the electron transport layer, its electron mobility, energy level matching with the perovskite layer, defect state density, structural morphology and interface properties play a crucial role in the performance of perovskite solar cells. Generally, electron transport materials can be divided into two categories: organic materials and inorganic materials. Organic electron transport materials, such as [6,6]-phenyl-C61-butyric acid methyl ester (PCBM) and C60. However, organic ETL is usually expensive and has thermal and photoinstability. Inorganic electron transport materials, such as titanium oxide, have low electron mobility and photoinstability. Therefore, low-cost and stable inorganic electron transport materials are considered to be more promising electron transport layers in PSCs. Tin oxide is considered to be one of the most promising electron transport materials. Tin oxide has a deep conduction band and well-defined energy levels, a wide optical band gap, high transmittance, high electron mobility and high conductivity, and can be easily prepared at low temperature (<200°C).

[0003] The preparation methods of SnO2 thin films reported in the existing literature mainly include: (1) sol-gel method, SnCl2·2H2O is dissolved in anhydrous ethanol to prepare SnO2 sol, and then the sol is spin-coated onto a substrate and sintered at 450℃; (2) low-temperature spin coating (SC), SnCl4·5H2O is spin-coated at room temperature and then sintered at 180℃ in air; (3) atomic deposition method (ALD), using plasma enhanced atomic deposition to prepare dense and uniform SnO2 thin films at 100℃; (4) chemical bath deposition, placing the substrate in a solution of SnCl2·2H2O to prepare SnO2 at low temperature, and annealing at low temperature. Among them, chemical bath deposition is a low-cost, low-temperature, simple and easy to operate method that can deposit multiple sheets to prepare thin films. Therefore, chemical bath deposition to prepare thin films has been widely used. When chemical bath deposition is used to prepare cadmium sulfide, for example, the deposition time is short, and the sedimentation of particles during the deposition process does not occur quickly, and it may take several hours for the sedimentation to occur, which has little effect on the uniform distribution of particle size. However, when chemical bath deposition is used to prepare tin oxide, the deposition time is long, generally several hours. During the deposition process, the sedimentation of particles causes particles of different sizes to be not evenly distributed in the solution, which has a great impact on the deposited film. For small pieces (10*10cm) of tin oxide film, the film is relatively uniform and of good quality, but when preparing large pieces (≥20*20cm) of tin oxide film, there are some problems, such as uneven film thickness and uneven film coverage, which greatly reduces the electron transfer rate, resulting in poor device performance. Summary of the invention

[0004] The purpose of the present invention is to provide a method for rapidly batch preparing a large-area, uniform tin oxide electron transport layer for a perovskite cell and a perovskite cell. The method is simple to operate, can be mass-produced, has low use cost, and causes little environmental pollution. The obtained tin oxide film is uniform and dense, and has good conductivity, permeability, and crystallinity. When used in perovskite solar cells, the method can realize rapid charge transmission and improve the performance of the device.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] A method for rapidly batch preparing a large-area, uniform tin oxide electron transport layer for perovskite cells is provided, comprising the following steps:

[0007] 1) inserting one or more cleaned and dried substrates vertically or horizontally into a substrate rack, and performing ozone or plasma treatment on the substrate surface;

[0008] 2) placing the substrate holder of step 1) together with the treated substrate into a tin oxide precursor solution, sealing and placing on a heater that has reached a predetermined temperature, and starting to form an eddy current for deposition, wherein the eddy current speed is 0.1 to 1 m / s;

[0009] 3) After the deposition is completed, the substrate is immediately taken out and placed in cold water for ultrasonic cleaning, blow-drying, and annealing to obtain the tin oxide electron transport layer of the perovskite cell.

[0010] According to the above scheme, in step 1), the substrate is FTO.

[0011] According to the above scheme, in step 1), the substrate area is ≥ 400 cm 2 .

[0012] According to the above scheme, in step 1), the number of substrates is 1 to 20.

[0013] According to the above scheme, in the step 2), the tin oxide precursor solution is prepared by mixing tin oxide mother liquor and water in a volume ratio of 1:4-5; the tin oxide mother liquor includes urea, concentrated hydrochloric acid, thioglycolic acid, sulfuric acid, amino acid, stannous chloride, mercaptosuccinic acid, potassium chloride, ammonium chloride and water, and the mass volume ratio of each component is: 2-12g: 2-12ml: 50-250μL: 0-2ml: 0-100μL: 0.5-3g: 0-100μL: 0-10mg: 0-20mg: 200-1500mL. Preferably, the mass volume ratio of stannous chloride and water is 1g: 500mL.

[0014] According to the above scheme, in step 2), the predetermined temperature is 50-150° C., and the deposition time is 1.5-5.5 h.

[0015] According to the above scheme, in the step 2), the vortex is formed by installing a propeller on the inner wall of the container, or placing the container on a shakeable instrument, or placing a substrate holder fixed by a rotating shaft in the solution and rotating it, or using a water pump to extract the solution from the bottom and inject the solution from the top to make the solution in the container circulate.

[0016] According to the above scheme, in step 3), the deposition time is 1.5 to 5.5 hours.

[0017] According to the above scheme, in step 4), the thickness of the obtained tin oxide electron transport layer is 5 to 50 nm.

[0018] According to the above scheme, in step 4), the annealing temperature is 100-200° C., and the annealing time is 0.5-3 h.

[0019] Provided is a perovskite solar cell, comprising an electron transport layer, wherein the electron transport layer is a tin oxide electron transport layer prepared by the above method.

[0020] According to the above solution, the thickness of the tin oxide electron transport layer is 5 to 50 nm.

[0021] According to the above scheme, the perovskite solar cell also includes transparent conductive glass, a perovskite absorption layer, a hole transport layer, and a metal electrode, and the electron transport layer is located between the transparent conductive glass and the perovskite absorption layer.

[0022] According to the above scheme, the transparent conductive glass is FTO; the components of the perovskite precursor solution are lead iodide, lead bromide, methylammonium bromide, formamidine iodide, and cesium iodide, and the obtained perovskite absorption layer has a thickness of 400 to 500 nm; the hole transport layer is Spiro-OMeTAD, and the thickness is 100 to 200 nm.

[0023] The present invention adopts chemical bath deposition to prepare tin oxide film. The reason for the uneven phenomenon of preparing large tin oxide films by chemical bath deposition is mainly that the concentration, pH, etc. of the deposition solution at different depths are different. Because in the process of preparing the tin oxide film, a chemical reaction occurs, and large particles are generated and settle to the bottom, resulting in uneven deposition on the glass. The present invention changes the static deposition into dynamic vertical or horizontal deposition, wherein the dynamic deposition is not just a simple mechanical stirring or magnetic stirring. For large-area deposition, the solution must be moved as a whole to form a vortex at a certain rate, and particles of different sizes can be evenly distributed in the solution, so that the influencing factor of the deposition depth is greatly weakened, so that the deposition liquid can fully and evenly cover the glass substrate, thereby depositing a uniform and dense tin oxide film, thereby improving the performance of the device.

[0024] The beneficial effects of the present invention are:

[0025] 1. The present invention adopts chemical bath deposition to prepare tin oxide thin film. During the deposition process, dynamic deposition is performed by controlling a certain eddy current rate, thereby overcoming the problem of uneven tin oxide thin film deposited by conventional chemical bath. The obtained film has uniform thickness, dense coverage, good conductivity, permeability and crystallinity. As an electron transport layer, the device has high opening voltage and high filling, and the energy conversion efficiency is greatly improved.

[0026] 2. The present invention can realize batch preparation of large-area tin oxide electron transport layers, which can improve efficiency and increase area while ensuring excellent film quality. The deposition temperature is low, the process is safe and reliable, the pollution is small, there is no need to add complex equipment, the cost is low, and it has broad application prospects.

[0027] 3. The perovskite solar cell provided by the present invention has a large area, fast charge transfer and excellent device performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 Schematic diagram of a deposition device for generating horizontal vortex in Example 1 of the present invention.

[0029] Figure 2Schematic diagram of a deposition device for generating vertical vortex in Example 1 of the present invention.

[0030] Figure 3 This is a SEM test result diagram of the surface morphology of the SnO2 film prepared in Example 1 of the present invention.

[0031] Figure 4 This is a cross-sectional SEM test result diagram of the SnO2 film prepared in Example 1 of the present invention.

[0032] Figure 5 Schematic diagram of the SnO2 thin film prepared in Example 1 of the present invention.

[0033] Figure 6 This is a diagram showing the efficiency distribution test results of a device prepared from SnO2 thin film in Example 1 of the present invention.

[0034] Figure 7 This is a schematic diagram of a large component prepared from SnO2 thin film in Example 1 of the present invention.

[0035] Figure 8 This is a graph showing the efficiency distribution test results of a device prepared from SnO2 thin film in Comparative Example 1 of the present invention.

[0036] Fig. 9 This is a cross-sectional SEM test result diagram of the SnO2 film prepared in Example 2 of the present invention.

[0037] Fig.10 This is a cross-sectional SEM test result diagram of the SnO2 film prepared in Example 3 of the present invention.

[0038] Fig.11 This is a cross-sectional SEM test result diagram of the SnO2 film prepared in Example 4 of the present invention.

[0039] Fig.12 This is a cross-sectional SEM test result diagram of the SnO2 film prepared in Example 5 of the present invention.

[0040] Fig.13 This is a graph showing the efficiency distribution test results of a device prepared from SnO2 thin film in Comparative Example 2 of the present invention.

[0041] Fig.14 This is a cross-sectional SEM test result diagram of the SnO2 film prepared in Example 6 of the present invention.

[0042] Fig.15 This is a cross-sectional SEM test result diagram of the SnO2 film prepared in Example 7 of the present invention.

[0043] Fig.16 This is a cross-sectional SEM test result diagram of the SnO2 film prepared in Example 8 of the present invention.

[0044] Fig.17 This is a cross-sectional SEM test result diagram of the SnO2 film prepared in Example 9 of the present invention.

[0045] Fig.18 This is a graph showing the test results of the photoelectric performance of the device prepared with the SnO2 thin film according to Example 1 of the present invention.

[0046] Fig.19 This is a graph showing the test results of the photoelectric performance of the device prepared with the SnO2 thin film according to Example 10 of the present invention.

[0047] Fig. 20 This is a graph showing the test results of the photoelectric performance of the device prepared with the SnO2 thin film according to Example 11 of the present invention. DETAILED DESCRIPTION

[0048] The present invention is further explained below by way of examples.

[0049] Example 1

[0050] The present embodiment provides a method for rapidly batch preparing a large-area, uniform tin oxide electron transport layer for perovskite cells, the method specifically comprising the following steps:

[0051] 1) Select 10 pieces with a thickness of 2.5mm and a size of 20*20cm 2 A square transparent conductive substrate FTO is cleaned with detergent, water, and ethanol in turn and ultrasonically treated for 15 minutes. After drying, the substrate is inserted vertically or horizontally into a substrate rack, and the surface is treated with ozone or plasma for standby use.

[0052] 2) Prepare tin oxide mother liquor with 5 g urea, 5 ml hydrochloric acid, 100 μL thioglycolic acid, 10 μL mercaptosuccinic acid, 10 mg potassium chloride, 1 g stannous chloride, and 500 ml deionized water. Stir continuously for 15 min, and then prepare tin oxide precursor solution with a volume ratio of mother liquor to deionized water of 1:4.

[0053] 3) Place the substrate rack together with the treated substrate into the tin oxide precursor solution, seal it with plastic wrap, and then place it on a heater that has reached a predetermined temperature. Start to form a vortex to move the solution. The vortex speed is 0.4 m / s. Control the deposition time to 4.5 h so that the film thickness is 20 nm.

[0054] 4) After the deposition is completed, the mixture is cleaned with deionized water and ultrasonically treated for 15 minutes, and then placed in an oven for annealing at 160° C. for 1.5 hours to obtain a tin oxide electron transport layer for a perovskite cell.

[0055] In this embodiment, eddies are formed to move the solution, and the eddies in both directions have the same effect on the deposited film. Figure 1 and Figure 2 As shown, Figure 1 It forms a horizontal vortex. Figure 2 It forms a vertical vortex.

[0056] The surface morphology SEM test results of the SnO2 thin film sample prepared in this embodiment are as follows: Figure 3 As shown by Figure 3 It can be seen that the film has no voids and is relatively uniform.

[0057] The cross-sectional SEM test results of the SnO2 thin film sample prepared in this embodiment are as follows: Figure 4 As shown in the figure, it can be seen that the film is relatively dense.

[0058] The large SnO2 film obtained in this embodiment is shown in FIG. Figure 5 shown.

[0059] The efficiency distribution diagram of the device prepared by the SnO2 film in this embodiment is as follows: Figure 6 As shown, the horizontal axis 1-6 is Figure 5 From the 1st, 3rd, 5th, 7th, 9th, and 10th rows. Figure 6 It can be seen that the efficiency distribution is uniform, indicating uniform tin oxide deposition over a large area.

[0060] In this embodiment, the large perovskite solar cell module prepared by the SnO2 film is as follows Figure 7 As shown. The perovskite solar cell component includes transparent conductive glass as FTO; the electron transport layer is tin oxide with a thickness of 20nm; the components of the perovskite precursor solution are lead iodide, lead bromide, methylamine bromide, formamidine iodide, and cesium iodide, and the obtained perovskite absorption layer has a thickness of 500nm; the hole transport layer is Spiro-OMeTAD with a thickness of 200nm.

[0061] Example 2

[0062] The method of this embodiment for rapidly and batch-producing a large-area, uniform tin oxide electron transport layer for perovskite cells is the same as the preparation method of this embodiment 1, except that the eddy current velocity in step 3) is 0.2 m / s.

[0063] The cross-sectional SEM test results of the SnO2 thin film sample prepared in this embodiment are as follows: Fig. 9 shown.

[0064] Example 3

[0065] The method of this embodiment for rapidly and batch-producing a large-area, uniform tin oxide electron transport layer for perovskite cells is the same as the preparation method of this embodiment 1, except that the eddy current velocity in step 3) is 0.6 m / s.

[0066] The cross-sectional SEM test results of the SnO2 thin film sample prepared in this embodiment are as follows: Fig.10 shown.

[0067] Example 4

[0068] The method of this embodiment for rapidly and batch-producing a large-area, uniform tin oxide electron transport layer for perovskite cells is the same as the preparation method of this embodiment 1, except that the eddy current velocity in step 3) is 0.8 m / s.

[0069] The cross-sectional SEM test results of the SnO2 thin film sample prepared in this embodiment are as follows: Fig.11 shown.

[0070] Example 5

[0071] The method of this embodiment for rapidly and batch-producing a large-area, uniform tin oxide electron transport layer for perovskite cells is the same as the preparation method of this embodiment 1, except that the eddy current velocity in step 3) is 1 m / s.

[0072] The cross-sectional SEM test results of the SnO2 thin film sample prepared in this embodiment are as follows: Fig.12 shown.

[0073] The corresponding embodiments 2, 3, 4, and 5 are Fig. 9 , 10 , 11, and 12, it can be seen that the tin oxide coverage is complete and the film is relatively dense.

[0074] Example 6

[0075] The method of this embodiment for rapidly and batch-producing a large-area, uniform tin oxide electron transport layer for perovskite cells is the same as the preparation method of this embodiment 1, except that the thickness of the film is controlled to be 5 nm during the deposition time of 1.5 h in step 3).

[0076] The cross-sectional SEM test results of the SnO2 thin film sample in this embodiment are shown in FIG. Fig.14 shown.

[0077] Example 7

[0078] The method of this embodiment for rapidly and batch-producing a large-area, uniform tin oxide electron transport layer for perovskite cells is the same as the preparation method of this embodiment 1, except that the thickness of the film is controlled to be 9 nm during the deposition time of 2.5 h in step 3).

[0079] The cross-sectional SEM test results of the SnO2 thin film sample in this embodiment are shown in FIG. Fig.15 shown.

[0080] Example 8

[0081] The method of this embodiment for rapidly and batch-producing a large-area, uniform tin oxide electron transport layer for perovskite cells is the same as the preparation method of this embodiment 1, except that the thickness of the film is controlled to be 14 nm during the deposition time of 3.5 h in step 3).

[0082] The cross-sectional SEM test results of the SnO2 thin film sample in this embodiment are shown in FIG. Fig.16 shown.

[0083] Example 9

[0084] The method of this embodiment for rapidly and batch-producing a large-area, uniform tin oxide electron transport layer for perovskite cells is the same as the preparation method of this embodiment 1, except that the thickness of the film is controlled to be 22 nm during the deposition time of 5.5 h in step 3).

[0085] The cross-sectional SEM test results of the SnO2 thin film sample in this embodiment are shown in FIG. Fig.17 shown.

[0086] Example 10

[0087] The method of this embodiment for rapidly and batch-producing a large-area, uniform tin oxide electron transport layer for perovskite cells is the same as the preparation method of this embodiment 1, except that the annealing temperature in step 4) is 180°C.

[0088] Embodiment 11

[0089] The method of this embodiment for rapidly and batch-producing a large-area, uniform tin oxide electron transport layer for perovskite cells is the same as the preparation method of this embodiment 1, except that the annealing temperature in step 4) is 200°C.

[0090] The photoelectric performance of the SnO2 perovskite solar cell devices prepared in Examples 1, 10 and 11 was tested respectively. The test results are as follows: Fig.18 , 19 , 20. It can be seen from the figure that the film effect of tin oxide after annealing at 160℃ is the best.

[0091] Comparative Example 1

[0092] The method for rapidly and batch-producing a large-area, uniform tin oxide electron transport layer for perovskite cells in this comparative example is the same as the preparation method in this embodiment 1, except that the eddy current velocity in step 3) is 0 m / s.

[0093] The efficiency distribution diagram of the device prepared by this SnO2 film in this comparative example is as follows Figure 8 As shown, the horizontal axis 1-6 is Figure 5 From the 1st, 3rd, 5th, 7th, 9th, and 10th rows. Figure 8It can be seen that the efficiency distribution is not uniform, indicating that the tin oxide deposition is not uniform over a large area.

[0094] Comparative Example 2

[0095] The method for rapidly and batch-producing a large-area, uniform tin oxide electron transport layer for perovskite cells in this comparative example is the same as the preparation method in this embodiment 1, except that the eddy current velocity in step 3) is 1.2 m / s.

[0096] The test results of the perovskite solar cell device distribution of the SnO2 thin film prepared in this comparative example are as follows: Fig.13 As shown. Fig.13 It can be seen that the efficiency distribution is uneven, so the uniformity of the prepared film is poor.

[0097] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for rapidly preparing a large-area, uniform tin oxide electron transport layer for perovskite cells in batches, characterized in that: The steps include: 1) inserting one or more cleaned and dried substrates vertically or horizontally into a substrate rack, and performing ozone or plasma treatment on the substrate surface; 2) placing the substrate rack of step 1) together with the treated substrate into a tin oxide precursor solution, sealing and placing on a heater that has reached a predetermined temperature, starting to form an eddy current for deposition, and the deposition time is 1.5 to 5.5 hours; wherein the eddy current speed is 0.1 to 1 m / s; the tin oxide precursor solution is prepared by configuring a tin oxide mother liquor and water in a volume ratio of 1:4 to 5; the tin oxide mother liquor comprises urea, concentrated hydrochloric acid, thioglycolic acid, sulfuric acid, amino acid, stannous chloride, mercaptosuccinic acid, potassium chloride, ammonium chloride and water, and the mass volume ratio of each component is: 2 to 12 g: 2 to 12 ml: 50 to 250 μL: 0 to 2 ml: 0 to 100 μL: 0.5 to 3 g: 0 to 100 μL: 0 to 10 mg: 0 to 20 mg: 200 to 1500 mL; 3) After the deposition is completed, the substrate is immediately taken out and placed in cold water for ultrasonic cleaning, blow-drying, and annealing to obtain a tin oxide electron transport layer for a perovskite cell; the thickness of the obtained tin oxide electron transport layer is 5 to 50 nm.

2. The method according to claim 1, characterized in that In step 1), the substrate area is ≥ 400 cm 2 .

3. The method according to claim 1, characterized in that In the step 1), the number of substrates is 1 to 20.

4. The method according to claim 1, characterized in that: In the step 1), the substrate is FTO.

5. The method according to claim 1, characterized in that In the step 2), the predetermined temperature is 50-150°C.

6. The method according to claim 1, characterized in that In the step 3), the annealing temperature is 100-200° C., and the annealing time is 0.5-3 h.

7. A perovskite solar cell comprising an electron transport layer, characterized in that: The electron transport layer is a tin oxide electron transport layer prepared by the method according to any one of claims 1 to 6.

8. The perovskite solar cell according to claim 7, characterized in that: The perovskite solar cell further comprises a transparent conductive glass, a perovskite absorption layer, a hole transport layer and a metal electrode, and the electron transport layer is located between the transparent conductive glass and the perovskite absorption layer.

Citation Information

Patent Citations

  • A preparation method of large-area perovskite thin film and a battery module thereof

    CN109103338A

  • Packaging method of perovskite solar cell

    CN111864083A

  • Preparation method of stable and efficient perovskite solar cell

    CN111864084A

  • Film growth method and device

    CN112962139A

  • Electroless plating of low-density particles - using both a stirrer and gas bubbles to keep particles in suspension

    FR2267149A1