A catalytic cracking catalyst and its preparation method
Through the in-situ crystallization and ion exchange treatment of kaolin modified NSY molecular sieve, combined with multi-stage pore structure and rare earth modification, the problem of high coking of Y-type molecular sieve catalysts in the prior art is solved, and the high conversion rate of heavy oil is achieved Reduce coke selectivity and improve the efficiency of catalytic cracking reaction.
Patent Information
- Application Number
- CN202010581808.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-06-23
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-06-23
AI Technical Summary
The existing in-situ crystallized Y-type molecular sieve catalysts have high coke selectivity during heavy oil conversion and are difficult to effectively reduce.
Modified NSY molecular sieve was used to synthesize the in-situ crystallization of kaolin and undergo ion exchange treatment to reduce the sodium oxide content, combine multi-stage pore structure and rare earth modification to prepare a catalyst with high cracking activity and low coke selectivity.
On the basis of maintaining high heavy oil conversion, the coke selectivity is significantly reduced, and the efficiency and product yield of catalytic cracking reaction are improved.
Smart Images

Figure BDA0002552587490000081 
Figure BDA0002552587490000091 
Figure BDA0002552587490000101
Abstract
Description
Technical Field
[0001] The present invention relates to a catalytic cracking catalyst, and more particularly to a low-coking catalytic cracking catalyst and a preparation method thereof. Background Art
[0002] Catalytic cracking (FCC) is an important secondary processing of crude oil and plays a pivotal role in the oil refining industry. In the catalytic cracking process, heavy fractions such as vacuum distillate or heavier residual oil react in the presence of a catalyst to convert into high value-added products such as liquefied gas, gasoline, and diesel. In this process, catalytic materials with high cracking activity are usually required. Y-type zeolite is widely used in catalytic cracking reactions due to its excellent shape-selective catalytic performance and high cracking reaction activity. Y-type zeolite is obtained through two technologies: one technology is to first synthesize Y-type zeolite using alkaline silica-alumina gel, then mix Y-type zeolite with a matrix, and spray-dry to obtain a microsphere catalyst. The Y-type zeolite synthesized by alkaline silica-alumina gel has the characteristics of high molecular sieve content and high silicon-aluminum ratio. It can have a variety of reaction characteristics by using different modification methods; the other technology is in-situ crystallization technology, which first forms microspheres, and then crystallizes the molecular sieve on the microspheres to directly obtain catalyst microspheres containing both active components-molecular sieves and non-molecular sieve components. The catalyst synthesized by in-situ crystallization technology has strong resistance to heavy metal pollution, high activity index, good hydrothermal stability, good structural stability, etc. However, the existing in-situ crystallized Y-type molecular sieves synthesized for heavy oil conversion have a relatively high coke yield.
[0003] Bao Xiaojun CN103043680A uses natural kaolin and diatomite minerals to provide all silicon and aluminum sources for molecular sieve synthesis, and uses them as the matrix for molecular sieve growth, and forms a crystalline product through in-situ crystallization. In the composite material, the mass percentage of NaY molecular sieve is 25% to 50%, and the silicon-aluminum ratio of NaY molecular sieve is 3 to 5.5.
[0004] Zheng Shuqin (Synthesis of Hierarchical Porous Channel Catalytic Materials by Hydrothermal Crystallization of Si-Al Gel and Kaolin, Acta Petrolei Sinica (Petroleum Processing), V30(1), 32-37) reported the hydrothermal synthesis of hierarchical porous channel catalytic materials by Si-Al gel and kaolin. The method is to prepare Si-Al gel using water glass and sodium aluminate as silicon source and aluminum source respectively, and then spray it with kaolin to form balls, and then synthesize it.
[0005] The above disclosure does not involve how to reduce the coke selectivity of a catalyst containing an in-situ crystallized Y-type molecular sieve for heavy oil conversion. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a catalytic cracking catalyst with less coking under the condition of higher heavy oil conversion rate, which contains NSY molecular sieve active components, in view of the high coking problem of in-situ crystallized Y-type molecular sieve catalytic cracking catalyst in the prior art.
[0007] A catalytic cracking catalyst comprises: 10-70 wt% of a cracking active component, 10-60 wt% of a binder and 10-70 wt% of clay, wherein the cracking active component comprises 5-100 wt% of a first Y-type molecular sieve and 0-95 wt% of a second molecular sieve, the first Y-type molecular sieve is a modified NSY molecular sieve, and the modified NSY molecular sieve is obtained by modifying NSY molecules synthesized by in-situ crystallization of kaolin.
[0008] The NSY molecular sieve synthesized by in-situ crystallization of kaolin has a crystallinity of ≥60% measured by the peak height method using an X-ray diffraction method, and the ratio of the crystallinity to the peak area method is K1, K1=0.76-0.89; the silicon-aluminum ratio measured by the unit cell constant a0 is 5.0-5.5, and the ratio to the silicon-aluminum ratio measured by the chemical method is K2, K2=0.87-0.93, and the silicon-aluminum ratio is the molar ratio of silicon oxide to aluminum oxide. The crystallinity measured by the peak height method is ≥80%. The K1=0.80-0.89 or the K1=0.80-0.85. The K2=0.87-0.92 or the K2=0.88-0.90.
[0009] In a preferred embodiment, the NSY molecular sieve synthesized by in-situ crystallization of kaolin has K1=0.77-0.88 and K2=0.87-0.91.
[0010] In one embodiment, the large mesopore ratio of the NSY molecular sieve synthesized by in-situ crystallization of kaolin is 10-20%.
[0011] In one embodiment, the NSY molecular sieve synthesized by in-situ crystallization of kaolin has a silicon-to-aluminum ratio of 5.2 to 5.5 as measured by the unit cell constant a0.
[0012] In a preferred embodiment, the modified NSY molecular sieve contains rare earth (the modified Y molecular sieve containing rare earth is also called the NSY molecular sieve containing rare earth), and its rare earth content is preferably 10 wt% to 20 wt% in terms of RE2O3. When the rare earth content of the modified NSY molecular sieve is within this range, the catalytic cracking catalyst can have a higher heavy oil conversion activity.
[0013] The present invention provides a method for preparing a catalytic cracking catalyst, comprising the following steps:
[0014] (S1) preparing a modified NSY molecular sieve;
[0015] (S2) slurrying clay, cracking active components including modified NSY molecular sieve and optional second molecular sieve, and a binder;
[0016] (S3) spray drying the slurry obtained in step S2.
[0017] According to the preparation method of the catalytic cracking catalyst provided by the present invention, the modified NSY molecular sieve is a modified kaolin in-situ crystallized NSY molecular sieve (hereinafter referred to as in-situ crystallized NSY molecular sieve) obtained by modification treatment.
[0018] According to the preparation method of the catalytic cracking catalyst provided by the present invention, the preparation method of the modified NSY molecular sieve can be obtained by modifying the NSY molecular sieve synthesized by in-situ crystallization of kaolin. The NSY molecular sieve synthesized by in-situ crystallization of kaolin is a Y-type molecular sieve composite material. The crystallinity of the NSY molecular sieve synthesized by in-situ crystallization of kaolin (or the Y-type molecular sieve composite material) measured by the X-ray diffraction method is ≥60% by the peak height method, and the ratio of the crystallinity to the peak area method is K1, K1=0.76~0.89; the silicon-aluminum ratio measured by the unit cell constant a0 is 5.0~5.5, and the ratio to the silicon-aluminum ratio measured by the chemical method is K2, K2=0.87~0.90, and the silicon-aluminum ratio is the molar ratio of silicon oxide to aluminum oxide. The modified NSY molecular sieve is a molecular sieve material obtained by modifying the NSY molecular sieve synthesized by in-situ crystallization of kaolin, wherein the modification reduces the sodium oxide content in the NSY molecular sieve synthesized by in-situ crystallization of kaolin to below 2 wt %. The modification may be, for example, ion exchange.
[0019] The NSY molecular sieve synthesized by in-situ crystallization of kaolin described in the present invention has spherical bodies of 5 to 20 microns, wherein the crystallinity measured by the peak height method is ≥60%, that is, the mass percentage of the NaY molecular sieve is at least 60%. Preferably, the crystallinity measured by the peak height method is greater than 75%, more preferably ≥80%.
[0020] According to the common sense of crystallization, the difference between the crystallinity measured by the peak height method and the crystallinity measured by the peak area method is related to the size of the crystal grains. The Y-type molecular sieve composite material of the present invention (hereinafter referred to as the composite material) sets the crystal factor K1, K1 = S 峰高 / S 峰面积 , that is, the ratio of the crystallinity measured by the peak height method to the crystallinity measured by the peak area method. The size of the K1 value indicates the size of the crystallites. The larger the K1 value, the larger the crystallite size. The preferred K1 is 0.80 to 0.89, and more preferably 0.80 to 0.85.
[0021] The molar ratio of silicon oxide to aluminum oxide calculated by the unit cell constant a0 is the framework silicon-aluminum ratio of the molecular sieve, and the molar ratio of silicon oxide to aluminum oxide determined by the chemical method is the overall silicon-aluminum ratio of the composite material. The NSY molecular sieve synthesized by kaolin in-situ crystallization of the present invention has a framework silicon-aluminum ratio of 5.0 to 5.5, preferably 5.2 to 5.5, determined by the unit cell constant a0, and the overall silicon-aluminum ratio determined by the chemical method is the macroscopic silicon-aluminum ratio of the entire material. The two values of the framework silicon-aluminum ratio and the overall silicon-aluminum ratio are related to the framework integrity and purity of the molecular sieve in the composite material. The NSY molecular sieve synthesized by kaolin in-situ crystallization of the present invention is obtained by crystallization of metakaolin, in which a part of the metakaolin is in the intermediate of crystallization to Y-type molecular sieve, therefore, the intermediate system coefficient K2 is set, i.e., K2=framework silicon-aluminum ratio / overall silicon-aluminum ratio. The size of the K2 value indicates the degree of compositeness of the composite material. The smaller the K2 value, the more intermediates are contained. The preferred K2 is 0.87 to 0.92, and more preferably 0.88 to 0.90.
[0022] The NSY molecular sieve (also called Y-type molecular sieve composite material) synthesized by in-situ crystallization of kaolin described in the present invention preferably has K1=0.77-0.88, for example, K1=0.81-0.88 or K1=0.86-0.88 and K2=0.87-0.91.
[0023] In the present invention, pores with a pore diameter greater than 0.8 nm are defined as medium and macropores. The NSY molecular sieve synthesized by in-situ crystallization of kaolin described in the present invention has a suitable medium and macropore ratio, wherein the macropore ratio is 10-20%.
[0024] According to the preparation method of the catalytic cracking catalyst provided by the present invention, the NSY molecular sieve synthesized by in-situ crystallization of kaolin described in the present invention is a Y-type molecular sieve composite material. One preparation method thereof comprises the following steps: (1) calcining and dehydrating kaolin at 500-900° C. to convert it into metakaolin, and crushing it to prepare metakaolin powder with a particle size of less than 10 microns; (2) adding sodium silicate, a directing agent, a sodium hydroxide solution and water to the metakaolin powder to prepare a molar ratio of (1-2.5) Na2O: The invention relates to a reaction raw material A of Al2O3: (4-9) SiO2: (40-100) H2O, wherein the mass ratio of the directing agent to the kaolin is 0.01-1.0; (3) crystallizing the reaction raw material A under stirring at 88-98°C, and adding a second silicon source after the crystallization time reaches 1-70 hours to obtain a reaction raw material B, wherein the second silicon source accounts for 0.1-10 weight % of the total silicon feed, all calculated as silicon oxide; (4) crystallizing the reaction raw material B under stirring at 88-98°C and recovering the product.
[0025] According to the preparation method of the catalytic cracking catalyst provided by the present invention, in the preparation method of NSY molecular sieve synthesized by in-situ crystallization of kaolin, the directing agent can be synthesized according to conventional methods, such as according to the preparation methods of USP3574538, USP3639099, USP3671191, USP4166099, and EUP0435625. The molar composition of the directing agent is: (10-17) SiO2: (0.7-1.3) Al2O3: (11-18) Na2O: (200-350) H2O. During the synthesis, the raw materials are aged at 4-35°C, preferably 4-20°C to obtain the directing agent.
[0026] According to the preparation method of the catalytic cracking catalyst provided by the present invention, in the preparation method of the NSY molecular sieve synthesized by in-situ crystallization of kaolin, the sodium content of the second silicon source is 0.01% by weight to 10% by weight, preferably less than 1% by weight, calculated as Na2O. Considering the cost control factor, the preferred second silicon source is solid silica gel. The solid silica gel is included in the total synthesis ratio, and the solid silica gel used can be solid silica gel of different pore sizes. According to the pore size, there are fine-pore silica gel, coarse-pore silica gel and medium-pore silica gel between the two. It is customary to call silica gel with an average pore size of less than 1.5-2.0nm as fine-pored silica gel (e.g., type A solid silica gel from Qingdao Ocean Chemical Group Special Silica Gel Factory), and silica gel with an average pore size of more than 4.0-5.0nm as coarse-pored silica gel (e.g., type C solid silica gel from Qingdao Ocean Chemical Group Special Silica Gel Factory); in addition, silica gel with an average pore size of more than 10.0nm is called extra coarse-pored silica gel, and silica gel with an average pore size of less than 0.8nm is called extra fine-pored silica gel (e.g., type B solid silica gel from Qingdao Ocean Chemical Group Special Silica Gel Factory). The second silicon source may also be liquid silica gel. When liquid silica gel is used as the second silicon source, preferably, the mass content of SiO2 therein is at least 30%.
[0027] According to the preparation method of the catalytic cracking catalyst provided by the present invention, in the preparation method of the NSY molecular sieve synthesized by in-situ crystallization of kaolin, a multi-level pore Y-type molecular sieve composite material product containing certain medium and large pores is obtained by crystallization under stirring, and the crystallization stirring speed can be, but is not limited to, 50 to 1000 rpm, preferably 300 to 500 rpm, and the time is 16 to 48 hours, preferably 24 to 32 hours. The drying temperature of the zeolite after crystallization is 100 to 120°C.
[0028] According to the preparation method of the catalytic cracking catalyst provided by the present invention, in the preparation method of the NSY molecular sieve synthesized by in-situ crystallization of kaolin, the second silicon source accounts for 0.1-10 weight % of the total silicon feed, preferably 4-10 weight %.
[0029] According to the preparation method of the catalytic cracking catalyst provided by the present invention, in the preparation method of the NSY molecular sieve synthesized by kaolin in-situ crystallization, sodium silicate and the second silicon source are added into the synthesis preparation system in different processes, and the second silicon source is added during the crystal growth period. The present invention combines the means of adding different silicon sources at different stages of the crystallization process to control the synthesis ratio technology with the kaolin in-situ crystallization synthesis technology (using natural minerals as the main aluminum source and silicon source), changes the crystal growth environment through the silicon source, and adopts two completely different material ratios in the crystal nucleation period and the crystal growth period. In the crystal nucleation period, the method of the present invention adopts a larger sodium-silicon ratio (Na2O / SiO2) in the material, which is conducive to the rapid nucleation of the Y-type molecular sieve, and in the crystal growth period, a low-sodium or sodium-free silicon source is added to increase the silicon-aluminum ratio (SiO2 / A12O3) in the synthetic material, while reducing the sodium-silicon ratio (Na2O / SiO2) in the material, which is conducive to the improvement of the product silicon-aluminum ratio under the premise of shortening the crystallization time, and the skeleton silicon-aluminum ratio is increased to 5.0-5.5.
[0030] According to the preparation method of the catalytic cracking catalyst provided by the present invention, in the preparation step (4) of the NSY molecular sieve synthesized by in-situ crystallization of kaolin, the product is recovered after the crystallization is completed to obtain the NSY molecular sieve synthesized by in-situ crystallization of kaolin. The recovery generally includes a filtering step, and optionally, may also include one or more processes of washing, drying, and roasting.
[0031] According to the preparation method of the catalytic cracking catalyst provided by the present invention, the preparation method of the modified NSY molecular sieve comprises: subjecting the above-mentioned recovered product to a modification treatment such as ion exchange to obtain the modified NSY molecular sieve.
[0032] According to the preparation method of the catalytic cracking catalyst provided by the present invention, the NSY molecular sieve synthesized by in-situ crystallization of kaolin can be treated by any method capable of reducing the sodium content so that the sodium oxide content therein does not exceed 2% by weight, for example, a modified NSY molecular sieve is obtained by ion exchange. The ion exchange can be carried out using ammonium salt and / or rare earth salt solution, and the present invention has no special requirements. Preferably, the ion exchange makes the rare earth content in the obtained modified NSY molecular sieve be 10% to 20% by weight in terms of RE2O3, and the sodium oxide content is less than 2% by weight. In one embodiment, the NSY molecular sieve synthesized by in-situ crystallization of kaolin is mixed with an exchange solution and stirred at 20 to 90°C for 10 to 120 minutes. The above process can be carried out once or multiple times, and the exchange solution exchanged each time can contain ammonium ions, rare earth ions, or both ammonium ions and rare earth ions. Preferably, the concentration of ammonium salt in the exchange solution is 5-700 g / L, for example, 5-100 g / L and / or the concentration of rare earth salt is 5-400 g / L, for example, 5-200 g / L in terms of RE2O3. The ammonium salt is, for example, one or more of ammonium chloride, ammonium nitrate, and ammonium sulfate. The rare earth salt is, for example, one or more of rare earth chloride and rare earth nitrate. The rare earth may include one or more of lanthanide rare earths and actinide rare earths, for example, one or more of La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, TB, Dy, Ho, Er, Tm, Yb, and Lu.
[0033] According to the preparation method of the catalytic cracking catalyst provided by the present invention, the NSY molecular sieve synthesized by in-situ crystallization of kaolin may further include one or more steps of filtration, washing, drying and calcination after ion exchange. These steps may refer to the filtration, washing, drying and calcination methods well known to those skilled in the art.
[0034] In the method for preparing a catalytic cracking catalyst provided by the present invention, in step S2, clay, modified NSY molecular sieve, optional second molecular sieve and binder are made into slurry, and clay, modified NSY molecular sieve, optional second molecular sieve, binder and water are mixed and stirred evenly.
[0035] According to the preparation method of the catalytic cracking catalyst provided by the present invention, in step S3, the slurry obtained in step S2 is spray dried to obtain catalyst microsphere particles, and the catalyst microsphere particles can be further calcined and / or washed, and the washing can be performed before and / or after calcination. The spray drying, washing and calcination can be performed according to the existing catalytic cracking catalyst production spray drying and calcination methods. For example, the washing is such as washing with an ammonium salt solution, and the calcination can be performed at 350 to 650°C, and the calcination temperature can be 1 to 4 hours.
[0036] The catalytic cracking catalyst provided by the present invention has good coke selectivity and can reduce coke selectivity on the basis of having high hydrocarbon oil conversion catalytic activity. Preferably, the catalytic cracking catalyst provided by the present invention can also have higher hydrocarbon oil conversion activity and / or liquid product yield. DETAILED DESCRIPTION
[0037] The following specific embodiments and examples are used to further illustrate the present invention. It should be understood that the specific embodiments and implementations described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0038] The catalytic cracking catalyst provided by the present invention comprises: 10-70 wt %, such as 20-60 wt % or 25-65 wt %, of a cracking active component, 10-60 wt %, such as 20-45 wt %, of a binder and 10-70 wt %, such as 20-60 wt % or 25-55 wt % of clay, wherein the cracking active component comprises 5-100 wt %, such as 40-100 wt %, of a first Y-type molecular sieve and 0-95 wt %, such as 0-60 wt %, of a second molecular sieve.
[0039] The catalytic cracking catalyst provided by the present invention may also contain a second molecular sieve, and the second molecular sieve is preferably faujasite and / or a molecular sieve with a five-membered ring structure, and the faujasite is, for example, one or more of HY, REY, REHY, USY, REUSY, DASY and REDASY. The molecular sieve with a five-membered ring structure is, for example, a BEA structure molecular sieve, an MFI structure molecular sieve, or a mordenite, and is preferably one or more of a BEA structure molecular sieve and an MFI structure molecular sieve. The BEA structure molecular sieve may be obtained by crystallization without amine, or may be obtained by calcining a molecular sieve prepared by a template method, for example, the BEA structure molecular sieve is, for example, a β molecular sieve; the MFI structure molecular sieve is, for example, at least one of a rare earth-containing MFI structure molecular sieve, a phosphorus-containing MFI structure molecular sieve, an iron-containing MFI structure molecular sieve, and a phosphorus- and transition metal-containing MFI structure molecular sieve; the mordenite is, for example, at least one of a high-silicon mordenite or a low-silicon mordenite.
[0040] The catalytic cracking catalyst provided by the present invention contains clay, and the clay can be one or more of kaolin, halloysite, montmorillonite, diatomite, halloysite, pseudo-halloysite, saponite, rectorite, sepiolite, attapulgite, hydrotalcite and bentonite.
[0041] The catalytic cracking catalyst provided by the present invention contains a binder, and the binder can be selected from one or more of silica sol, aluminum sol, acidified aluminum stone (pseudo-boehmite, referred to as aluminum stone in the present invention), and metal-modified aluminum stone.
[0042] In the catalytic cracking catalyst provided by the present invention, the first Y-type molecular sieve is a modified NSY molecular sieve, preferably a rare earth-containing NSY molecular sieve, whose rare earth content is 10% to 20% by weight in terms of RE2O3, and the sodium oxide content does not exceed 2% by weight, preferably does not exceed 1.5% by weight.
[0043] In one embodiment, the modified NSY molecular sieve is prepared according to the following steps:
[0044] (1) calcining kaolin at 500-900°C to dehydrate it and convert it into metakaolin, which is then crushed to form a powder with a particle size of less than 10 microns;
[0045] (2) adding sodium silicate, a directing agent, a sodium hydroxide solution and water to the metakaolin powder to prepare a reaction slurry, wherein the mass ratio of the directing agent to the metakaolin is 0.01 to 1.0;
[0046] (3) crystallizing the reaction slurry obtained in (2) at 88 to 98° C. under stirring for 1 to 70 h, for example, 5 to 40 h, 6 to 30 h, or 8 to 16 h, and then adding solid silica gel, wherein the mass ratio of solid silica gel to metakaolin is 0.01 to 1.0;
[0047] (4) crystallizing the reaction raw material obtained in (3) at 88-98° C. under stirring for 1-20 h, such as 8-20 h or 12-16 h, and then filtering and drying to obtain an in-situ crystallized NSY molecular sieve; and
[0048] (5) contacting the obtained in-situ crystallized NSY molecular sieve with an ammonium salt and / or rare earth salt solution to carry out ion exchange, filtering, washing, drying and calcining to obtain a modified NSY molecular sieve, wherein the rare earth content in the modified NSY molecular sieve is preferably 10 wt% to 20 wt% in terms of RE2O3, and the sodium oxide content is less than 2 wt%. The contacting may be carried out once or multiple times, and each contact exchange may be carried out with a solution containing both rare earth ions and ammonium ions, or with a solution containing one of the ions to carry out ammonium ion exchange or rare earth ion exchange.
[0049] In one embodiment, the NSY molecular sieve synthesized by in-situ crystallization contains 20% to 30% by weight of an intermediate of metakaolin to Y-type molecular sieve crystallization. Due to the presence of the intermediate, K2 is in the range of 0.87 to 0.93.
[0050] In the embodiments and comparative examples:
[0051] The element content in the catalyst was determined by XRF, and the specific surface area and pore volume were determined by low-temperature nitrogen adsorption-desorption method.
[0052] The raw material specifications used in the catalyst preparation example are as follows:
[0053] Pseudo-boehmite (abbreviated as diaspore): product of Shandong Aluminum Company, solid content 75% by weight;
[0054] Kaolin: solid content 75% by weight, produced by China Kaolin Co., Ltd. (Suzhou);
[0055] REY molecular sieve: product of Sinopec Catalyst Co., Ltd. Qilu Branch, rare earth content 17.6% by weight;
[0056] ZSP-3 molecular sieve: a product of Qilu Branch of Sinopec Catalyst Co., Ltd., with a P2O5 content of 3.02% by weight.
[0057] Aluminum sol: a product of Qilu Branch of Sinopec Catalyst Co., Ltd., with a solid content of 23% by weight.
[0058] The content of NaY zeolite in the composite material in the example is determined according to the RIPP146-90 standard method (the RIPP standard method is shown in "Petrochemical Analysis Method (RIPP Test Method)", edited by Yang Cuiding et al., Science Press, published in 1990, the same below).
[0059] The unit cell constant a0 is determined according to the RIPP 145-90 standard method. The framework silicon-aluminum ratio is calculated from the unit cell constant a0 (angstroms) according to the following formula: SiO2 / Al2O3 (molar ratio) = 2×(25.858-a0) / (a0-24.191).
[0060] The specific surface area was determined by nitrogen adsorption method (GB / T5816-1995); the pore volume was determined by nitrogen adsorption method (RIPP151-90). The pores with a mesopore diameter greater than 0.8 nm determined by nitrogen adsorption method were defined as mesopores and macropores. The mesopore ratio was calculated as (V 总孔 -V 微孔 ) / V 总孔 ×100%.
[0061] In the examples and comparative examples, the preparation of the guiding agent is as follows: 250 kg of sodium silicate solution (containing 20.05 wt% SiO2 and 6.41 wt% Na2O) is slowly added with 120 kg of sodium aluminate solution (containing 3.15 wt% Al2O3 and 21.1 wt% Na2O) at 30°C under rapid stirring, stirred for 1 hour, aged at 20°C for 48 hours to obtain the guiding agent. The guiding agent has a composition of 16Na2O:Al2O3:15SiO2:320H2O.
[0062] Molecular sieve preparation example 1
[0063] 100 kg of pulverized metakaolin powder was stirred and added with 400 kg of sodium silicate solution (containing 20.05 wt% SiO2, 6.41 wt% Na2O), 60 kg of directing agent and 100 kg of 5 wt% sodium hydroxide solution. The mixture was heated to 95°C and stirred at a constant temperature. After 8 hours, 10 kg of solid silica gel (Type A, from Qingdao Ocean Chemical Group Special Silica Gel Factory) was added and crystallized for 12 hours. The stirring speed during the addition and crystallization was 400 rpm. After the crystallization was completed, the crystallization tank was quenched, filtered and washed with water until the pH value of the washing liquid was less than 10. The mixture was dried at 120°C for 2 hours to obtain zeolite material Y-1. Y-1 was measured by X-ray diffraction method, and the crystallinity of the peak height method, the K1 value of the ratio of the crystallinity of the peak height method to the crystallinity of the peak area method, the silicon-aluminum ratio determined by the unit cell constant a0, the K2 value of the ratio of the silicon-aluminum ratio determined by the unit cell constant a0 to the silicon-aluminum ratio determined by the chemical method, and the medium and macro porosity are shown in Table 1.
[0064] Molecular sieve preparation example 2
[0065] According to the method of preparing the molecular sieve in Example 1, 100 kg of pulverized metakaolin powder was stirred and added with 380 kg of sodium silicate solution (containing 20.05% by weight of SiO2 and 6.41% by weight of Na2O), 60 kg of directing agent, and 100 kg of sodium hydroxide solution with a concentration of 5% by weight. The mixture was heated to 93°C and stirred at a constant temperature. After 8 hours, 15 kg of solid silica gel (special silica gel factory of Qingdao Ocean Chemical Group, type A) was added and crystallized for 14 hours. The stirring speed during the addition and crystallization was 400 rpm. After the crystallization was completed, the crystallization tank was quenched, filtered, and washed with water until the pH value of the washing liquid was less than 10. Dry at 120°C for 2 hours to obtain zeolite material Y-2. Y-2 was measured by X-ray diffraction method, and the crystallinity of the peak height method, the K1 value of the ratio of the crystallinity of the peak height method to the crystallinity of the peak area method, the silicon-aluminum ratio determined by the unit cell constant a0, the K2 value of the ratio of the silicon-aluminum ratio determined by the unit cell constant a0 to the silicon-aluminum ratio determined by the chemical method, and the medium and macro porosity are shown in Table 1.
[0066] Molecular sieve preparation example 3
[0067] According to the method of preparing the molecular sieve in Example 1, 100 kg of pulverized metakaolin powder was stirred and added with 360 kg of sodium silicate solution (containing 20.05 wt% SiO2, 6.41 wt% Na2O), 60 kg of directing agent, and 100 kg of sodium hydroxide solution with a concentration of 5 wt%. The mixture was heated to 95°C and stirred at a constant temperature. After 8 hours, 20 kg of solid silica gel (Special Silica Gel Factory of Qingdao Ocean Chemical Group, Type A) was added and crystallized for 16 hours. The stirring speed during the addition and crystallization was 400 rpm. After the crystallization was completed, the crystallization tank was quenched, filtered, and washed with water until the pH value of the washing liquid was less than 10. Dry at 120°C for 2 hours to obtain zeolite material Y-3. Y-3 was measured by X-ray diffraction method, and the crystallinity of the peak height method, the K1 value of the ratio of the crystallinity of the peak height method to the crystallinity of the peak area method, the silicon-aluminum ratio determined by the unit cell constant a0, the K2 value of the ratio of the silicon-aluminum ratio determined by the unit cell constant a0 to the silicon-aluminum ratio determined by the chemical method, and the medium and macro porosity are shown in Table 1.
[0068] Molecular sieve preparation comparative example 1
[0069] This comparative example illustrates the situation where two silicon sources are added into the reaction system at one time.
[0070] According to the method of preparing the molecular sieve in Example 1, 100 kg of pulverized metakaolin powder was stirred and added with 400 kg of sodium silicate solution (containing 20.05 wt% SiO2, 6.41 wt% Na2O), 60 kg of directing agent, 105 kg of 5 wt% sodium hydroxide solution, and 10 kg of solid silica gel (Qingdao Ocean Chemical Group Special Silica Gel Factory, Type A). The temperature was raised to 94°C and stirred at a constant temperature for 24 hours. The stirring speed during the addition and crystallization was 400 rpm. After the crystallization was completed, the crystallization tank was quenched, filtered, and washed with water until the pH value of the washing liquid was less than 10. Dry at 120°C for 2 hours to obtain the zeolite material DY-1. The crystallinity of DY-1 measured by X-ray diffraction method, the K1 value of the ratio of the crystallinity of the peak height method to the crystallinity of the peak area method, the silicon-aluminum ratio determined by the unit cell constant a0, the K2 value of the ratio of the silicon-aluminum ratio determined by the unit cell constant a0 to the silicon-aluminum ratio determined by the chemical method, and the medium- and macro-porosity are shown in Table 1. DY-1 has low crystallinity and contains impurities.
[0071] Molecular sieve preparation comparative example 2
[0072] This comparative example illustrates the case where no second silicon source is added.
[0073] According to the method of molecular sieve preparation example 1, 100 kg of pulverized metakaolin powder was stirred and added with 400 kg of sodium silicate solution (containing 20.05 wt% SiO2, 6.41 wt% Na2O), 60 kg of directing agent, and 100 kg of sodium hydroxide solution with a concentration of 5 wt%. The temperature was raised to 94°C and stirred at a constant temperature for 24 hours. The stirring speed during the addition and crystallization was 400 rpm. After the crystallization was completed, the crystallization tank was quenched, filtered, and washed with water until the pH value of the washing liquid was less than 10. Dry at 120°C for 2 hours to obtain zeolite DY-2. The crystallinity of DY-2 measured by the X-ray diffraction method, the K1 value of the ratio of the crystallinity of the peak height method to the crystallinity of the peak area method, the silicon-aluminum ratio determined by the unit cell constant a0, the K2 value of the ratio of the silicon-aluminum ratio determined by the unit cell constant a0 to the silicon-aluminum ratio determined by the chemical method, and the medium-macroporosity are shown in Table 1. The crystallinity of DY-2 is not bad, but the silicon-aluminum ratio is low.
[0074] Molecular sieve preparation comparative example 3
[0075] This comparative example illustrates the NaY molecular sieve prepared according to the method of CN101468803A.
[0076] 189 ml of deionized water, 86.6 g of directing agent, 130 ml of aluminum sulfate solution (product of the catalyst plant of Changling Oil Refinery and Chemical Plant, specific gravity 1.28, Al2O3 content 88.2 g / L) and 100 ml of low sodium aluminate solution (product of the catalyst plant of Changling Oil Refinery and Chemical Plant, specific gravity 1.23, Al2O3 content 102 g / L, Na2O content 151.9 g / L) were added to 401 ml of sodium silicate, and after strong stirring for 30 min, the product was allowed to stand at 100°C for crystallization for 33 h, and the product was recovered and numbered DY-3.
[0077] DY-3 was measured by X-ray diffraction method, and the crystallinity of the peak height method, the K1 value of the ratio of the crystallinity of the peak height method to the crystallinity of the peak area method, the silicon-aluminum ratio determined by the unit cell constant a0, the K2 value of the ratio of the silicon-aluminum ratio determined by the unit cell constant a0 to the silicon-aluminum ratio determined by the chemical method, and the medium and macro porosity are shown in Table 1.
[0078] Table 1
[0079]
[0080] Catalyst Preparation Example 1
[0081] (1) Preparation of modified NSY molecular sieve: Take zeolite material Y-1 and add deionized water to slurry to obtain a molecular sieve slurry with a solid content of 10 wt%; take lanthanum chloride and add water to slurry to form a lanthanum chloride solution with a La2O3 concentration of 5 wt%; add the lanthanum chloride solution to the molecular sieve slurry, and the weight ratio of lanthanum chloride (calculated as La2O3) to molecular sieve (calculated on a dry basis) is 1:6; stir at 70°C for 1 hour, filter, wash, dry at 150°C for 8 hours, and calcine at 500°C for 4 hours to obtain a modified NSY molecular sieve containing rare earth.
[0082] (2) Catalyst preparation: The catalyst formula is shown in Table 2. First, kaolin and water are slurried to obtain a kaolin slurry with a solid content of 20% by weight; the modified NSY molecular sieve containing rare earth is slurried with water and dispersed with a homogenizer to obtain a modified NSY molecular sieve slurry with a solid content of 35% by weight; the kaolin slurry and the modified NSY molecular sieve slurry are mixed and stirred, and then an acidified aluminum stone with a solid content of 10% by weight is added (wherein the acidified aluminum stone, the molar ratio of HCl to aluminum stone based on Al2O3 is 0.2), stirred for 10 minutes, and finally aluminum sol is added and stirred for 30 minutes to obtain a catalyst slurry. The catalyst slurry is spray-dried to obtain catalyst microspheres, and the obtained catalyst microspheres are calcined at 500°C for 2 hours, and then washed with an ammonium sulfate solution with an ammonium sulfate concentration of 2% by weight, and the weight ratio of the ammonium sulfate solution to the catalyst microsphere dry basis is 10:1 to obtain a catalytic cracking catalyst C1.
[0083] Catalyst Preparation Examples 2 to 6
[0084] The catalyst was prepared according to the method of Example 1, by adjusting the weight ratio of lanthanum chloride (calculated as La2O3) to molecular sieve (calculated as dry basis), or by performing the process multiple times to obtain a modified NSY molecular sieve. The rare earth content in the zeolite material used and the modified NSY molecular sieve obtained is shown in Table 2, wherein the ZSP-3 molecular sieve was slurried with water to form a ZSP-3 molecular sieve slurry with a solid content of 35% by weight, mixed with kaolin slurry and modified NSY molecular sieve slurry, and then the acidified aluminum stone was added, stirred for 10 minutes, and then aluminum sol was added, stirred for 30 minutes, and spray dried and the calcined and washed. The catalyst formula is shown in Table 2.
[0085] Table 2
[0086]
[0087] The formulation composition in Table 2 is calculated on a dry basis, the rare earth content in the modified NSY molecular sieve is calculated on a RE2O3 basis, and B in the catalyst preparation example number represents a comparative example.
[0088] In Table 2, in catalysts DB2 to DB4, the corresponding modified NSY molecular sieve content, rare earth content in the modified NSY molecular sieve and Na2O content in the modified NSY molecular sieve are the percentage content of the modified Y molecular sieve obtained after rare earth exchange of DY-1 to DY-3 in the catalyst, the rare earth content in the corresponding modified Y molecular sieve and the sodium oxide content, respectively.
[0089] Catalyst Preparation Comparative Examples 1 to 4
[0090] The catalyst was prepared according to the method of Catalyst Preparation Example 1. The catalyst formula is shown in Table 2.
[0091] Catalyst Evaluation:
[0092] The catalyst was deactivated by aging at 800°C and 100% steam for 24 hours. The catalyst was evaluated on a fixed fluidized bed microreactor ACE. The feedstock oil was Wu-mixed feedstock oil (composition and physical properties are shown in Table 3. The evaluation conditions were: reaction temperature of 500°C, catalyst-to-oil ratio (weight) of 6, WHSV of 16h -1 The results are listed in Table 4.
[0093] Among them, conversion rate = gasoline yield + liquefied gas yield + dry gas yield + coke yield
[0094] Total liquid yield = gasoline yield + liquefied gas yield + circulating oil yield
[0095] Coke selectivity = coke yield / conversion rate × 100
[0096] Coke factor = coke yield × (1-conversion rate) / conversion rate × 100
[0097] The coke generation factor is an important indicator for judging the coke selectivity of catalysts. The smaller the coke generation factor, the better the coke selectivity of the catalyst.
[0098] Table 3
[0099]
[0100] Table 4
[0101]
[0102] As can be seen from Table 4, compared with the catalytic cracking catalyst provided in the comparative example, the catalytic cracking catalyst provided by the present invention can reduce the coke selectivity and significantly reduce the coke generation factor in the catalytic cracking reaction while having a higher conversion rate. Preferably, the conversion rate can be further improved and the total liquid yield can be increased.
Claims
1. A catalytic cracking catalyst comprising: 10-70 wt% of a cracking active component, 10-60 wt% of a binder and 10-70 wt% of clay, wherein the cracking active component comprises 5-100 wt% of a first Y-type molecular sieve and 0-95 wt% of a second molecular sieve; wherein the first Y-type molecular sieve is a modified NSY molecular sieve obtained by modifying an NSY molecular sieve synthesized by in-situ crystallization of kaolin, and the sodium oxide content of the modified NSY molecular sieve is less than 2 wt%; the NSY molecular sieve synthesized by in-situ crystallization of kaolin is Molecular sieve, measured by X-ray diffraction method, the crystallinity of the peak height method is ≥60%, and the ratio of the crystallinity to the peak area method is K1, K1=0.76-0.89; the silicon-aluminum ratio measured by the unit cell constant a0 is 5.0-5.5, and the ratio to the silicon-aluminum ratio measured by the chemical method is K2, K2=0.87-0.93, and the silicon-aluminum ratio is the molar ratio of silicon oxide to aluminum oxide; the NSY molecular sieve synthesized by in-situ crystallization of kaolin, and its preparation method comprises the following steps: (1) calcining and dehydrating kaolin at 500-900° C. to convert it into metakaolin, and crushing it into metakaolin powder with a particle size of less than 10 μm; (2) adding a directing agent, sodium silicate, sodium hydroxide solution and water to the metakaolin powder to prepare a reaction raw material A, wherein the mass ratio of the directing agent to the metakaolin is 0.01-1.0, and the ratio of the reaction raw material A is (1-2.5) Na2O:Al2O3:(4-9)SiO2:(40-100)H2O in molar ratio; (3) crystallizing the reaction raw material A at 88-98° C. for 1-70 hours under stirring, and then adding a second silicon source to obtain a reaction raw material B, wherein the second silicon source accounts for 0.1-10% by weight of the total silicon feed, calculated as silicon oxide; (4) crystallizing the reaction raw material B at 88-98° C. under stirring and recovering the product; The sodium content of the second silicon source is less than 1% by weight in terms of Na2O.
2. The catalytic cracking catalyst according to claim 1, wherein The crystallinity determined by the peak height method is ≥80%.
3. The catalytic cracking catalyst according to claim 1, wherein The K1=0.80-0.
89.
4. The catalytic cracking catalyst according to claim 1, wherein The K1=0.80-0.
85.
5. The catalytic cracking catalyst according to claim 1, wherein The K2=0.87~0.
92.
6. The catalytic cracking catalyst according to claim 1, wherein The K2=0.88-0.
90.
7. The catalytic cracking catalyst according to claim 1, wherein The K1 is 0.77 to 0.88 and K2 is 0.87 to 0.
91.
8. The catalytic cracking catalyst according to claim 1, wherein The large mesopore ratio of the NSY molecular sieve synthesized by in-situ crystallization of kaolin is 10-20%.
9. The catalytic cracking catalyst according to claim 1, wherein The silicon-aluminum ratio measured by the unit cell constant a0 is 5.2-5.
5.
10. The catalytic cracking catalyst according to any one of claims 1 to 9, wherein The modified NSY molecular sieve contains rare earth, and the rare earth content in the modified NSY molecular sieve is 10 wt% to 20 wt% calculated as RE2O3.
11. The catalytic cracking catalyst according to claim 1, wherein The second molecular sieve is selected from faujasite and / or a molecular sieve with a five-membered ring structure; the faujasite is one or more of HY, REY, REHY, USY, REUSY, DASY and REDASY; the molecular sieve with a five-membered ring structure includes one or more of BEA structure molecular sieve, MFI structure molecular sieve and mordenite; the binder is selected from one or more of silica sol, alumina sol, acidified pseudo-boehmite and metal-modified pseudo-boehmite; the clay is one or more of kaolin, montmorillonite, diatomaceous earth, halloysite, saponite, rectorite, sepiolite, attapulgite, hydrotalcite and bentonite.
12. The method for preparing the catalytic cracking catalyst according to any one of claims 1 to 11, comprising the following steps: (1) preparing modified NSY molecular sieve; (2) forming a slurry with clay, cracking active components and a binder; the cracking active components include the modified NSY molecular sieve and an optional second molecular sieve; (3) spray drying the slurry obtained in step (2).
13. The method for preparing a catalytic cracking catalyst according to claim 12, wherein: The preparation method of the modified NSY molecular sieve comprises the following steps: (1) calcining kaolin at 500-900° C. to dehydrate and convert it into metakaolin, and crushing it to prepare metakaolin powder with a particle size of less than 10 μm; (2) adding sodium silicate, a directing agent, a sodium hydroxide solution and water to a metakaolin powder to prepare a reaction raw material A having a ratio of (1-2.5) Na2O:Al2O3:(4-9)SiO2:(40-100)H2O, wherein the mass ratio of the directing agent to the metakaolin is 0.01-1.0; (3) crystallizing the reaction raw material A at 88-98° C. under stirring, and adding a second silicon source after the crystallization time reaches 1-70 hours to obtain the reaction raw material B, wherein the second silicon source accounts for 0.1% to 10% by weight of the total silicon feed, calculated as silicon oxide; (4) crystallizing the reaction raw material B at 88-98° C. under stirring and recovering the product; (5) Recover the product and conduct ion exchange.
14. The method for preparing a catalytic cracking catalyst according to claim 13, wherein: The composition of the directing agent is: (10-17) SiO2: (0.7-1.3) Al2O3: (11-18) Na2O: (200-350) H2O.
15. The preparation method according to claim 13, wherein The sodium content of the second silicon source is less than 1% by weight in terms of Na2O.
16. The method for preparing a catalytic cracking catalyst according to claim 15, wherein: The second silicon source is solid silica gel.
17. The method for preparing a catalytic cracking catalyst according to claim 16, wherein: The average pore size of the solid silica gel is 1.5 to 2.0 nm, or the average pore size of the solid silica gel is 4.0 to 5.0 nm, or the average pore size of the solid silica gel is above 10.0 nm, or the average pore size of the solid silica gel is below 0.8 nm.
18. The method for preparing a catalytic cracking catalyst according to claim 15, wherein: The second silicon source is liquid silica gel.
19. The method for preparing a catalytic cracking catalyst according to claim 18, wherein: The mass content of SiO2 in the liquid silica gel is 1-30%.
20. The method for preparing a catalytic cracking catalyst according to claim 13, wherein: Calculated as silicon oxide, the second silicon source accounts for 4-10 weight % of the total silicon input.
21. The method for preparing a catalytic cracking catalyst according to claim 13, wherein: The ion exchange in step (5) is ammonium ion exchange and / or rare earth ion exchange.
22. The method for preparing a catalytic cracking catalyst according to claim 21, wherein: The ion exchange product obtained in step (5) is further calcined.
23. The method for preparing a catalytic cracking catalyst according to claim 22, wherein: The ion exchange includes rare earth ion exchange. The rare earth content of the modified NSY molecular sieve obtained in step (5) is 10% to 20% by weight in terms of RE2O3, and the sodium oxide content is less than 2% by weight.
24. A catalytic cracking method, comprising the step of contacting hydrocarbon oil with the catalytic cracking catalyst according to any one of claims 1 to 11.
Citation Information
Patent Citations
Method for synthesizing fine grain NaY molecular sieve
CN101468803A
NaY molecular sieve / natural mineral composite material having multistage pore structure and preparation method thereof
CN103043680A
Process for preparing high silica faujasite
US3574538A
Preparation of high-silica faujasite