A super impact-resistant MPP pipe and its preparation method

By designing annular buffer layers and modified fillers in MPP pipes, the brittleness problem of MPP pipes in long-sunlight and low-temperature environments is solved, impact resistance and aging resistance are significantly improved, and service life is extended.

CN113824079BActive Publication Date: 2024-10-01NORTH ZHONGYI NEW MATERIALS (TONGLU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110991224.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-26
Publication Date
2024-10-01
Estimated Expiration
2041-08-26

AI Technical Summary

Technical Problem

MPP pipes are prone to free radical migration leading to macromolecule breakage in long-sunlight environments, and are susceptible to external impact in low-temperature environments, leading to brittle rupture, which limits their range of use and lifespan.

Method used

It adopts an inner and outer tube structure, with a braided layer and a buffer layer in the middle. The buffer layer includes a sleeve, a first buffer component and a second buffer component. An annular buffer layer is formed through the design of multiple shells, springs and transmission blocks to enhance impact resistance. performance, and improve the crystal structure of polypropylene resin through modified fillers and beta nucleating agents.

Benefits of technology

In long-sunlight and low-temperature environments, the impact resistance and aging resistance of MPP pipes are significantly improved, the service life is extended, brittle fracture is avoided, and the scope of use is expanded.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113824079B_ABST
    Figure CN113824079B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of MPP pipes, and in particular to a super impact-resistant MPP pipe and a preparation method thereof, comprising an inner pipe and an outer pipe, a braided layer is arranged on the inner pipe, a buffer layer is arranged between the braided layer and the outer pipe, the buffer layer comprises a sleeve, a first buffer component and a second buffer component, the sleeve is sleeved on the braided layer, the first buffer component and the second buffer component are intermittently arranged on the sleeve, and the first buffer component and the second buffer component are transmission-connected. The purpose of the present invention is to make the MPP pipe have good impact resistance and aging resistance, and can be used for a long time in a long-day environment and a low-temperature environment, so as to avoid brittle fracture of the MPP pipe under the action of external force in a low-temperature environment, increase the use range of the MPP pipe, and extend the service life of the MPP pipe.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of MPP pipes, and in particular to a super-strong impact-resistant MPP pipe and a preparation method thereof. Background Art

[0002] At present, there are two types of conventional power pipes on the market: MPP power pipes and CPVC power pipes. MPP power pipes are divided into trenchless and excavation types. MPP power pipes use modified polypropylene as the main raw material. They do not require a large amount of dredging, digging, or damaging the road surface. They are used for laying pipelines and cables in special areas such as roads, railways, buildings, and riverbeds. Compared with the traditional "trench digging and pipe laying method", trenchless power pipe projects are more in line with current environmental protection requirements, eliminating dust, traffic congestion and other nuisance factors caused by traditional construction. This technology can also be used to lay pipelines in some areas where excavation operations cannot be carried out, such as historic sites protection areas, downtown areas, crop and farmland protection areas, highways, rivers, etc.

[0003] MPP power cable protection pipe is a pipe with modified polypropylene as the main material. It has the advantages of good electrical insulation, high temperature resistance, corrosion resistance, etc. MPP pipe plays an important role in the development of power technology. However, in actual use, MPP pipe is prone to free radical migration under ultraviolet rays in a long-day environment, resulting in macromolecular breakage and accelerated aging. When the temperature drops at night, MPP pipe is easily brittle fractured after being impacted by external force in a low temperature environment, which limits the scope of use of MPP pipe and reduces the service life of MPP pipe. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a super impact-resistant MPP pipe and a preparation method thereof, so that the MPP pipe has good impact resistance and aging resistance, can be used for a long time in a long-day environment and a low-temperature environment, avoid the brittle fracture of the MPP pipe caused by external force in a low-temperature environment, increase the scope of use of the MPP pipe, and extend the service life of the MPP pipe.

[0005] The present invention solves the above technical problems by the following technical means:

[0006] A super impact-resistant MPP pipe comprises an inner tube and an outer tube, wherein a braided layer is arranged on the inner tube, a buffer layer is arranged between the braided layer and the outer tube, the buffer layer comprises a sleeve, a first buffer assembly and a second buffer assembly, the sleeve is sleeved on the braided layer, the first buffer assembly and the second buffer assembly are intermittently arranged on the sleeve, the first buffer assembly and the second buffer assembly are transmission-connected, the first buffer assembly comprises a connecting plate, a plurality of shells, a plurality of first springs, a transmission block, a first arc plate and a buffer, a plurality of the shells are evenly arranged on the sleeve, a cavity is formed between two adjacent shells, the connecting plate is installed in the shell, a groove is opened on the connecting plate, a plurality of the first springs are installed in the groove, the transmission block is installed in the groove, one end of the first spring is fixedly connected to the bottom of the groove, and the other end is fixedly connected to the transmission block, the first arc plate is fixedly arranged on the transmission block, the top of the first arc plate is against the top of the shell, the buffer is installed on the connecting plate, the second buffer assembly is installed in the cavity, and the buffer is transmission-connected to the second buffer assembly.

[0007] Further, the buffer component includes two mounting blocks, a connecting rod, a first transmission plate, a second transmission plate and multiple second springs, the two mounting blocks are fixedly arranged on the connecting plate, the connecting rod is rotatably passed through the two mounting blocks, one end of the first transmission plate is fixedly arranged with multiple first connecting tubes, one end of the second transmission plate is fixedly arranged with multiple second connecting tubes, multiple first connecting tubes and second connecting tubes are staggered and sleeved on the connecting rod, one end of multiple second springs is fixedly connected to the first transmission plate, and the other end is fixedly connected to the second transmission plate, both sides of the shell are respectively provided with a first through groove and a second through groove, the end of the first transmission plate passes through the first through groove, and the end of the second transmission plate passes through the second through groove, such an arrangement further enhances the buffering performance of the first buffer assembly.

[0008] Furthermore, a pad is provided in the shell, and the pad abuts against the inner walls of the first transmission plate and the second transmission plate. This arrangement prevents the first transmission plate and the second transmission plate from directly squeezing the shell, thereby enhancing the impact resistance of the shell.

[0009] Further, the second buffer assembly includes a semicircular sleeve, a second arc-shaped plate, a fixed plate, a third transmission plate, a fourth transmission plate, four support blocks, a first fixed rod and a second fixed rod. The second arc-shaped plate is fixedly arranged on the fixed plate, the semicircular sleeve is arranged on the second arc-shaped plate, the four support blocks are respectively fixedly arranged on both sides of the fixed plate, the first fixed rod and the second fixed rod are respectively penetrated through the four support blocks, one end of the third transmission plate is rotatably mounted on the first fixed rod, and the other end is abutted against the first transmission plate, one end of the fourth transmission plate is rotatably mounted on the second fixed rod, and the other end is abutted against the second transmission plate. Such an arrangement, in conjunction with the first buffer assembly, further enhances the impact resistance of the entire pipe and can further disperse the impact force received by the pipe. After the impact force, the first buffer assembly and the second buffer assembly can be reset.

[0010] Furthermore, the third transmission plate and the fourth transmission plate have the same structure, a mounting tube is fixedly provided on the third transmission plate, a torsion spring is provided in the mounting tube, the torsion spring is sleeved on the first fixed rod, one end of the torsion spring is fixedly connected to the mounting tube, and the other end is fixedly connected to one of the support blocks, such an arrangement enables the third transmission plate and the fourth transmission plate to be reset after being subjected to impact force.

[0011] Furthermore, a plurality of filling blocks are evenly arranged on the inner wall of the outer tube, and the filling blocks are filled between the shell and the semicircular sleeve. Such arrangement enables the impact force to be evenly dispersed to the first buffer component and the second buffer component when the pipe is subjected to impact force.

[0012] The present invention also discloses a method for preparing a super impact-resistant MPP pipe, and the preparation of the above-mentioned MPP pipe comprises the following steps:

[0013] A braided layer is sleeved on the inner tube, and a buffer layer is sleeved on the braided layer. When the buffer layer is sleeved, the sleeve and the shell are set as a whole, and then the first buffer component and the second buffer component are assembled and formed. A notch is opened on one side of each shell, and the notch is respectively connected with the first through groove and the second through groove. The first buffer component is pushed into the shell, and the second buffer component is pushed into the cavity formed by two adjacent shells, so that multiple first buffer components and multiple second buffer components are intermittently abutted against each other, and the pad is pushed into the bottom of the shell, and the notch is filled by melting the same material as the shell, and then the outer tube is sleeved on the buffer layer by pushing the outer tube in, so as to obtain a super impact-resistant MPP pipe.

[0014] Furthermore, the inner tube and the outer tube are made of the same material, and the inner tube comprises the following raw materials in parts by weight: 100 parts of polypropylene resin, 10-30 parts of modified filler, 1-2 parts of plasticizer, 0.5-1.5 parts of β-crystal nucleating agent, 1-3 parts of calcium zinc stabilizer and 2-4 parts of a mixed dispersant of stearamide and higher alcohol.

[0015] Further, the preparation of the inner tube comprises the following steps:

[0016] Place polypropylene resin in a high-speed mixer, stir for 5-10 minutes at 60-90°C, add modified filler and a mixed dispersant of stearamide and higher alcohol and continue stirring for 10-30 minutes, add plasticizer and calcium zinc stabilizer, continue stirring for 10-20 minutes at 130-150°C, add β-crystal nucleating agent, continue stirring for 3-5 minutes, after stirring, transfer to a twin-screw extruder, set the main engine temperature to 160-170°C, the mold temperature to 170-190°C, the head temperature to 190-200°C, extrude, shape, and vacuum cool to obtain an inner tube.

[0017] By adding modified fillers to the MPP pipe process, the impact resistance and aging resistance of the MPP pipe can be effectively enhanced due to the good impact resistance and aging resistance of the modified fillers. Since polypropylene is a crystalline resin, the crystallization process includes two stages: nucleation and crystal growth. Under the condition of spontaneous crystallization, the ordered areas formed by the segments of the polypropylene melt during the cooling process will form nuclei when some ordered areas exceed the critical size and stabilize. However, the number of nuclei obtained by this spontaneous nucleation method is small, the crystallization rate is slow, the spherulite size is large, and the crystallinity is low, which leads to poor impact resistance of the polypropylene material. The impact resistance of the polypropylene resin can be enhanced by adding modified fillers, and then by adding β-crystal nucleating agents, the polypropylene material is induced to crystallize into β-crystals, thereby promoting the crystallization process of polypropylene molecules and accelerating the crystallization rate, so that the molecules have a microcrystalline structure, and further improve the impact strength of the polypropylene material, so that the MPP pipe has good impact resistance and aging resistance.

[0018] Further, the preparation of the modified filler comprises the following steps:

[0019] S1 Glass fiber modification: Place polymerized rosin in a mixer, stir at 100-150°C for 30-60 min, add glass fiber, p-alkoxyphenol and titanate coupling agent, continue stirring at 300-500r / min for 1-2 hours, and after stirring, transfer to a wire drawing machine for wire drawing to obtain modified glass fiber;

[0020] S2 Preparation of modified filler: Place the modified glass fiber prepared in step S1 in active nano-calcium carbonate, heat to 60-90° C., seal and stir for 1-3 hours, and after stirring, cool and sieve to obtain the modified filler.

[0021] Glass fiber is a commonly used filler with good insulation, heat resistance, corrosion resistance, and mechanical strength, but it has disadvantages such as brittleness and poor wear resistance. Polymerized rosin is mainly a dimer, containing a mixture of rosin and rosin hydrocarbons, with the characteristics of high viscosity, non-crystallization, high softening point, good compatibility, excellent oxidation resistance, and strong durability. With glass fiber as the matrix, by cross-linking and coating the polymerized rosin on the glass fiber, it can not only enhance the impact resistance of the MPP pipe, but also effectively improve the shortcomings of the glass fiber such as brittleness and poor wear resistance, so that the MPP pipe has good impact resistance and wear resistance. Because the polymerized rosin is coated with glass fiber, the oxidation resistance and compatibility of the glass fiber can be enhanced, so that when the glass fiber is filled, the compatibility of the glass fiber and the polypropylene resin can be improved, and the oxidation resistance of the polypropylene resin can be enhanced. p-Alkoxyphenol has a p-π conjugated system, which can stabilize free radicals and make the generated tertiary carbon free radicals migrate to p-alkoxyphenol in time, thereby preventing various reactions of the molecular chain. Polymerized rosin and p-alkoxyphenol have a certain synergistic effect, which can synergistically enhance the anti-aging properties of glass fiber, thereby further enhancing the anti-aging properties of MPP pipes.

[0022] Active nano-calcium carbonate has the ability to scatter and shield ultraviolet rays. By coating the active nano-calcium carbonate on the modified glass fiber, the modified filler forms a three-layer composite structure. When exposed to ultraviolet rays, the active nano-calcium carbonate refracts and shields, and the polymerized rosin and p-alkoxyphenol synergistically prevent the migration of free radicals, so that the MPP pipe has good anti-aging and impact resistance.

[0023] The super impact-resistant MPP pipe and the preparation method thereof of the present invention have the following advantages:

[0024] 1. By modifying the filler in the preparation of MPP pipes, the modified filler has good impact resistance and aging resistance, thereby enhancing the impact resistance and aging resistance of MPP pipes, so that MPP pipes can be used for a long time in long-day and low-temperature environments, avoiding brittle fracture of MPP pipes under external forces in low-temperature environments, expanding the use range of MPP pipes, and extending the service life of MPP pipes;

[0025] 2. By adding a buffer layer between the prepared outer tube and the inner tube, the buffer layer includes a sleeve, a first buffer component and a second buffer component. The sleeve, the first buffer component and the second buffer component form an annular covering on the inner tube, and the first buffer component and the second buffer component are intermittently arranged, so that when the pipe is impacted by external force, multiple first buffer components and second buffer components can cooperate to disperse the external impact force, avoid a single buffer component being subjected to force alone, increase the upper limit of the force of the buffer component, thereby enhancing the impact resistance of the MPP pipe and extending its service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a structural schematic diagram of a super impact-resistant MPP pipe of the present invention;

[0027] Figure 2 This is a schematic diagram of the cross-sectional structure of a super impact-resistant MPP pipe of the present invention. Figure 1 ;

[0028] Figure 3 yes Figure 2 A schematic diagram of the enlarged structure at A in the middle;

[0029] Figure 4 It is a schematic diagram of the installation structure of the sleeve and the shell in a super impact-resistant MPP pipe of the present invention;

[0030] Figure 5 This is a schematic diagram of the cross-sectional structure of a super impact-resistant MPP pipe of the present invention. Figure 2 ;

[0031] Figure 6 yes Figure 5 A schematic diagram of the enlarged structure at B in the middle;

[0032] Figure 7 yes Figure 6 Schematic diagram of the enlarged structure at C in the middle;

[0033] Among them, the inner tube 1, the braided layer 2, the sleeve 3, the shell 31, the first through slot 311, the second through slot 312, the cavity 32, the outer tube 4, and the filling block 41;

[0034] Connecting plate 5, groove 51, first spring 52, transmission block 53, first arc plate 54, mounting block 55, connecting rod 56, first connecting tube 57, first transmission plate 571, second transmission plate 572, second spring 573, pad 58, semicircular sleeve 6, second arc plate 61, fixing plate 62, support block 63, first fixing rod 64, second fixing rod 641, torsion spring 642, third transmission plate 65, mounting tube 651, fourth transmission plate 66. DETAILED DESCRIPTION

[0035] The present invention will be described in detail below with reference to the accompanying drawings and specific embodiments:

[0036] Example 1

[0037] like Figure 1-7As shown, a super impact-resistant MPP pipe of this embodiment includes an inner pipe 1 and an outer pipe 4, a braided layer 2 is provided on the inner pipe 1, and a buffer layer is provided between the braided layer 2 and the outer pipe 4. The buffer layer can enhance the impact resistance of the MPP pipe, so that when the MPP pipe is subjected to external force, the external impact force can be dispersed and weakened to damage the pipe, thereby extending the service life of the MPP pipe. By providing the braided layer 2, the compression of the buffer layer on the inner pipe 1 is reduced when the buffer layer is subjected to force.

[0038] The buffer layer includes a sleeve 3, a first buffer component and a second buffer component. The sleeve 3 is sleeved on the braided layer 2. The first buffer component and the second buffer component are intermittently arranged on the sleeve 3 to form an annular buffer layer. The first buffer component and the second buffer component are transmission-connected so that when the outer tube 4 receives an external impact force, multiple first buffer components and second buffer components can cooperate to disperse the external impact force, avoid a single buffer component being subjected to force alone, increase the upper limit of the force of the buffer component, thereby enhancing the impact resistance of the MPP pipe and extending its service life.

[0039] The first buffer assembly includes a connecting plate 5, a plurality of housings 31, a plurality of first springs 52, a transmission block 53, a first curved plate 54 and a buffer. The plurality of housings 31 are evenly fixedly arranged on the sleeve 3, and a cavity 32 is formed between two adjacent housings 31. The connecting plate 5 is installed in the housing 31, a groove 51 is provided on the connecting plate 5, a plurality of first springs 52 are installed in the groove 51, and a transmission block 53 is installed in the groove 51. One end of the first spring 52 is fixedly connected to the bottom of the groove 51, and the other end is fixedly connected to the transmission block 53. The first curved plate 54 is fixedly arranged on the transmission block 53, and the top of the first curved plate 54 is against the top of the housing 31, so that when the top of the housing 31 is impacted by the outside world, the first curved plate 54 is squeezed, and the first curved plate 54 squeezes the plurality of first springs 52, thereby reducing the impact force of the outside world, and after the impact force disappears, the first curved plate 54 can be reset. The buffer is installed on the connecting plate 5 to further enhance the buffering capacity of the first buffer assembly. The second buffer assembly is installed in the cavity 32, and the buffer member is transmission-connected with the second buffer assembly, so that when the buffer member is squeezed by an external force, it can drive the second buffer assembly to disperse the impact force.

[0040] The buffer component includes two mounting blocks 55, a connecting rod 56, a first transmission plate 571, a second transmission plate 572 and a plurality of second springs 573. The two mounting blocks 55 are fixedly arranged at both ends of the connecting plate 5. The connecting rod 56 is rotatably passed through the two mounting blocks 55. A plurality of first connecting tubes 57 are fixedly arranged at one end of the first transmission plate 571. A plurality of second connecting tubes are fixedly arranged at one end of the second transmission plate 572. The plurality of first connecting tubes 57 and the plurality of second connecting tubes are alternately sleeved on the connecting rod 56 so that the first transmission plate 571 and the second transmission plate 572 can rotate relative to the connecting rod 56. One end of the plurality of second springs 573 is fixedly connected to the first transmission plate 571, and the other end is fixedly connected to the second transmission plate 572. The first through slot 311 and the second through slot 312 are respectively provided on both sides of the housing 31. The end of the first transmission plate 571 passes through the first through slot 311, and the end of the second transmission plate 572 passes through the second through slot 312, so that when the connecting plate 5 is squeezed by an external force, the connecting plate 5 moves downward, driving the first transmission plate 571 and the second transmission plate 572 to move along the first through slot 311 and the second through slot 312 respectively, and in the process of moving, the second springs 573 are stretched, so that the first transmission plate 571 and the second transmission plate 572 can automatically reset when the connecting plate 5 is reset. A pad 58 is provided in the housing 31, and the pad 58 abuts against the inner walls of the first transmission plate 571 and the second transmission plate 572 to prevent the first transmission plate 571 and the second transmission plate 572 from directly squeezing the housing 31, thereby enhancing the impact resistance of the housing 31.

[0041] The second buffer assembly includes a semicircular sleeve 6, a second arc plate 61, a fixed plate 62, a third transmission plate 65, a fourth transmission plate 66, four support blocks 63, a first fixed rod 64 and a second fixed rod 641. The second arc plate 61 is fixedly arranged on the fixed plate 62, the semicircular sleeve 6 is arranged on the second arc plate 61, the four support blocks 63 are respectively fixedly arranged on both sides of the fixed plate 62, the first fixed rod 64 and the second fixed rod 641 are respectively penetrated on the four support blocks 63, one end of the third transmission plate 65 is rotatably mounted on the first fixed rod 64, and the other end is abutted against the first transmission plate 571, and one end of the fourth transmission plate 66 is rotatably mounted on the second fixed rod 641, and the other end is abutted against the second transmission plate 572 When two adjacent first buffer components are impacted by the outside world, the first transmission plate 571 and the second transmission plate 572 move along the first through groove 311 and the second through groove 312, and the first transmission plate 571 and the second transmission plate 572 can respectively squeeze the third transmission plate 65 and the fourth transmission plate 66 in the two adjacent second buffer components, thereby dispersing the impact force received, and in the process of the first transmission plate 571 squeezing the third transmission plate 65 and the second transmission plate 572 squeezing the fourth transmission plate 66, the third transmission plate 65 and the fourth transmission plate 66 move toward the middle, so that the fixed plate 62, the second arc plate 61 and the semicircular sleeve 6 move upward, thereby supporting the impacted part and reducing the external squeezing force on the pipe. When two adjacent second buffer components are impacted by the outside world, the semicircular sleeve 6 and the second arc plate 61 move downward, driving the third transmission plate 65 and the fourth transmission plate 66 to open to both sides of the fixed plate 62, thereby respectively squeezing the first transmission plate 571 and the second transmission plate 572 in the two adjacent first buffer components, and the first transmission plate 571 and the second transmission plate 572 drive the connecting plate 5 to move upward, thereby supporting the impact point and reducing the external squeezing force on the pipe. Through the intermittently arranged first buffer components and second buffer components, when the pipe is impacted in any direction, multiple first buffer components and multiple second buffer components can cooperate to disperse the impact force, thereby reducing the impact force on the pipe and preventing the external impact force from damaging the pipe.

[0042] The third transmission plate 65 and the fourth transmission plate 66 have the same structure. A mounting tube 651 is fixedly arranged on the third transmission plate 65. A torsion spring 642 is arranged in the mounting tube 651. The torsion spring 642 is sleeved on the first fixing rod 64. One end of the torsion spring 642 is fixedly connected to the mounting tube 651, and the other end is fixedly connected to one of the supporting blocks 63, so that the third transmission plate 65 and the fourth transmission plate 66 can be reset after the impact force disappears, and when the first transmission plate 571 and the second transmission plate 572 no longer squeeze the third transmission plate 65 and the fourth transmission plate 66, the third transmission plate 65 and the fourth transmission plate 66 can be reset. A plurality of filling blocks 41 are evenly fixedly arranged on the inner wall of the outer tube 4. The filling blocks 41 are filled between the shell 31 and the semicircular sleeve 6, so that when the pipe is subjected to impact force, the impact force can be evenly dispersed to the first buffer assembly and the second buffer assembly, ensuring the uniformity of the force of the first buffer assembly and the second buffer assembly.

[0043] Example 2

[0044] The method for preparing the super impact-resistant MPP pipe of Example 1 comprises the following steps:

[0045] A braided layer is sleeved on the inner tube, and a buffer layer is sleeved on the braided layer. When the buffer layer is sleeved, the sleeve and the shell are set as a whole, and then the first buffer component and the second buffer component are assembled and formed. A notch is opened on one side of each shell, and the notch is respectively connected with the first through groove and the second through groove. The first buffer component is pushed into the shell, and the second buffer component is pushed into the cavity formed by two adjacent shells, so that multiple first buffer components and multiple second buffer components are intermittently abutted against each other, and the pad is pushed into the bottom of the shell, and the notch is filled by melting the same material as the shell, and then the outer tube is sleeved on the buffer layer by pushing the outer tube in, so as to obtain a super impact-resistant MPP pipe.

[0046] The inner tube 1 and the outer tube 4 are made of the same material, and the preparation of the inner tube 1 and the outer tube 4 includes the following steps:

[0047] Example 3, Preparation of modified filler

[0048] S1 Glass fiber modification: 10 parts by mass of polymerized rosin were placed in a mixer, stirred at 100°C for 30 minutes, 8 parts by mass of glass fiber, 2 parts by mass of p-alkoxyphenol and 1 part by mass of titanate coupling agent were added, and the mixture was stirred at 300 r / min for 1 hour. After the stirring was completed, the mixture was transferred to a wire drawing machine for drawing to obtain modified glass fiber. The modified glass fiber was tested and the diameter was 8 um.

[0049] S2 Preparation of modified filler: 10 parts by mass of the modified glass fiber prepared in step S1 are placed in 30 parts by mass of active nano-calcium carbonate, heated to 60°C, sealed and stirred for 1 hour, and after stirring, cooled and sieved to remove excess active nano-calcium carbonate to obtain a modified filler.

[0050] Example 4, Preparation of modified filler II

[0051] S1 Glass fiber modification: 20 parts by mass of polymerized rosin were placed in a mixer, stirred at 125°C for 45 minutes, 15 parts by mass of glass fiber, 5 parts by mass of p-alkoxyphenol and 2.5 parts by mass of titanate coupling agent were added, and stirring was continued at a speed of 400r / min for 1.5 hours. After stirring, the mixture was transferred to a wire drawing machine for drawing to obtain modified glass fiber. The modified glass fiber was tested and the diameter was 12um.

[0052] S2 Preparation of modified filler: 20 parts by mass of the modified glass fiber prepared in step S1 are placed in 50 parts by mass of active nano-calcium carbonate, heated to 75°C, sealed and stirred for 1.5 hours. After stirring, the mixture is cooled and sieved to remove excess active nano-calcium carbonate to obtain a modified filler.

[0053] Example 5, Preparation of modified filler

[0054] S1 Glass fiber modification: 30 parts by mass of polymerized rosin were placed in a mixer, stirred at 150°C for 60 minutes, 24 parts by mass of glass fiber, 8 parts by mass of p-alkoxyphenol and 4 parts by mass of titanate coupling agent were added, and stirring was continued at a speed of 500r / min for 2 hours. After stirring, the mixture was transferred to a wire drawing machine for drawing to obtain modified glass fiber. The modified glass fiber was tested and the diameter was 15um.

[0055] S2 Preparation of modified filler: 30 parts by mass of the modified glass fiber prepared in step S1 is placed in 70 parts by mass of active nano-calcium carbonate, heated to 90°C, sealed and stirred for 2 hours. After stirring, it is cooled and sieved to remove excess active nano-calcium carbonate to obtain a modified filler.

[0056] Example 6, Preparation of MPP inner tube

[0057] 100 parts by mass of polypropylene resin are placed in a high-speed mixer, stirred at 60°C for 5 minutes, 10 parts by mass of modified filler and 2 parts by mass of a mixed dispersant of stearamide and higher alcohol are added, and stirring is continued for 10 minutes, 1 part by mass of plasticizer and 1 part by mass of calcium zinc stabilizer are added, stirring is continued for 10 minutes at 130°C, 0.5 parts by mass of β-crystal nucleating agent are added, stirring is continued for 3 minutes, after stirring is completed, transfer to a twin-screw extruder, set the main engine temperature to 160-170°C, the mold temperature to 170-190°C, the head temperature to 190-200°C, extrude, shape, and vacuum cool to obtain an inner tube.

[0058] Example 7, Preparation of MPP inner tube II

[0059] 100 parts by mass of polypropylene resin are placed in a high-speed mixer, stirred at 80°C for 8 minutes, 20 parts by mass of modified filler and 3 parts by mass of a mixed dispersant of stearamide and higher alcohol are added, and stirring is continued for 20 minutes, 1.5 parts by mass of plasticizer and 2 parts by mass of calcium zinc stabilizer are added, stirring is continued for 15 minutes at 140°C, 1 part by mass of β-crystal nucleating agent is added, stirring is continued for 4 minutes, after stirring is completed, transfer to a twin-screw extruder, set the main engine temperature to 160-170°C, the mold temperature to 170-190°C, the head temperature to 190-200°C, extrude, shape, and vacuum cool to obtain an inner tube.

[0060] Example 8, Preparation of MPP inner tube III

[0061] 100 parts by weight of polypropylene resin were placed in a high-speed mixer, stirred at 90°C for 10 minutes, 30 parts by weight of modified filler and 4 parts by weight of a mixed dispersant of stearamide and higher alcohol were added, and stirring was continued for 30 minutes, 2 parts by weight of plasticizer and 3 parts by weight of calcium zinc stabilizer were added, stirring was continued for 20 minutes at 150°C, 1.5 parts by weight of β-crystal nucleating agent were added, stirring was continued for 5 minutes, and after stirring, the mixture was transferred to a twin-screw extruder, the main engine temperature was set to 160-170°C, the mold temperature was set to 170-190°C, the head temperature was set to 190-200°C, extrusion molding was performed, shaping was performed, and vacuum cooling was performed to obtain an inner tube.

[0062] The impact resistance and aging resistance of the MPP inner tubes prepared in Examples 6-8 were tested, and the test results are shown in the following table:

[0063]

[0064] It can be seen from the data in the table that the MPP pipes prepared in Examples 6-8 have better impact resistance and aging resistance in both low and high temperature environments compared with ordinary MPP pipes, indicating that the modified filler and β-crystal nucleating agent added in this scheme can effectively enhance the impact resistance and aging resistance of the MPP pipes.

[0065] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it should be understood by those skilled in the art that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the purpose and scope of the technical solutions of the present invention, which should be included in the scope of the claims of the present invention. The techniques, shapes, and structural parts not described in detail in the present invention are all known technologies.

Claims

1. A super impact-resistant MPP pipe, characterized by: The invention comprises an inner tube and an outer tube, wherein the inner tube and the outer tube are made of the same material, a braided layer is arranged on the inner tube, a buffer layer is arranged between the braided layer and the outer tube, the buffer layer comprises a sleeve, a first buffer component and a second buffer component, the sleeve is sleeved on the braided layer, the first buffer component and the second buffer component are intermittently arranged on the sleeve, the first buffer component and the second buffer component are transmission-connected, the first buffer component comprises a connecting plate, a plurality of shells, a plurality of first springs, a transmission block, a first arc-shaped plate and a buffer, a plurality of the shells are evenly arranged on the sleeve, a cavity is formed between two adjacent shells, the connecting plate is installed in the shell, a groove is provided on the connecting plate, a plurality of the first springs are installed in the groove, the transmission block is installed in the groove, one end of the first spring is fixedly connected to the bottom of the groove, and the other end is fixedly connected to the transmission block, the first arc-shaped plate is fixedly arranged on the transmission block, the top of the first arc-shaped plate is against the top of the shell, the buffer is installed on the connecting plate, the second buffer component is installed in the cavity, and the buffer is transmission-connected to the second buffer component; The buffer member includes two mounting blocks, a connecting rod, a first transmission plate, a second transmission plate and a plurality of second springs, the two mounting blocks are fixedly arranged on the connecting plate, the connecting rod is rotatably arranged on the two mounting blocks, a plurality of first connecting tubes are fixedly arranged on one end of the first transmission plate, a plurality of second connecting tubes are fixedly arranged on one end of the second transmission plate, a plurality of the first connecting tubes and the second connecting tubes are staggered and sleeved on the connecting rod, a plurality of the second springs have one end fixedly connected to the first transmission plate, and the other end fixedly connected to the second transmission plate, a first through slot and a second through slot are respectively provided on both sides of the housing, a terminal end of the first transmission plate passes through the first through slot, and a terminal end of the second transmission plate passes through the second through slot; The second buffer assembly includes a semicircular sleeve, a second arc-shaped plate, a fixed plate, a third transmission plate, a fourth transmission plate, four support blocks, a first fixed rod and a second fixed rod. The second arc-shaped plate is fixedly arranged on the fixed plate, the semicircular sleeve is arranged on the second arc-shaped plate, the four support blocks are respectively fixedly arranged on both sides of the fixed plate, the first fixed rod and the second fixed rod are respectively penetrated on the four support blocks, one end of the third transmission plate is rotatably mounted on the first fixed rod, and the other end is abutted against the first transmission plate, and one end of the fourth transmission plate is rotatably mounted on the second fixed rod, and the other end is abutted against the second transmission plate.

2. The super impact-resistant MPP pipe according to claim 1 is characterized in that: A pad is arranged in the shell, and the pad abuts against the inner walls of the first transmission plate and the second transmission plate.

3. The super impact-resistant MPP pipe according to claim 2 is characterized in that: The third transmission plate and the fourth transmission plate have the same structure. A mounting tube is fixedly arranged on the third transmission plate. A torsion spring is arranged in the mounting tube. The torsion spring is sleeved on the first fixing rod. One end of the torsion spring is fixedly connected to the mounting tube, and the other end is fixedly connected to one of the support blocks.

4. The super impact-resistant MPP pipe according to claim 1 is characterized in that: A plurality of filling blocks are evenly arranged on the inner wall of the outer tube, and the filling blocks are filled between the shell and the semicircular sleeve.

5. A method for preparing the super impact-resistant MPP pipe according to claim 1, characterized in that: The invention comprises the following steps: sleeve a braided layer on the inner tube, sleeve a buffer layer on the braided layer, when sleeve the buffer layer, set the sleeve and the shell as a whole, then assemble the first buffer component and the second buffer component into shape, open a notch on one side of each shell, make the notch communicate with the first through groove and the second through groove respectively, push the first buffer component into the shell, push the second buffer component into the cavity formed by two adjacent shells, make multiple first buffer components and multiple second buffer components intermittently abut against each other, push the pad into the bottom of the shell, fill the notch by melting the same material as the shell, and then sleeve the outer tube on the buffer layer by pushing the outer tube into the outer tube to obtain the super impact-resistant MPP pipe.

6. The method for preparing a super impact-resistant MPP pipe according to claim 5, characterized in that: The inner tube and the outer tube are made of the same material. The inner tube comprises the following raw materials in parts by weight: 100 parts of polypropylene resin, 10-30 parts of modified filler, 1-2 parts of plasticizer, 0.5-1.5 parts of β-crystal nucleating agent, 1-3 parts of calcium zinc stabilizer and 2-4 parts of a mixed dispersant of stearamide and higher alcohol.

7. The method for preparing a super impact-resistant MPP pipe according to claim 6, characterized in that: The preparation of the inner tube comprises the following steps: Place polypropylene resin in a high-speed mixer, stir for 5-10 minutes at 60-90°C, add modified filler and a mixed dispersant of stearamide and higher alcohol and continue stirring for 10-30 minutes, add plasticizer and calcium zinc stabilizer, continue stirring for 10-20 minutes at 130-150°C, add β-crystal nucleating agent, continue stirring for 3-5 minutes, after stirring, transfer to a twin-screw extruder, set the main engine temperature to 160-170°C, the mold temperature to 170-190°C, the head temperature to 190-200°C, extrude, shape, and vacuum cool to obtain an inner tube.

8. The method for preparing a super impact-resistant MPP pipe according to claim 7, characterized in that: The preparation of the modified filler comprises the following steps: S1 Glass fiber modification: Place polymerized rosin in a mixer, stir at 100-150°C for 30-60 min, add glass fiber, p-alkoxyphenol and titanate coupling agent, continue stirring at 300-500r / min for 1-2h, after stirring, transfer to a wire drawing machine, draw to obtain modified glass fiber; S2 Preparation of modified filler: Place the modified glass fiber prepared in step S1 in active nano-calcium carbonate, heat to 60-90° C., seal and stir for 1-3 hours, and after stirring, cool and sieve to obtain the modified filler.