A method and application of preparing block copolymer homoporous membrane by non-solvent induced phase separation
By combining specially made carbon nanotubes with block copolymers through a non-solvent-induced phase separation method, nanoporous films with high water flux and antibacterial properties were prepared, solving the problem of insufficient film performance in existing technologies and realizing simple and efficient industrial production.
Patent Information
- Application Number
- CN202110914306.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-10
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-08-10
AI Technical Summary
Existing technologies struggle to produce uniform nanoporous films with high water flux, antibacterial properties, and toughness, especially given the challenge of ease of operation during large-scale commercialization and industrialization.
A non-solvent-induced phase separation method was used to mix specially made carbon nanotubes with block copolymer polystyrene-block-polyacrylic acid, and a film with a microporous structure of 20-30 nanometers was prepared by a blade coating method. Silver nanoparticles were attached to the surface of the carbon nanotubes to enhance antibacterial properties and toughness.
A nanoporous membrane with uniform pores and long-range order was prepared, which significantly improved water flux and antibacterial properties, and is suitable for water treatment, biomedicine and preventive medicine.
Smart Images

Figure CN113813802B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of porous material separation membranes, and relates to a polymer isoporous membrane doped with specially made carbon nanotubes and a preparation method thereof. Background Art
[0002] In recent years, the use of phase separation to prepare block copolymers with self-assembly properties into isoporous films has become a research hotspot in the field of nanomaterial technology due to its advantages such as simple operation method, stable structural characteristics, and wide application range. After development in recent years, phase separation technology has extended to multiple branches such as non-solvent induced phase separation, thermally induced phase separation, and solvent evaporation induced phase separation. Among them, non-solvent induced phase separation has attracted the most attention. This method can be completed at room temperature and pressure without complex instruments and cumbersome steps. Therefore, it is also the method with the most hope of achieving large-scale commercial industrialization in the future.
[0003] At the same time, since the discovery of carbon nanotubes in 1991, their superior and unique characteristics such as aspect ratio, ultra-lightness, high tensile strength, electrical conductivity, chemical stability and thermal stability have also made them occupy an important position in biology, chemistry, medicine, water treatment and other fields. Carbon nanotubes are a one-dimensional nanomaterial with a special hollow tubular structure. When it is stretched or squeezed by external forces, this structure allows the carbon nanotubes to undergo elastic deformation, thereby absorbing the external impact energy to a large extent, which makes it have greater toughness. The classification of carbon tubes is rich and varied. In addition to being divided into single-walled carbon nanotubes and multi-walled carbon nanotubes, they can also be attached with different functional groups such as hydroxyl, carboxyl, amino, etc., which give them a variety of chemical properties, which greatly broadens the development prospects and scope of this material. Summary of the invention
[0004] The purpose of the present invention is to prepare a uniform porous film from a block copolymer compounded with special carbon nanotubes by using the non-solvent induced phase separation method mentioned above. The present invention combines special carbon tubes with antibacterial properties with block copolymers to prepare a new type of nanoporous film with uniform and long-range ordered pores. The film can achieve a higher water flux by adjusting the volatilization time. By adding carbon nanotubes and silver, the antibacterial property of the film is also significantly improved.
[0005] In order to solve the technical problem of the present invention, a technical solution is proposed: a method for preparing a homoporous block copolymer membrane by non-solvent induced phase separation, which is achieved by the following specific steps:
[0006] (1) dispersing multi-walled carbon nanotubes with carboxyl functional groups in ethanol and ultrasonically dispersing them, then dropping a silver nitrate solution with a concentration of 0.11 mol / L and ultrasonically treating them again;
[0007] (2) subjecting the solution obtained in step (1) to rotary evaporation to completely evaporate the ethanol to obtain dry carbon nanotubes, which are then placed in a tubular furnace and burned for a period of time;
[0008] (3) mixing the specially prepared carbon tubes obtained in the above step (2) with polystyrene-block-polyacrylic acid (PS-b-PAA) in a certain proportion, dissolving them in an organic solvent and fully sealing and stirring;
[0009] (4) applying the obtained mixed solution evenly on the support material by a doctor blade coating method, and after a certain volatilization time, immersing the mixed solution in deionized water;
[0010] (5) taking out the membrane material in the deionized water and drying it, finally obtaining an asymmetric isoporous membrane composited with specially prepared carbon nanotubes; the surface of the membrane is a microporous structure of 20-30 nanometers, the lower layer is a sponge-like pore support part, and the film is also penetrated by carbon nanotubes attached with silver nanoparticles to increase its toughness and antibacterial properties;
[0011] In the step (3), the mass ratio of the specially prepared carbon tube to polystyrene-block-polyacrylic acid (PS-b-PAA) is 0.9%-11%; the organic solvent in the step (3) can be 1,4-dioxane, or a solvent prepared by mixing 1,4-dioxane and tetrahydrofuran in a ratio of 2:1;
[0012] The volatilization time in step (4) should be controlled within the range of 5s-120s.
[0013] Preferably, the multi-walled carbon nanotubes with carboxyl functional groups in step (1) have a length of 10-30 micrometers, an inner diameter of 5-10 nanometers, and an outer diameter of 20-30 nanometers.
[0014] Preferably, the power and ultrasonic time of the ultrasonic instrument in step (1) should be as large as possible to effectively disperse the carbon nanotubes. The power used in the present invention is 100W and the ultrasonic time is 30 minutes. The concentration of this part of the silver nitrate solution can be changed accordingly according to demand, but it should be noted that the silver ion concentration and the amount of carbon nanotubes added should not be too high, otherwise the silver nanoparticles will aggregate or separate from the carbon nanotubes.
[0015] Preferably, in step (2), the heating rate of the tubular furnace is 10° C. per minute, and after reaching 450° C., the temperature is kept at that temperature for 3 hours.
[0016] Preferably, the support material in step (4) is a non-woven fabric, which has stable properties and strong adsorption capacity with the film and will not chemically react with other substances used in the invention.
[0017] Preferably, the stirring time in step (3) and the drying time in step (5) are both 12 hours; and the soaking time in step (4) is 24 hours.
[0018] In order to solve the technical problem of the present invention, another technical solution is proposed: a block copolymer homoporous membrane having certain toughness and antibacterial properties is prepared by any method using non-solvent induced phase separation.
[0019] In order to solve the technical problem of the present invention, another technical solution is proposed: the application of the non-solvent induced phase separation to prepare a block copolymer homoporous membrane with certain toughness and antibacterial properties can be applied in the fields of water treatment, biomedicine or preventive medicine technology.
[0020] The ultrasonic treatment time in step (1) is 30 minutes to 1 hour.
[0021] In step (2), the heating rate of the tube furnace is 10 degrees Celsius per minute until it reaches 450 degrees Celsius and is maintained for 3 hours. After calcination, the carboxyl groups on the carboxyl carbon nanotubes will be decomposed, and the silver particles will be reduced to silver element and attached to the wall of the multi-walled carbon nanotubes in the form of silver nanoparticles.
[0022] The block copolymer polystyrene-block-polyacrylic acid selected in step (3) consists of segment a and segment b, wherein segment a is polystyrene with a molecular weight of 70,500; segment b is polyacrylic acid with a molecular weight of 13,000.
[0023] The organic solvent mentioned in step (3) is dioxane, and the sealed stirring time is 12 hours.
[0024] The supporting material in step (4) is non-woven fabric, and the thickness of the film coated is 200 μm.
[0025] The volatilization time mentioned in step (4) is generally 5s-60s. The advantage is that the volatilization time can change the density of the sponge-like layer but does not affect the size of the pores on the surface of the film. The immersion time in deionized water is 24 hours. In this process, water is a non-solvent and can replace the dioxane in the film, thereby fixing the film morphology.
[0026] Beneficial effects:
[0027] Compared with electrochemical deposition and vapor deposition, the liquid deposition method selected in this experiment is simpler and requires fewer instruments. This method has more advantages in preparing silver nanoparticles on carbon nanotubes.
[0028] The polymer selected in the present invention, polystyrene-block-polyacrylic acid, has a relatively large molecular weight, so the film structure obtained by scraping is relatively stable, and the pore size distribution on the surface of the film is uniform.
[0029] The present invention controls the ratio of the special carbon tube to polystyrene-block-polyacrylic acid (PS-b-PAA) within the range of 0.9%-11%. Within this range, the carbon nanotubes are evenly dispersed in the film without aggregation. When the content of carbon nanotubes is too low, the antibacterial effect of the film will not achieve the expected effect; when the content of carbon nanotubes is too high, the surface of the film will be blocked, cracked, etc.
[0030] The film prepared by the present invention has a very high surface regularity and long-range order, which is rare in most previous inventions and is also a major feature of the film. The pore size of the film is maintained at 20-30nm, which will better maintain the water flux of the film in the later application process, and the effect will be more significant when applied to the filtration and interception of some small-sized nanoparticles.
[0031] According to tests, the volatilization time of the solvent in the air in the present invention has little effect on the pore size of the film surface, and the range is controlled within 5s-120s. This range will allow the organic solvent to volatilize and form uniform and orderly pores on the surface of the film. When the volatilization time is less than 5s, the long-range order of the pores formed on the film surface is low; when the time is too long, the pores on the film surface will expand and crack or form stripe-shaped, textured and other morphologies.
[0032] The present invention uses 1,4-dioxane as a solvent to effectively distinguish the hydrophilic segment and the hydrophobic segment in the block copolymer. If other solvents such as tetrahydrofuran, N,N-dimethylformamide or toluene are used, the film morphology will be messy or the film cannot be formed.
[0033] The carbon nanotubes used in this invention have multiple functions such as increasing the antibacterial properties of the film, improving the thermal conductivity of the film, etc., so that the film can be used in multiple directions.
[0034] When multi-walled carbon nanotubes with amino functional groups are used in step (1), effective binding with silver ions cannot be achieved. In addition, amino carbon nanotubes are difficult to disperse uniformly in the solvent required for this experiment.
[0035] The power and ultrasonic time of the ultrasonic instrument in step (1) should be as large as possible to effectively disperse the carbon nanotubes. The power of the ultrasonic instrument in step (1) is 100W, and the ultrasonic time is 30 minutes. The concentration of this part of the silver nitrate solution can be changed accordingly according to demand, but it should be noted that the silver ion concentration and the amount of added carbon nanotubes should not be too high, otherwise the silver nanoparticles will aggregate or separate from the carbon nanotubes. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 The surface characteristics of the film of the present invention;
[0037] Figure 2The morphological characteristics of the films prepared in different solvents and different solvent ratios;
[0038] Figure 3 XRD images of unsintered and sintered carbon nanotubes in Example 1;
[0039] Figure 4 Field emission scanning electron microscope (FE-SEM) images of the changes in film pores with increasing volatilization time in Example 1;
[0040] Figure 5 is the variation curve of the membrane water flux with the increase of volatilization time in Example 1;
[0041] Figure 6 is the variation curve of membrane water flux with the increase of MWCNTs-Ag mass in Example 2;
[0042] Figure 7 The diagram shows the antibacterial effect of the film on Escherichia coli;
[0043] Figure 8 The diagram shows the antibacterial effect of the film on Staphylococcus aureus; DETAILED DESCRIPTION
[0044] Comparative Example 1
[0045] Take 9 screw-mouth glass bottles with a capacity of 5 mL, and add 1,4-dioxane (Diox), tetrahydrofuran (THF) and N,N-dimethylformamide (DMF) to each bottle in various proportions (the total amount of solution is 3 mL). Add 24 mg of multi-walled carbon nanotubes to each bottle and ultrasonically disperse for 30 minutes. Take 300 μl of each mixed solution and add 80 mg of polystyrene-block-polyacrylic acid (PS-b-PAA). Add a magnet to each vial and stir for 12 hours until the mixture is evenly mixed to obtain a viscous casting liquid. Take a clean glass plate, fix the non-woven fabric on the glass plate, and use a scraper with a thickness of 200 μm to evenly scrape the casting liquid on the non-woven fabric. After 10 seconds of volatilization time, soak it in deionized water for 24 hours, take it out and dry it for 12 hours.
[0046] The films were photographed using an electron microscope. Figure 2 The figure shows the comparison of the films and the ratio of the organic solvents used. It is obvious from the figure that when pure dioxane is used, the uniform pore morphology of the film is more obvious and more regular, followed by the case of using a mixed solution of dioxane and tetrahydrofuran in a ratio of 2:1 as the solvent, but under this condition, the pore size of the film is not uniform enough.
[0047] Example 1
[0048] (1) Preparation of carbon nanotubes with silver nanoparticles
[0049] Disperse 100 mg of carboxyl multi-walled carbon nanotubes (brand: aladdin; purity ≥95%; inner diameter 5-10 nm; outer diameter 10-20 nm; length 10-30 μm) in 40 ml of anhydrous ethanol and ultrasonically treat for 30 minutes to evenly disperse the carbon nanotubes. Then add a pre-prepared 0.5 mol / L silver nitrate aqueous solution at a mass ratio of 3:10 between silver and carbon nanotubes, mix thoroughly, and ultrasonicate again for 30 minutes. After standing overnight, the solution is subjected to rotary evaporation to obtain dry MWCNTs-COOAg, which is placed in a tubular furnace, heated to 450°C at a rate of 10°C / min, and kept warm for 3 hours. After cooling, the product is taken out to finally obtain MWCNTs-Ag. Attached Figure 3 This is the XRD analysis comparison diagram of unsintered and sintered MWCNTs-COOAg. It can be seen that after sintering, three characteristic peaks of silver element Ag111, Ag200 and Ag220 appear, indicating that after sintering, the carboxyl groups on the carbon nanotubes are decomposed and the silver ions are reduced to silver element.
[0050] (2) Preparation of self-assembled block copolymer films
[0051] Take 24 mg of the above-obtained MWCNTs-Ag, mix it with 3 ml of dioxane and ultrasonically disperse it for 30 minutes. Take 300 μl of the mixed solution and add 80 mg of polystyrene-block-polyacrylic acid (PS-b-PAA), that is, the mass ratio of MWCNTs-Ag to polystyrene-block-polyacrylic acid is 3:100. Then add a magnetic bar and stir for 12 hours until the mixture is evenly mixed to obtain a viscous casting liquid. Take a clean glass plate, fix the non-woven fabric on the glass plate, and use a scraper with a thickness of 200 μm to evenly scrape the casting liquid on the non-woven fabric. After a certain volatilization time (5s, 10s, 30s, 50s, 90s, 120s), soak it in deionized water for 24 hours, take it out and dry it for 12 hours. Attachment Figure 4 The field emission scanning electron microscope (FE-SEM) images of each film at 160,000 times magnification are shown in the figure. As can be seen from the figure, when the solvent evaporation time is between 10s and 90s, the surface of the film is all orderly holes with a size of about 20 nanometers, which proves that the film is less affected by the solvent evaporation time, which can also greatly facilitate future production applications.
[0052] (3) Membrane water flux test
[0053] Each membrane was cut into a disc with a diameter of 2.5 cm and placed in an ultrafiltration cup. The ultrafiltration cup was filled with about 10 ml of ultrapure water, which was pressurized to 0.05 Pa by nitrogen gas to allow the water to pass through the membrane at a constant speed. The time required for each milliliter of water to pass through the membrane was recorded multiple times, and the average time was substituted into the formula F = V / (APT) to obtain the water flux of each membrane. The change of membrane water flux with increasing evaporation time is shown in the attached figure. Figure 5 As shown in the figure, it can be seen that when the solvent volatilization time is 50s, the water flux of the film reaches the maximum value, and the performance of the film is in the best state at this time.
[0054] Example 2
[0055] (1) Preparation of carbon nanotubes with silver nanoparticles
[0056] Disperse 100 mg of carboxyl multi-walled carbon nanotubes in 40 ml of anhydrous ethanol and ultrasonicate for 30 minutes to evenly disperse the carbon nanotubes. Then add a pre-prepared 0.5 mol / L silver nitrate aqueous solution at a mass ratio of 3:10 between silver and carbon nanotubes, mix thoroughly, and ultrasonicate again for 30 minutes. After standing overnight, the solution is subjected to rotary evaporation to obtain dry MWCNTs-COOAg, which is placed in a tubular furnace, heated to 450°C at a rate of 10°C / min, and kept warm for 3 hours. After cooling, take out the product to finally obtain MWCNTs-Ag.
[0057] (2) Preparation of self-assembled block copolymer films
[0058] Take 8.1mg, 24.7mg, 42.1mg, 88.9mg of the above-obtained MWCNTs-Ag, mix with 3ml of dioxane and ultrasonically disperse for 30 minutes. Take 300μl of each mixed solution and add 80mg of polystyrene-block-polyacrylic acid (PS-b-PAA) to make a mixed solution with a mass percentage of 1%, 3%, 5%, and 10% of MWCNTs-Ag. Then add a magnetic particle and stir for 12 hours until the mixture is evenly mixed to obtain a viscous casting liquid. Take a clean glass plate, fix the non-woven fabric on the glass plate, and use a scraper with a thickness of 200μm to evenly scrape the casting liquid on the non-woven fabric. After 30 seconds of volatilization time, soak in deionized water for 24 hours, take out and dry for 12 hours.
[0059] (3) Membrane water flux test
[0060] Each membrane was cut into a disc with a diameter of 2.5 cm and placed in an ultrafiltration cup. The ultrafiltration cup was filled with about 10 ml of ultrapure water, which was pressurized to 0.05 Pa by nitrogen gas to allow the water to pass through the membrane at a uniform speed. The time required for each milliliter of water to pass through the membrane was recorded multiple times, and the average time was substituted into the formula F = V / (APT) to obtain the water flux of each membrane. The change of membrane water flux with the increase of MWCNTs-Ag mass is shown in the attached figure. Figure 6 As shown in the figure, in order to ensure the water flux of the film, the content of carbon nanotubes should be as low as possible, but its antibacterial effect should still have significant changes, so the following antibacterial experiment was carried out.
[0061] (4) Film antibacterial performance testing
[0062] Take three 12mL bacterial culture tubes, add 3mL LB liquid culture medium, pick single colonies from Escherichia coli and Staphylococcus aureus solid culture medium and add them to the corresponding liquid culture medium, and use the other tube as a blank control group. Place in a constant temperature oscillator (37°C, 200rpm) for 15h of shaking culture.
[0063] In the first group of experiments, a 10 mm diameter disc was taken out using a hole puncher from the control group, a blank PS-b-PAA film sample without carbon nanotubes (P1), and a film sample with a carbon nanotube content of 1% (C1). The discs were added into disposable sterile small dishes with corresponding numbers, and the front and back sides were sterilized by ultraviolet irradiation for 30 minutes respectively for use.
[0064] Pipette 1 mL of the resuscitated E. coli solution, centrifuge at 5000 rpm for 5 min, discard the supernatant, and resuspend the precipitate with 1 mL of sterile PBS. Dilute the resuspended solution to 10 8 CFU / mL, and add 10 μL of diluted bacterial solution to each corresponding sample, and place it in a 37°C constant temperature incubator for co-cultivation for 12 h (humidity ≥ 90%).
[0065] After the co-culture, the bacterial solution was washed with 1 mL of sterile PBS, and then the washed bacterial solution was diluted 10 times with PBS solution (10 2 , 10 3 , 10 4 Three dilution multiples), take 100 μL of each gradient for plate coating, place in a 37°C constant temperature incubator for 18 hours, take out and take pictures and count. Figure 7 The photographic results, colony counts and bacterial concentration of the E. coli test. From the bacterial concentration results, it can be calculated that the antibacterial rate of film P1 is almost 0, while the antibacterial rate of film C1 with carbon nanotubes added reaches 94.27%; the experimental results are shown in Table 1.
[0066] Table 1
[0067]
[0068] The second group of experiments also used three samples: the control group, a blank PS-b-PAA film without carbon nanotubes (P2), and a film with a carbon nanotube content of 1% (C2). The E. coli solution was replaced with Staphylococcus aureus, and the rest of the steps were exactly the same. Figure 8 The photographic results, colony counts and bacterial concentration of the Staphylococcus aureus test. The antibacterial rate of film P2 is 40.58%, while the antibacterial rate of C2 is 73.62%. The experimental results are shown in Table 2.
[0069] Table 2
[0070]
[0071] Experimental verification shows that when the carbon nanotube content is low, the film already has good antibacterial ability, and when the water flux is high, the application ability of the film is stronger. Therefore, the best experimental condition for this experiment should be a film made of a mixed solution with a carbon nanotube mass percentage of 1%.
[0072] Example 3
[0073] The preparation method of this example is basically the same as that of Example 1, except that in (1) the preparation of carbon nanotubes with silver nanoparticles, the concentration of silver nitrate is changed to 0.1 mol / L, 0.3 mol / L, 0.7 mol / L, and 1 mol / L for comparison. In (2) the preparation of the self-assembled block copolymer film, the volatilization time of the film is fixed at 50 s.
[0074] The prepared isoporous film is similar to that in Example 1. This demonstrates that the concentration of silver nitrate in the present invention can be varied within the range of 0.1-1 mol / L.
[0075] Example 4
[0076] The preparation method of this embodiment is basically the same as that of embodiment 1, except that: in the preparation of (2) the self-assembled block copolymer film, the volatilization time of the film is fixed at 50 s; the stirring time of the mixed solution is changed to 10 hours, 18 hours, and 24 hours for comparison. The film immersion time is changed to 18 hours, 30 hours, and 36 hours for comparison. And the film drying time is changed to 8 hours, 10 hours, 14 hours, and 16 hours for comparison.
[0077] The prepared uniform porous film is similar to that in Example 1. It is proved that the stirring time in the invention can be varied within the range of 10-24 hours; the film soaking time can be varied within the range of 18-36 hours; and the film drying time can be varied within the range of 8-16 hours.
Claims
1. A method for preparing a block copolymer homoporous membrane by non-solvent induced phase separation, characterized in that: This is achieved through the following specific steps: (1) dispersing multi-walled carbon nanotubes with carboxyl functional groups in ethanol and ultrasonically dispersing them, then dropping a silver nitrate solution with a concentration of 0.11 mol / L and ultrasonically treating them again; (2) The solution obtained in step (1) is subjected to rotary evaporation to completely evaporate the ethanol to obtain dry carbon nanotubes, which are then placed in a tubular furnace and burned for a period of time; (3) The special carbon tubes obtained in step (2) are mixed with polystyrene- block -Polyacrylic acid (PS- b -PAA) in a certain proportion, dissolved in an organic solvent and fully sealed and stirred; (4) applying the obtained mixed solution evenly on the support material by a doctor blade coating method, and after a certain volatilization time, immersing the mixed solution in deionized water; (5) Taking out the membrane material from the deionized water and drying it, finally obtaining an asymmetric isoporous membrane composited with specially prepared carbon nanotubes; the surface of the membrane is a microporous structure of 20-30 nanometers, the lower layer is a sponge-like pore support part, and the film is also penetrated by carbon nanotubes with silver nanoparticles attached; In step (3), the mass ratio of the specially prepared carbon tube to polystyrene-block-polyacrylic acid (PS-b-PAA) is 0.9%-11%; the organic solvent in step (3) is 1,4-dioxane, or a solvent prepared by mixing 1,4-dioxane and tetrahydrofuran in a ratio of 2:1; The volatilization time in step (4) should be controlled within a range of 5s-120s.
2. The method for preparing a block copolymer homoporous membrane by non-solvent induced phase separation according to claim 1, characterized in that: The multi-walled carbon nanotubes with carboxyl functional groups in step (1) have a length of 10-30 micrometers, an inner diameter of 5-10 nanometers, and an outer diameter of 20-30 nanometers.
3. The method for preparing a block copolymer homoporous membrane by non-solvent induced phase separation according to claim 1, characterized in that: In step (1), the power of the ultrasonic instrument is 150W and the ultrasonic time is 30 minutes.
4. The method for preparing a block copolymer homoporous membrane by non-solvent induced phase separation according to claim 1, characterized in that: In step (2), the temperature of the tubular furnace is increased at a rate of 10°C per minute, and after reaching 450°C, the temperature is kept at that temperature for 3 hours.
5. The method for preparing a block copolymer homoporous membrane by non-solvent induced phase separation according to claim 1, characterized in that: The supporting material described in step (4) is non-woven fabric.
6. The method for preparing a block copolymer homoporous membrane by non-solvent induced phase separation according to claim 1, characterized in that: The stirring time in step (3) and the drying time in step (5) are both 12 hours; the soaking time in step (4) is 24 hours.
7. A block copolymer homoporous membrane having certain toughness and antibacterial properties prepared by non-solvent induced phase separation according to any one of claims 1 to 6.
8. The use of non-solvent induced phase separation to prepare a block copolymer homoporous membrane having certain toughness and antibacterial properties according to claim 7, characterized in that: It can be applied in the fields of water treatment, biomedicine or preventive medicine technology.
Citation Information
Cited By
Method for preparing uniform-hole straight-through membrane by using non-solvent-induced phase separation quaternary system