Polarizing plate and method for manufacturing the same, and image display device

A polarizing film that absorbs and orients iodine on a polyvinyl alcohol-based resin layer uses a urea compound to suppress the decrease in transmittance in high-temperature environments, solving the problem of lower transmittance of polarizing plates in image display devices and improving durability. and visibility.

CN113906321BActive Publication Date: 2024-10-15SUMITOMO CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080039111.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-06-14
Filing Date
2020-05-25
Publication Date
2024-10-15
Estimated Expiration
2040-05-25

AI Technical Summary

Technical Problem

In an image display device composed of interlayer filling in a high-temperature environment, the transmittance of the polarizing plate is significantly reduced, resulting in problems of reduced visibility and insufficient durability.

Method used

A polyvinyl alcohol-based resin polarizing film containing urea, urea derivatives or thiourea derivatives is used. By adsorbing iodine on the polyvinyl alcohol-based resin layer and orienting the iodine, the polarizing film formed is characterized by its excellent transmittance in high-temperature environments. and polarization reduction suppression effect.

Benefits of technology

It effectively suppresses the decrease in transmittance in high-temperature environments, improves the durability of the polarizing plate, and ensures display characteristics and visibility in high-temperature environments in image display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113906321B_ABST
    Figure CN113906321B_ABST
Patent Text Reader

Abstract

The present invention aims to provide a polarizing plate which, when used in an image display device with an interlayer filling structure, has a small decrease in transmittance under high temperature environment and excellent durability, and a method for manufacturing the polarizing plate, and further provides a durable image display device with improved display characteristics under high temperature environment. The present invention provides a polarizing plate, characterized in that it is a polarizing plate having a polyvinyl alcohol-based resin polarizing film formed by absorbing and orienting iodine, and a protective film formed on at least one surface of the polarizing film, wherein the polarizing film contains at least one urea compound selected from urea, urea derivatives, thiourea, and thiourea derivatives.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polarizing plate and a method for producing the same, and also to an image display device in which one surface of the polarizing plate is bonded to an image display unit and the other surface is bonded to a transparent member such as a touch panel or a front panel. Background Art

[0002] Liquid crystal display devices (LCD) are not only used in liquid crystal televisions, but are also widely used in personal computers, mobile devices such as mobile phones, and in-vehicle applications such as navigation systems. Generally, a liquid crystal display device has a liquid crystal panel member with polarizing plates attached to both sides of a liquid crystal cell with an adhesive, and displays are performed by controlling light from a backlight member using the liquid crystal panel member.

[0003] In recent years, organic EL display devices have also begun to be widely used in televisions, mobile devices such as mobile phones, and in-vehicle applications such as navigation devices, just like liquid crystal display devices.

[0004] In an organic EL display device, in order to prevent external light from being reflected by the metal electrode (cathode) and observed as a mirror surface, a circular polarizing plate (a laminate including a polarizing element and a λ / 4 plate, sometimes simply referred to as a polarizing plate) is sometimes arranged on the visible side surface of the image display panel.

[0005] As mentioned above, polarizing plates are increasingly being installed in vehicles as components of liquid crystal display devices and organic EL display devices. Polarizing plates used in vehicle-mounted image display devices are more often exposed to high-temperature environments than those used in other mobile devices such as televisions and mobile phones, and are required to have less change in characteristics under high temperatures (high-temperature durability).

[0006] On the other hand, for the purpose of preventing damage to the image display panel caused by impact from the external surface, the configuration of providing a front panel (also called a "window layer" or the like) such as a transparent resin plate or a glass plate on the visible side of the image display panel relative to the polarizing plate is increasing. In addition, in a display device having a touch panel, a configuration of providing a touch panel on the visible side of the image display panel relative to the polarizing plate and providing a front panel on the visible side relative to the touch panel is widely adopted.

[0007] In this structure, if there is an air layer between the image display panel and transparent components such as the front panel and the touch panel, reflected glare of external light caused by the reflection of light is generated at the interface of the air layer, and the visibility of the picture tends to decrease. Therefore, the use of a structure in which the space between the polarizing plate arranged on the visible side surface of the image display panel and the front transparent component is filled with a material having a refractive index close to these materials (hereinafter sometimes referred to as an "interlayer filling structure") is expanding. As an interlayer filling material, an adhesive or a UV curing adhesive is used for the purpose of suppressing the reduction in visibility caused by reflection at the interface and bonding and fixing the components together (for example, refer to Patent Document 1).

[0008] The above-mentioned interlayer filling structure is increasingly being adopted in mobile devices such as mobile phones that are often used outdoors. In addition, due to the increasing demand for visibility in recent years, in vehicle-mounted applications such as navigation devices, a structure is also being studied in which a front panel is arranged on the surface of the image display panel and an interlayer filling is performed between the panels with an adhesive layer or the like.

[0009] However, when such a structure is adopted, there have been reports that the results of a heat durability test (conducted at 95°C for 200 hours, etc.) showed that a significant decrease in transmittance was observed in the central part of the polarizing plate surface. On the other hand, in the case of a single polarizing plate, no significant decrease in transmittance was observed even under the conditions of 95°C and 1000 hours. There have also been reports that, based on these results, a significant decrease in the transmittance of the polarizing plate in a high-temperature environment is a problem unique to the case where an image display device using an interlayer filling structure in which one surface of the polarizing plate is bonded to an image display unit and the other surface is bonded to a transparent component such as a touch panel or a front panel is exposed to a high-temperature environment (Patent Document 2).

[0010] In addition, in the above-mentioned Patent Document 2, the polarizing plate having an interlayer filler structure and a significantly reduced transmittance has a Raman spectroscopic measurement at 1100 cm -1 Nearby (from =CC= key) and 1500cm -1 There is a peak near (derived from the -C=C- bond), so it is considered that a polyene structure (-C=C) is formed. n -, which is presumably caused by polyenylation of the polyvinyl alcohol forming the polarizing element due to dehydration (Patent Document 2, paragraph

[0012] ).

[0011] In addition, the inventors conducted Raman spectroscopy on samples subjected to high temperature durability tests using interlayer filling structures and observed that a decrease in transmittance at 1100 cm -1 Near 1500cm -1 The sum of the areas of nearby peaks is increasing.

[0012] As a solution to this problem, Patent Document 2 proposes a method of suppressing a decrease in transmittance by setting the moisture content per unit area of ​​the polarizing plate to a predetermined amount or less and setting the saturated water absorption of a transparent protective film adjacent to the polarizing element to a predetermined amount or less.

[0013] However, the results of verification tests conducted by the inventors of the present invention have shown that the reduction and suppression effects of the above-mentioned solutions are not necessarily sufficient. In addition, in order to reduce the moisture content of the polarizing plate when making the panel, the polarizing plate and the panel bonded with the polarizing plate need to be heated, which creates a new problem of reducing the productivity of the panel.

[0014] Prior art literature

[0015] Patent Literature

[0016] Patent Document 1: Japanese Patent Application Laid-Open No. 11-174417

[0017] Patent Document 2: Japanese Patent Application Publication No. 2014-102353 Summary of the invention

[0018] Problems to be solved by the invention

[0019] In view of the above situation, the problem to be solved by the present invention is to provide a polarizing plate, which, when used in an image display device composed of interlayer filling, has a small decrease in transmittance under high temperature environment and excellent durability, and to provide a method for manufacturing the polarizing plate. In addition, another object of the present invention is to provide a durable image display device with improved display characteristics under high temperature environment.

[0020] Means used to solve problems

[0021] The inventors of the present invention have conducted in-depth research and found that by containing at least one urea compound selected from urea, urea derivatives, thiourea and thiourea derivatives in a polarizing film formed by allowing a polyvinyl alcohol resin layer to adsorb iodine and orient the iodine, it is possible to suppress the reduction in transmittance under high temperature conditions in an interlayer filling structure in which one surface of a polarizing plate using the polarizing film is bonded to an image display unit and the other surface is bonded to a transparent component such as a touch panel or a front panel.

[0022] Furthermore, the inventors have found that, as a method for causing a polarizing film in which iodine is adsorbed and oriented on a polyvinyl alcohol-based resin layer and contains a urea-based compound, treating the polarizing film with a treatment liquid containing a urea-based compound is effective.

[0023] It was also found that in a device using an interlayer filling structure, among the urea compounds of the present invention, urea derivatives or thiourea derivatives not only showed excellent effects in suppressing the reduction in transmittance under high temperature environments, but also showed excellent performance in suppressing the reduction in polarization (orthogonal light leakage suppression) under high temperature environments.

[0024] The present inventors have completed the present invention based on such newly discovered facts.

[0025] The problems to be solved by the present invention can be solved by the following means.

[0026] (1) A polarizing plate comprising a polyvinyl alcohol-based resin polarizing film formed by absorbing and orienting iodine, and a protective film formed on at least one surface of the polarizing film,

[0027] The polarizing film contains at least one urea compound selected from urea, urea derivatives, thiourea, and thiourea derivatives.

[0028] (2) The polarizing plate according to (1), wherein the urea compound is a urea derivative and / or a thiourea derivative.

[0029] (3) The polarizing plate according to (1) or (2), characterized in that the polarizing plate is used in an image display device having an interlayer filling structure.

[0030] (4) A method for producing a polarizing plate, characterized in that it is a method for producing a polarizing plate having a protective film,

[0031] The method comprises the step of contacting a polyvinyl alcohol-based resin film with a solution containing at least one urea-based compound selected from urea, urea derivatives, thiourea and thiourea derivatives.

[0032] (5) The method for producing a polarizing plate according to (4), wherein the urea compound is a urea derivative and / or a thiourea derivative.

[0033] (6) The method for producing a polarizing plate according to (4) or (5), wherein the contact treatment step is performed after the dyeing treatment step.

[0034] (7) The method for producing a polarizing plate according to any one of (4) to (6), wherein the contact treatment step includes immersing the polyvinyl alcohol-based resin film in a solution containing the urea-based compound.

[0035] (8) The method for producing a polarizing plate according to any one of (4) to (6), wherein the contact treatment step includes a step of applying a solution containing the urea compound to the polyvinyl alcohol-based resin film.

[0036] (9) An image display device, characterized in that it comprises:

[0037] An image display panel having a polarizing plate according to any one of (1) to (3) bonded to a visible side surface of an image display unit via an adhesive layer; and

[0038] A transparent member bonded to the viewing side polarizing plate surface of the image display panel via an adhesive layer.

[0039] (10) The image display device according to (9), wherein the transparent member is a glass plate or a transparent resin plate.

[0040] (11) The image display device according to (9), wherein the transparent member is a touch panel.

[0041] Effects of the Invention

[0042] According to the present invention, a polarizing plate can be provided, which, when used in an image display device composed of an interlayer filling structure, has a small reduction in transmittance under high temperature conditions and excellent high temperature durability, and a method for manufacturing the polarizing plate is provided. In addition, by using the polarizing plate of the present invention, a display device can be provided in which the reduction in transmittance under high temperature conditions is suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 It is a cross-sectional view schematically showing the manufacturing apparatus of the polarizing film of the present invention. Figure 1 The arrow in the figure indicates the transport direction of the film. DETAILED DESCRIPTION

[0044] The polarizing film used in the polarizing plate of the present invention is a polarizing film obtained by adsorbing iodine on a polyvinyl alcohol-based resin film and orienting the iodine, and further contains at least one urea compound selected from urea, urea derivatives, thiourea and thiourea derivatives.

[0045] [Polarizing film manufacturing method]

[0046] In the present invention, the polarizing film is a polarizing film in which iodine is adsorbed and oriented on a uniaxially stretched polyvinyl alcohol resin film. The polyvinyl alcohol resin forming the polyvinyl alcohol resin film is usually obtained by saponifying a polyvinyl acetate resin. Its degree of saponification is usually about 85 mol% or more, preferably about 90 mol% or more, and more preferably about 99 mol% or more. The polyvinyl acetate resin can be, for example, polyvinyl acetate which is a homopolymer of vinyl acetate, and can also be a copolymer of vinyl acetate and other monomers copolymerizable therewith. As other monomers that can be copolymerized, for example, unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, etc. can be cited. The degree of polymerization of the polyvinyl alcohol resin is usually about 1000 to 10000, preferably about 1500 to 5000.

[0047] These polyvinyl alcohol-based resins may be modified. For example, polyvinyl formal, polyvinyl acetal, polyvinyl butyral, etc. modified with aldehydes may be used.

[0048] In the present invention, an unstretched polyvinyl alcohol resin film (raw material film) having a thickness of 65 μm or less (e.g., 60 μm or less), preferably 50 μm or less, more preferably 35 μm or less, and further preferably 30 μm or less is used as a raw material for the manufacture of a polarizing film. This can obtain a thin polarizing film that is increasingly required by the market. The width of the raw material film is not particularly limited, and for example, it can be about 400 to 6000 mm. For example, the raw material film is prepared in the form of a roll (raw material roll) of a long unstretched polyvinyl alcohol resin film.

[0049] In addition, the polyvinyl alcohol-based resin film used in the present invention may be a film laminated on a substrate film supporting it, that is, the polyvinyl alcohol-based resin film may be prepared in the form of a laminated film of a substrate film and a polyvinyl alcohol-based resin film laminated thereon. In this case, the polyvinyl alcohol-based resin film may be manufactured, for example, by applying a coating liquid containing a polyvinyl alcohol-based resin on at least one surface of the substrate film and drying it.

[0050] For example, a film containing a thermoplastic resin can be used as the substrate film. As a specific example, a film formed of a light-transmitting thermoplastic resin, preferably an optically transparent thermoplastic resin, can be a polyolefin resin such as a chain polyolefin resin (polypropylene resin, etc.) or a cyclic polyolefin resin (norbornene resin, etc.); a cellulose resin such as triacetyl cellulose and diacetyl cellulose; a polyester resin such as polyethylene terephthalate and polybutylene terephthalate; a polycarbonate resin; a (meth) acrylic resin such as methyl methacrylate resin; a polystyrene resin; a polyvinyl chloride resin; an acrylonitrile-butadiene-styrene resin; an acrylonitrile-styrene resin; a polyvinyl acetate resin; a polyvinylidene chloride resin; a polyamide resin; a polyacetal resin; a modified polyphenylene ether resin; a polysulfone resin; a polyethersulfone resin; a polyarylate resin; a polyamideimide resin; a polyimide resin, etc.

[0051] While unwinding the above-mentioned long strip of raw film from the raw material roll, it is continuously transported along the film transport path of the polarizing film manufacturing device, immersed in a treatment tank (hereinafter also referred to as a "treatment bath") containing a treatment liquid and then pulled out. After implementing the prescribed treatment process, a drying process is implemented, thereby continuously manufacturing the polarizing film in the form of a long strip of polarizing film. It should be noted that the treatment process is not limited to the method of immersing the film in the treatment bath as long as it is a method of treating the film by contacting the treatment liquid with the film, and it can also be a method of treating the film by making the treatment liquid adhere to the surface of the film by spraying, flowing, dripping, etc. In the case of performing the treatment process by immersing the film in a treatment bath, the treatment bath for one treatment process is not limited to one, and the film can also be immersed in two or more treatment baths in sequence to complete one treatment process.

[0052] As the above-mentioned treatment liquid, swelling liquid, dyeing liquid, cross-linking liquid, cleaning liquid, etc. can be exemplified. In addition, as the above-mentioned treatment process, a swelling process in which a swelling liquid is brought into contact with the original film to perform swelling treatment, a dyeing process in which a dyeing liquid is brought into contact with the film after swelling treatment to perform dyeing treatment, a cross-linking process in which a cross-linking liquid is brought into contact with the film after dyeing treatment to perform cross-linking treatment, a cleaning process in which a cleaning liquid is brought into contact with the film after cross-linking treatment to perform cleaning treatment, etc. can be exemplified. In addition, during these series of treatment processes, uniaxial stretching treatment is performed in a wet or dry manner. Other treatment processes can be added as needed.

[0053] The polarizing film used in the polarizing plate of the present invention contains a urea compound. The polarizing film may contain a urea compound by spraying, flowing, dripping, etc. as in the above-mentioned treatment steps, but preferably, the film is immersed in a treatment bath containing a urea compound and treated.

[0054] The treatment bath using the urea compound may be provided separately from the treatment bath used in the conventional production method, or the urea compound treatment function may be added by adding the urea compound to the conventional treatment bath. From the perspective of productivity, the method of adding the urea compound treatment function to the conventional treatment bath is more preferred.

[0055] The timing of adding a urea compound to the polarizing film is preferably to treat with a treatment solution containing a urea compound after dyeing with iodine. When the film contains a urea compound after dyeing, the color tone changes less and there is a tendency to further suppress the decrease in transmittance under high temperature environment in the interlayer filling structure.

[0056] Below, in reference Figure 1 At the same time, an example of the method for producing the polarizing film of the present invention will be described in detail. Figure 1 This is a cross-sectional view schematically showing an example of the method for producing a polarizing film of the present invention and a polarizing film producing apparatus used in the method. Figure 1 The polarizing film manufacturing apparatus shown is constructed as follows, that is, a raw material film 10 containing a polyvinyl alcohol-based resin is continuously unwound from a raw material roll 11 and transported along a film transport path, thereby sequentially passing through a swelling bath 13, a dyeing bath 15, a first cross-linking bath 17a, a second cross-linking bath 17b, and a cleaning bath 19 provided on the film transport path, and passing through a drying section 21. The obtained polarizing film 23 can be directly transported to a subsequent polarizing plate manufacturing process (a process of laminating a protective film on one or both sides of the polarizing film 23), for example. Figure 1 The arrow in the figure indicates the transport direction of the film.

[0057] In the above-mentioned manufacturing method, when a method of immersing the film in a treatment bath containing a urea compound is adopted as a method for making the polarizing film contain a urea compound, a method of making any one of the first cross-linking bath, the second cross-linking bath or the cleaning bath contain the urea compound is preferred, a method of making any one of the second cross-linking bath or the cleaning bath contain the urea compound is more preferred, and a method of making the second cross-linking bath contain the urea compound is further preferred.

[0058] Hereinafter, each step will be described.

[0059] (Swelling process)

[0060] Reference Figure 1 The original film 10 is continuously rolled out from the original roll 11 while being transported along the film transport path, and the original film 10 is immersed in the swelling bath 13 for a predetermined time and then pulled out, thereby implementing the swelling process. Figure 1In the example of , the original film 10 is transported along the film transport path constructed by the guide rollers 60, 61 and the clamping roller 50 from the time the original film 10 is unwound to the time the original film 10 is immersed in the swelling bath 13. During the swelling treatment, the original film 10 is transported along the film transport path constructed by the guide rollers 30 to 32 and the clamping roller 51.

[0061] As the swelling liquid of the swelling bath 13, in addition to pure water, an aqueous solution to which boric acid (Japanese Patent Publication No. 10-153709), chloride (Japanese Patent Publication No. 06-281816), inorganic acid, inorganic salt, water-soluble organic solvent, alcohol, etc. are added in a range of about 0.01 to 10 weight % can be used.

[0062] Figure 1 In the example shown, the film drawn out from the swelling bath 13 passes through the guide roller 32 , the nip roller 51 , and the guide roller 33 in sequence, and is then introduced into the dyeing bath 15 .

[0063] (Dyeing process)

[0064] The dyeing step is performed for the purpose of adsorbing the dichroic dye to the polyvinyl alcohol-based resin film after the swelling treatment and orienting the dichroic dye. The treatment conditions are determined within a range that can achieve this purpose without causing undesirable conditions such as extreme dissolution and devitrification of the film. Figure 1 The film is transported along the film transport path formed by the nip roller 51, the guide rollers 33 to 36 and the nip roller 52, and the film after the swelling treatment is immersed in the dye bath 15 for a predetermined time, and then pulled out, thereby performing the dyeing process. In order to improve the dyeability of the dichroic dye, the film provided to the dyeing process is preferably a film that has been subjected to at least a certain degree of uniaxial stretching treatment, or it is preferably subjected to uniaxial stretching treatment during the dyeing process instead of the uniaxial stretching treatment before the dyeing process, or it is preferably subjected to uniaxial stretching treatment during the dyeing process in addition to the uniaxial stretching treatment before the dyeing process.

[0065] Iodine is used as a dichroic pigment in the present invention. The dyeing solution of the dyeing bath 15 can be, for example, an aqueous solution having a concentration of iodine / potassium iodide / water = about 0.003 to 0.3 / about 0.1 to 10 / 100 in a weight ratio. Other iodides such as zinc iodide may be used instead of potassium iodide, or potassium iodide and other iodides may be used in combination. In addition, compounds other than iodides, such as boric acid, zinc chloride, cobalt chloride, etc., may coexist. When boric acid is added, it is different from the cross-linking treatment described later in that iodine is included. As long as the aqueous solution contains about 0.003 parts by weight or more of iodine relative to 100 parts by weight of water, it can be regarded as a dyeing bath 15.

[0066] Figure 1 In the example shown, the film drawn out from the dyeing bath 15 passes through the guide roller 36 , the nip roller 52 , and the guide roller 37 in sequence and is then introduced into the cross-linking bath 17 .

[0067] (Cross-linking process)

[0068] The cross-linking step is a treatment performed for the purpose of water resistance and color tone adjustment by cross-linking. Figure 1 In the example shown, two cross-linking baths are arranged as cross-linking baths for performing the cross-linking process. The first cross-linking process for the purpose of water resistance is performed in the first cross-linking bath 17a, and the second cross-linking process for the purpose of color tone adjustment is performed in the second cross-linking bath 17b. Figure 1 The first crosslinking step can be implemented by transporting the film along the film transport path constructed by the clamping roller 52, the guide rollers 37 to 40, and the clamping roller 53a, immersing the dyed film in the first crosslinking bath 17a for a predetermined time, and then pulling it out. The second crosslinking step can be implemented by transporting the film along the film transport path constructed by the clamping roller 53a, the guide rollers 41 to 44, and the clamping roller 53b, immersing the film after the first crosslinking step in the second crosslinking bath 17b for a predetermined time, and then pulling it out. Hereinafter, when a crosslinking bath is mentioned, both the first crosslinking bath 17a and the second crosslinking bath 17b are included, and when a crosslinking liquid is mentioned, both the first crosslinking liquid and the second crosslinking liquid are included.

[0069] As a cross-linking liquid, a solution in which a cross-linking agent is dissolved in a solvent can be used. As a cross-linking agent, for example, boric acid, borax and other boron compounds, glyoxal, glutaraldehyde and the like can be cited. They can be one, or two or more can be used in combination. As a solvent, for example, water can be used, and an organic solvent compatible with water can also be included. The concentration of the cross-linking agent in the cross-linking solution is preferably in the range of 1 to 20 weight %, but is not limited thereto.

[0070] The crosslinking treatment may be performed multiple times, usually 2 to 5 times. In this case, the composition and temperature of each crosslinking bath used may be the same or different as long as they are within the above range. The crosslinking treatment for water resistance by crosslinking and the crosslinking treatment for color tone adjustment may each be performed in multiple steps.

[0071] Figure 1 In the example shown, the film drawn out from the second cross-linking bath 17 b is introduced into the cleaning bath 19 after passing through the guide roller 44 and the nip roller 53 b in sequence.

[0072] (Cleaning process)

[0073] exist Figure 1In the example shown, a cleaning step after the cross-linking step is included. The cleaning process is performed for the purpose of removing excess chemicals such as boric acid and iodine attached to the polyvinyl alcohol resin film. The cleaning process is performed, for example, by immersing the cross-linked polyvinyl alcohol resin film in a cleaning bath 19. Water can be used as the cleaning liquid. The cleaning liquid can contain iodide such as potassium iodide and zinc iodide.

[0074] The cleaning step may be omitted depending on the situation.

[0075] (Stretching process)

[0076] The original film 10 is subjected to a uniaxial stretching treatment in a wet or dry manner during the above series of treatment steps. The specific method of the uniaxial stretching treatment may be, for example, inter-roll stretching in which a circumferential speed difference is set between two clamping rollers constituting the film conveying path to perform longitudinal uniaxial stretching, hot roller stretching as described in Japanese Patent No. 2731813, tenter stretching, etc., preferably inter-roll stretching. The uniaxial stretching step may be performed multiple times from the original film 10 to the polarizing film 23. As described above, the stretching treatment is also beneficial for suppressing the generation of wrinkles in the film.

[0077] The final cumulative stretch ratio of the polarizing film 23 based on the original film 10 is generally about 4.5 to 7 times, preferably 5 to 6.5 times. The stretching step can be performed in any treatment step, and when the stretching treatment is performed in two or more treatment steps, the stretching treatment can also be performed in any treatment step.

[0078] (Drying process)

[0079] The polyvinyl alcohol resin film may be dried after the cleaning step. There is no particular limitation on the film drying method. For example, a drying furnace equipped with a hot air dryer may be used. The drying temperature is, for example, about 30 to 100° C., and the drying time is, for example, about 30 to 600 seconds. The polyvinyl alcohol resin film may also be dried using a far-infrared heater. The thickness of the polarizing film 23 obtained as described above is, for example, about 5 to 30 μm.

[0080] [Urea compounds]

[0081] The polarizing film used for the polarizing plate of the present invention contains at least one urea compound selected from the group consisting of urea, urea derivatives, thiourea, and thiourea derivatives.

[0082] As a method for making a polarizing film contain a urea compound, a method of treating with the above-mentioned treatment bath containing a urea compound is preferred, however, a method of making any of the first cross-linking bath, the second cross-linking bath or the cleaning bath contain a urea compound is preferred, a method of making any of the second cross-linking bath or the cleaning bath contain a urea compound is more preferred, and a method of making it contain the second cross-linking bath is further preferred.

[0083] In addition, among urea compounds, there are water-soluble compounds and poorly soluble compounds, and water-soluble compounds are more preferred.

[0084] The concentration of the urea compound in the treatment bath is preferably 0.0001 to 0.1% by weight, more preferably 0.0005 to 0.05% by weight, and even more preferably 0.001 to 0.03% by weight.

[0085] (Urea or urea derivatives)

[0086] In the present invention, the urea derivative refers to a compound having a molecular structure in which a part of urea is substituted by a substituent. The urea derivative is preferably a compound in which at least one of the four hydrogen atoms in the urea molecule is substituted by a substituent.

[0087] In this case, the substituent is not particularly limited, but is preferably a substituent containing a carbon atom, a hydrogen atom, and an oxygen atom.

[0088] Specific examples of urea derivatives include, for monosubstituted urea, methyl urea, ethyl urea, propyl urea, butyl urea, isobutyl urea, N-octadecyl urea, 2-hydroxyethyl urea, hydroxy urea, acetyl urea, allyl urea, 2-propynyl urea, cyclohexyl urea, phenyl urea, 3-hydroxyphenyl urea, (4-methoxyphenyl) urea, benzyl urea, benzoyl urea, o-tolyl urea, and p-tolyl urea.

[0089] Examples of disubstituted ureas include 1,1-dimethylurea, 1,3-dimethylurea, 1,1-diethylurea, 1,3-diethylurea, 1,3-bis(hydroxymethyl)urea, 1,3-tert-butylurea, 1,3-dicyclohexylurea, 1,3-diphenylurea, 1,3-bis(4-methoxyphenyl)urea, 1-acetyl-3-methylurea, 2-imidazolidinone (ethylene urea), and tetrahydro-2-pyrimidinone (propylene urea).

[0090] Examples of the tetrasubstituted urea include tetramethylurea, 1,1,3,3-tetraethylurea, 1,1,3,3-tetrabutylurea, 1,3-dimethoxy-1,3-dimethylurea, 1,3-dimethyl-2-imidazolidinone, and 1,3-dimethyl-3,4,5,6-tetrahydro-2(1H)-pyrimidinone.

[0091] (Thiourea or thiourea derivatives)

[0092] In the present invention, the thiourea derivative refers to a compound having a molecular structure in which a part of thiourea is substituted by a substituent. The thiourea derivative is preferably a compound in which at least one of the four hydrogen atoms in the thiourea molecule is substituted by a substituent.

[0093] In this case, the substituent is not particularly limited, but is preferably a substituent containing a carbon atom, a hydrogen atom, and an oxygen atom.

[0094] Specific examples of thiourea derivatives include, for monosubstituted thiourea, N-methylthiourea, ethylthiourea, propylthiourea, isopropylthiourea, 1-butylthiourea, cyclohexylthiourea, N-acetylthiourea, N-allylthiourea, (2-methoxyethyl)thiourea, N-phenylthiourea, (4-methoxyphenyl)thiourea, N-(2-methoxyphenyl)thiourea, N-(1-naphthyl)thiourea, (2-pyridyl)thiourea, o-tolylthiourea, and p-tolylthiourea.

[0095] Examples of the disubstituted thiourea include 1,1-dimethylthiourea, 1,3-dimethylthiourea, 1,1-diethylthiourea, 1,3-diethylthiourea, 1,3-dibutylthiourea, 1,3-diisopropylthiourea, 1,3-dicyclohexylthiourea, N,N-diphenylthiourea, N,N'-diphenylthiourea, 1,3-di(o-tolyl)thiourea, 1,3-di(p-tolyl)thiourea, 1-benzyl-3-phenylthiourea, 1-methyl-3-phenylthiourea, N-allyl-N'-(2-hydroxyethyl)thiourea and ethylenethiourea.

[0096] Examples of trisubstituted thiourea include trimethylthiourea, and examples of tetrasubstituted thiourea include tetramethylthiourea and 1,1,3,3-tetraethylthiourea.

[0097] Among the above compounds, urea derivatives or thiourea derivatives are preferred, and urea derivatives are more preferred, from the viewpoint of less reduction in transmittance under high temperature environment and less reduction in polarization degree when used in an image display device composed of interlayer filling. Among urea derivatives, monosubstituted urea or disubstituted urea is preferred, and monosubstituted urea is more preferred. Disubstituted urea includes 1,1-substituted urea and 1,3-substituted urea, and 1,3-substituted urea is more preferred.

[0098] In addition, in this invention, urea, urea derivatives, thiourea, and thiourea derivatives are called urea compounds.

[0099] [Adhesive]

[0100] Any appropriate adhesive can be used as the adhesive for bonding the protective film to the polarizing film. Specifically, as the adhesive, a water-based adhesive, a solvent-based adhesive, an active energy ray-curable adhesive, etc. can be used, but a water-based adhesive is preferred.

[0101] It is also one of the preferred embodiments to contain a urea compound in the polarizing film and also in the adhesive. In this case, the urea compound contained in the polarizing film and the urea compound contained in the adhesive may be the same or different.

[0102] The thickness of the adhesive during coating can be set to any appropriate value. For example, it can be set in such a way that an adhesive layer having a desired thickness is obtained after curing or heating (drying). The thickness of the adhesive layer is preferably 0.01 μm to 7 μm, more preferably 0.01 μm to 5 μm, further preferably 0.01 μm to 2 μm, and most preferably 0.01 μm to 1 μm.

[0103] (Water-based adhesive)

[0104] In addition, as the above-mentioned water-based adhesive, any appropriate water-based adhesive can be used. Among them, it is preferred to use a water-based adhesive containing a PVA-based resin (PVA-based adhesive). The average degree of polymerization of the PVA-based resin contained in the water-based adhesive is preferably about 100 to 5500, and more preferably 1000 to 4500 from the aspect of adhesion. The average degree of saponification is preferably about 85 mol% to 100 mol%, and more preferably 90 mol% to 100 mol%, from the aspect of adhesion.

[0105] As the PVA resin contained in the above-mentioned water-based adhesive, a resin containing acetoacetyl groups is preferred, because the PVA resin layer has excellent adhesion to the protective film and excellent durability. The PVA resin containing acetoacetyl groups can be obtained, for example, by reacting the PVA resin with diketene using any method. The acetoacetyl modification degree of the PVA resin containing acetoacetyl groups is typically 0.1 mol% or more, preferably about 0.1 mol% to 20 mol%.

[0106] The resin concentration of the water-based adhesive is preferably 0.1% by weight to 15% by weight, and more preferably 0.5% by weight to 10% by weight.

[0107] (crosslinking agent, solvent)

[0108] The water-soluble PVA-based adhesive that can be preferably used in the present invention can also contain a crosslinking agent in addition to the above-mentioned PVA-based resin as needed. As the crosslinking agent, a known crosslinking agent can be used. For example, water-soluble epoxy compounds, dialdehydes, isocyanates, etc. can be mentioned.

[0109] When the PVA-based resin is an acetoacetyl group-containing PVA-based resin, the crosslinking agent is preferably any of glyoxal, glyoxylate, and methylolmelamine, more preferably glyoxal or glyoxylate, and particularly preferably glyoxal.

[0110] The water-soluble PVA-based adhesive of the present invention may contain an organic solvent. In this case, alcohols are preferred from the viewpoint of miscibility with water, and methanol or ethanol is more preferred among alcohols.

[0111] (Active energy ray-curable adhesive)

[0112] As the above-mentioned active energy ray-curable adhesive, any appropriate adhesive can be used as long as it is an adhesive that can be cured by irradiation with active energy rays. As active energy ray-curable adhesives, for example, ultraviolet curable adhesives, electron beam curable adhesives, etc. can be cited. As specific examples of the curing type of active energy ray-curable adhesives, free radical curing types, cation curing types, anion curing types, and combinations thereof (for example, a mixture of free radical curing types and cation curing types) can be cited.

[0113] Examples of the active energy ray-curable adhesive include an adhesive containing, as a curing component, a compound (eg, a monomer and / or an oligomer) having a radical polymerizable group such as a (meth)acrylate group or a (meth)acrylamide group.

[0114] Specific examples of the active energy ray-curable adhesive and the curing method thereof are described in, for example, Japanese Patent Application Laid-Open No. 2012-144690.

[0115] [Transparent protective film]

[0116] The transparent protective film used in the present invention (hereinafter also referred to as "protective film") is preferably bonded to at least one side of the polarizing film via an adhesive layer. The transparent protective film is bonded to one or both sides of the polarizing film, but more preferably bonded to both sides. In the present invention, a member having a protective film on at least one side of the polarizing film is also referred to as a polarizing plate.

[0117] The protective film may have other optical functions at the same time, and may have a laminated structure in which other layers are laminated.

[0118] From the viewpoint of optical properties, the protective film is preferably thin, but if it is too thin, the strength decreases and the processability deteriorates. The appropriate film thickness is 5 to 100 μm, preferably 10 to 80 μm, and more preferably 15 to 70 μm.

[0119] As the protective film, films such as cellulose acylate resin films, films made of polycarbonate resins, films made of cycloolefin resins such as norbornene, (meth)acrylic polymer films, and polyester resin films such as polyethylene terephthalate can be used.

[0120] In the case where the polarizing film has a protective film on both sides, when bonding them using a water-based adhesive such as a PVA-based adhesive, from the perspective of moisture permeability, it is preferred that the protective film on at least one side is either a cellulose acylate film or a (meth) acrylic polymer film, among which a cellulose acylate film is preferred.

[0121] At least one of the protective films may have a phase difference function for the purpose of viewing angle compensation or the like. In this case, the film itself may have the phase difference function, may have a phase difference layer separately, or may be a combination of both.

[0122] In addition, although the structure which laminated|laminated the film which has a phase difference function directly to a polarizing film via an adhesive is demonstrated, it may be laminated|laminated via a pressure-sensitive adhesive or an adhesive via another protective film laminated|laminated to a polarizing film.

[0123] [Configuration of Image Display Device]

[0124] The polarizing plate of the present invention, i.e., a polarizing plate in which a transparent protective film is bonded to at least one side of a polarizing film containing a urea compound via an adhesive layer, is used in various image display devices such as liquid crystal display devices and organic EL display devices. In particular, the polarizing plate of the present invention can be suitably used in an image display device having an interlayer filling structure in which a transparent member such as a front panel and a touch panel is arranged on the visible side of the image display device, and the image display panel and the transparent member are bonded using an adhesive layer or the like.

[0125] (Image display unit)

[0126] As the image display unit, a liquid crystal unit and an organic EL unit can be cited. As the liquid crystal unit, any of a reflective liquid crystal unit utilizing external light, a transmissive liquid crystal unit utilizing light from a light source such as a backlight, and a semi-transmissive and semi-reflective liquid crystal unit utilizing both light from the outside and light from the light source can be used. In the case where the liquid crystal unit is a liquid crystal unit utilizing light from a light source, in the image display device (liquid crystal display device), a polarizing plate is also configured on the side opposite to the visible side of the image display unit (liquid crystal unit), and a light source is also configured. The polarizing plate on the light source side is preferably bonded to the liquid crystal unit via a suitable adhesive layer. As the driving mode of the liquid crystal unit, for example, any type of mode such as VA mode, IPS mode, TN mode, STN mode, bending orientation (π type) can be used.

[0127] As the organic EL unit, an organic EL unit in which a transparent electrode, an organic light-emitting layer and a metal electrode are sequentially stacked on a transparent substrate to form a light-emitting body (organic electroluminescent light-emitting body) can be suitably used. The organic light-emitting layer is a laminate of various organic thin films, for example, a laminate of a hole injection layer containing a triphenylamine derivative or the like and a light-emitting layer containing a fluorescent organic solid such as anthracene, a laminate of these light-emitting layers and an electron injection layer containing a perylene derivative or the like, or a laminate of a hole injection layer, a light-emitting layer, and an electron injection layer can be used.

[0128] (Attachment of image display unit and polarizing plate)

[0129] In laminating the image display unit and the polarizing plate, an adhesive layer (adhesive sheet) can be appropriately used. Among them, from the viewpoint of operability, etc., it is preferred to laminate the polarizing plate with an adhesive layer having an adhesive layer attached to one surface of the polarizing plate and the image display unit. The adhesive layer can be attached to the polarizing plate in an appropriate manner. As an example, for example, a method of preparing an adhesive solution in which about 10 to 40 weight % of a base polymer or a combination thereof is dissolved or dispersed in a solvent containing a single substance or a mixture of appropriate solvents such as toluene and ethyl acetate, and directly attaching it to the polarizing plate by an appropriate development method such as a casting method and a coating method; or a method of forming an adhesive layer on a spacer as described above and then transferring it to the polarizing plate, etc.

[0130] (Adhesive layer)

[0131] The adhesive layer is described in paragraphs

[0103] to

[0143] of JP-A-2018-025765, and these adhesives can be used in the present invention.

[0132] (Transparent front part)

[0133] As the front transparent member disposed on the visible side of the image display unit, a front panel (window layer), a touch panel, etc. can be cited. As the front panel, a transparent plate with appropriate mechanical strength and thickness can be used. As such a transparent plate, for example, a transparent resin plate such as an acrylic resin or a polycarbonate resin, or a glass plate, etc. can be used. Functional layers such as an anti-reflection layer can also be stacked on the visible side of the transparent plate. In addition, when the transparent plate is a transparent resin plate, a hard coating layer can be stacked to improve physical strength, and a low moisture permeability layer can be stacked to reduce moisture permeability.

[0134] As the touch panel, various touch panels such as resistive film type, electrostatic capacitance type, optical type, ultrasonic type, etc., glass plates with touch sensor functions, transparent resin plates, etc. can be used. In the case of using an electrostatic capacitance type touch panel as the front transparent member, it is preferred to set a front panel formed of glass or a transparent resin plate on the visible side relative to the touch panel.

[0135] (Attachment of polarizing plate to front transparent member)

[0136] In laminating the polarizing plate to the front transparent member, an adhesive or a UV curable adhesive can be used appropriately. When an adhesive is used, the adhesive can be attached in an appropriate manner. As a specific attachment method, for example, the attachment method of the adhesive layer used in laminating the aforementioned image display unit to the polarizing plate can be cited.

[0137] When a UV curing adhesive is used, in order to prevent the adhesive solution before curing from spreading, the following method can be appropriately used, that is, a dam material is provided in a manner surrounding the peripheral portion on the image display panel, a front transparent member is placed on the dam material, and the adhesive solution is injected. After the adhesive solution is injected, alignment and degassing are performed as needed, and then UV light is irradiated for curing.

[0138] As described above in the description of the manufacturing method and components of the polarizing film, as a method for making the polarizing film contain a urea compound, a method of immersing the film in a treatment bath containing a urea compound and treating it can be preferably used, but as described above, a coating treatment using a spraying, flowing, dripping, etc. method can also be used. Among these methods, after applying a solution containing at least one selected from urea, urea derivatives, thiourea, and thiourea derivatives to at least one surface of a polarizing film formed of a stretched polyvinyl alcohol-based resin film in which iodine is adsorbed and oriented by any of the above methods, the polarizing film can also be manufactured by drying the coating solution.

[0139] As a preferred embodiment of such a method, there can be mentioned a method of preparing a polarizing film not containing a urea compound, and applying a urea compound by any of the above-mentioned methods after a drying step.

[0140] (Coating solution containing urea compound)

[0141] The solvent of the coating solution containing the urea compound of the present invention is preferably water, an organic solvent or a mixture thereof, more preferably water or a mixed solvent of water and alcohol. In the case of a mixed solvent of water and alcohol, the alcohol is preferably methanol or ethanol.

[0142] As the urea compound, the above-mentioned urea compounds can be preferably used. However, the urea compound is preferably water-soluble from the viewpoint that the urea compound is less likely to precipitate on the surface of the polarizing film after drying.

[0143] Furthermore, the coating liquid may contain a surfactant or the like as necessary.

[0144] Example

[0145] Hereinafter, the present invention will be specifically described based on the examples. The materials, reagents, amounts and ratios thereof, operations, etc. shown in the following examples may be appropriately changed without departing from the gist of the present invention. Therefore, the present invention is not limited or restricted by the following examples.

[0146] (Comparative Example 1: Preparation of a Polarizing Film Not Treated with a Urea Compound)

[0147] use Figure 1 The manufacturing apparatus shown in the figure manufactures the polarizing film of Comparative Example 1 from the polyvinyl alcohol-based resin film. Specifically, a long strip of polyvinyl alcohol (PVA) raw material film [trade name "Kuraray Vinylon VF-PE#6000" manufactured by Kuraray Co., Ltd., average polymerization degree 2400, saponification degree 99.9 mol % or more] with a thickness of 60 μm is continuously conveyed while being rolled out from a roll, and immersed in a swelling bath formed of pure water at 30° C. for a residence time of 89 seconds (swelling process). Thereafter, the film pulled out from the swelling bath is immersed in a dyeing bath containing iodine at 30° C. with a retention time of 156 seconds, wherein potassium iodide / boric acid / water is 2 / 0.3 / 100 (weight ratio) (dyeing process). Then, the film pulled out from the dyeing bath was immersed in a first crosslinking bath of 56°C with a potassium iodide / boric acid / water ratio of 12 / 4 / 100 (weight ratio) for 67 seconds, and then immersed in a second crosslinking bath of 40°C with a potassium iodide / boric acid / water ratio of 9 / 3 / 100 (weight ratio) for 11 seconds (crosslinking step). In the dyeing step and the crosslinking step, longitudinal uniaxial stretching was performed by roller stretching in the bath. The total stretching ratio based on the original film was set to 5.69 times.

[0148] Then, the film pulled out from the second crosslinking bath 17b and passed through the nip roller 53b was immersed in a cleaning bath 19 made of pure water at 5°C for a residence time of 3 seconds (cleaning step). Thereafter, the temperature in the high humidity treatment section 21 was set to 75°C and the absolute humidity to 147 g / cm 3 The film was exposed to a high humidity environment for 60 seconds at a relative humidity of 61%. At this time, a uniaxial stretching treatment of 1.14 times was simultaneously performed. Finally, the film was subjected to a drying process to obtain a polarizing film 12. The drying process was carried out in a drying furnace at a temperature of 30°C and an absolute humidity of 10 g / cm 3The film was dried under the conditions of 100 ℃ and 120 sec residence time. The thickness of the obtained polarizing film was 23 μm.

[0149] (Examples 1 to 11: Preparation of polarizing film)

[0150] Polarizing films 1 to 11 were obtained in the same manner except that a urea compound having a value shown in Table 1 was added to the second crosslinking bath. The obtained polarizing films each contained the urea compound shown in Table 1. The thickness of the obtained polarizing film was 23 μm.

[0151] Urea, methylurea, ethylurea, 1,3-dimethylurea, tetramethylurea, phenylurea, thiourea, and methylthiourea used above were all reagents produced by Tokyo Chemical Industry Co., Ltd.

[0152] (Preparation of PVA-based Adhesive 1)

[0153] 50 g of a modified PVA-based resin containing an acetoacetyl group (Gohsenx Z-410 manufactured by Mitsubishi Chemical Corporation) was dissolved in 950 g of pure water, and the mixture was heated at 90° C. for 2 hours and then cooled to room temperature to obtain a PVA solution A.

[0154] Then, the PVA solution A, maleic acid, glyoxal, and pure water were mixed so that the respective compounds had the following concentrations, thereby preparing a PVA-based adhesive 1.

[0155] PVA concentration: 3.0 wt%

[0156] Maleic acid 0.5 wt%

[0157] Glyoxal 0.15 wt%

[0158] (Saponification of Cellulose Acylate Film)

[0159] A commercially available cellulose acylate film TD40 (manufactured by Fujifilm Corporation: film thickness 40 μm) was immersed in a 1.5 mol / L NaOH aqueous solution (saponification solution) maintained at 55°C for 2 minutes, then washed with water, and then immersed in a 0.05 mol / L sulfuric acid aqueous solution at 25°C for 30 seconds, and then passed through a water bath under running water for 30 seconds to neutralize the film. Thereafter, water removal using an air knife was repeated three times, and after the water was removed, the film was retained in a drying zone at 70°C for 15 seconds and dried, thereby producing a saponified film.

[0160] (Production of Polarizing Plate 1)

[0161] On both sides of the polarizing film 1, a PVA-based adhesive 1 is applied to adjust the thickness of the adhesive layer after drying to 100 nm on both sides. The saponified cellulose acylate film prepared above is laminated using a roll laminator and then dried at 60°C for 10 minutes to obtain a polarizing plate 1 with cellulose acylate films on both sides.

[0162] (Production of Polarizing Plates 2 to 12)

[0163] Polarizing plates 2 to 12 were produced in the same manner as the polarizing plate 1 except that the polarizing film 1 was replaced with polarizing films 2 to 12 .

[0164] (Production of Laminated Body 1)

[0165] With reference to the example of Japanese Patent Publication No. 2018-025765, an acrylic adhesive (manufacturer: LINTEC, product model: #7) was applied to both sides of the polarizing plate 1 prepared above, thereby preparing an optical laminate 1 having an adhesive layer with a thickness of 25 μm on both sides.

[0166] (Production of Laminated Bodies 2 to 12)

[0167] Optical layered bodies 2 to 12 were produced in the same manner as in the optical layered body 1 except that the polarizing plate 1 was replaced with the polarizing plates 2 to 12 .

[0168] (Production of Laminated Body 13)

[0169] An optical laminate 13 was produced in the same manner as the optical laminate 12 except that the pressure-sensitive adhesive layer was laminated only on one surface of the optical laminate 12 .

[0170] (Evaluation of Laminated Body)

[0171] The laminate produced above was evaluated with reference to the examples of Japanese Patent Publication No. 2014-102353 and Japanese Patent Publication No. 2018-025765. It should be noted that the high temperature durability test was performed at 95°C and 105°C, and the high temperature durability test was performed at 95°C for 1000 hours. Except for Comparative Example 1 using the polarizing film 12 not containing the urea compound, no decrease in transmittance was observed. Table 1 only shows the results of the high temperature durability test at 105°C.

[0172] In the test results of Comparative Example 1, the coloration at 105° C.×100 hours is substantially the same as the result at 95° C.×1000 hours.

[0173] [Evaluation of single body transmittance after high temperature durability test (105°C)]

[0174] The optical laminates 1 to 12 prepared above were cut into a size of 50 mm × 100 mm, and the surfaces of the first adhesive layer and the second adhesive layer were bonded to alkali-free glass (trade name "EAGLE XG", manufactured by CORNING), thereby preparing evaluation samples. In addition, the optical laminate 13 was cut into a size of 50 mm × 100 mm, and the surface of the first adhesive layer was bonded to alkali-free glass (trade name "EAGLE XG", manufactured by CORNING), thereby preparing evaluation samples. It should be noted that when preparing these samples, no heating treatment for adjusting the moisture content was performed before bonding the glass plate.

[0175] The evaluation sample was subjected to a temperature of 50°C and a pressure of 5 kgf / cm 2 (490.3kPa) After 1 hour of autoclave treatment, place in an environment of temperature 23°C and relative humidity 55% for 24 hours. Afterwards, measure the transmittance (initial value), store in a heated environment of temperature 105°C, and measure the transmittance every 50 hours until 100 to 200 hours. Based on the time when the transmittance decreases by more than 5% relative to the initial value, the following criteria are used for evaluation. The results are shown in Table 1.

[0176] In addition, since the evaluation sample including the optical layered body 13 has a structure in which the alkali-free glass is laminated only on one surface, the transmittance does not decrease, and the evaluation result is A.

[0177] Samples with a transmittance drop of 5% or less after 200 hours: A

[0178] Samples whose transmittance drops by more than 5% after 150 to 200 hours: B

[0179] Samples whose transmittance drops by 5% or more after 100 to 150 hours: C

[0180] Samples with a transmittance drop of 5% or more after 100 hours: D

[0181] [Evaluation of cross light leakage after high temperature durability test]

[0182] The optical laminate 13 was cut into a size of 30 mm×30 mm, and the surface of the first pressure-sensitive adhesive layer was bonded to an alkali-free glass (trade name “EAGLE XG”, manufactured by CORNING CORPORATION) to prepare a sample 20 for orthogonal evaluation.

[0183] After the single transmittance evaluation sample after high temperature durability was evaluated after 100 hours, light leakage in a crossed Nicol prism state (hereinafter also referred to as “crossed light leakage”) was visually evaluated in the optical layered body and sample 20 according to the following criteria.

[0184] Samples where no orthogonal light leakage is observed: ◎

[0185] Samples where almost no orthogonal light leakage is observed: ○

[0186] Samples with slight orthogonal light leakage: △

[0187] Samples where orthogonal light leakage is clearly observed: ×

[0188] [Table 1]

[0189]

[0190] The addition amount of the urea-based compound in Table 1 is described.

[0191] The concentration of the urea compound added to the second cross-linking bath is preferably 0.0001 to 0.1% by weight, more preferably 0.0005 to 0.05% by weight, and even more preferably 0.001 to 0.03% by weight.

[0192] In the present invention, any urea compound shows a tendency that the higher the concentration, the smaller the change in single transmittance after the high-temperature durability test. Conversely, the lower the concentration, the smaller the orthogonal light leakage after the high-temperature durability test.

[0193] All the urea compounds described in the examples showed an effect that the change in single transmittance after the high-temperature durability test was B or more and the cross light leakage was △ or more, and had excellent effects in both performance aspects.

[0194] However, for the amount of the above-mentioned compounds, the concentration range that exhibits the preferred performance, that is, the single body transmittance change is greater than B and the orthogonal light leakage is greater than △, is strictly different for each compound. However, the concentration of any compound has an appropriate range within the preferred concentration range.

[0195] The concentrations listed in Table 1 show the values ​​of the minimum concentrations at which the single-unit transmittance reaches the evaluation A in each urea-based compound. In addition, for urea and thiourea, the concentrations are gradually reduced from the minimum concentrations at which the evaluation A is reached, and the values ​​of the concentrations at which the cross light leakage changes from △ to ○ (the single-unit transmittance changes to B at this time). In addition, for methyl urea, the concentrations are gradually reduced from the minimum concentrations at which the evaluation A is reached, and the values ​​of the concentrations at which the cross light leakage changes from ○ to ◎ (the single-unit transmittance changes to B at this time).

[0196] From the results shown in Table 1, the following conclusions can be drawn.

[0197] 1. The polarizing plate of the present invention using a polarizing film containing a urea compound can suppress a decrease in single-body transmittance even when exposed to a high-temperature environment for a long period of time when used in an image display device having an interlayer filler structure.

[0198] 2. Compared with polarizing plates using urea or thiourea, polarizing plates using urea derivatives or thiourea derivatives are particularly excellent in that they do not have a decrease in single-unit transmittance and do not have cross light leakage.

[0199] 3. A polarizing plate using a polarizing film containing two urea compounds can suppress a decrease in single-body transmittance even when exposed to a high-temperature environment for a long period of time, which is also one of the preferred aspects of the present invention.

[0200] Examples of embodiments in which a urea compound is contained in a polarizing film and an adhesive are given below. However, this embodiment is not limited to or restricted by the following examples.

[0201] (Preparation of PVA solution for adhesive)

[0202] 50 g of a modified PVA-based resin containing an acetoacetyl group (Gohsenx Z-410 manufactured by Mitsubishi Chemical Corporation) was dissolved in 950 g of pure water, and the mixture was heated at 90° C. for 2 hours and then cooled to room temperature to obtain a PVA solution for an adhesive.

[0203] (Preparation of methyl urea solution)

[0204] 10 g of methyl urea was added to 90 g of pure water to obtain a 10 wt % aqueous solution of methyl urea.

[0205] (Preparation of PVA-based Adhesive 2)

[0206] The PVA solution for adhesive prepared above, pure water and methanol were mixed so that the PVA concentration was 3.0%, the methanol concentration was 20% and the methyl urea concentration was 0.0% (without adding the methyl urea solution) to obtain Adhesive 2 for polarizing plates.

[0207] (Preparation of PVA-based Adhesive 3)

[0208] The PVA solution for adhesive prepared above, methyl urea solution, pure water and methanol were mixed so that the PVA concentration was 3.0%, the methanol concentration was 20% and the methyl urea concentration was 0.2%, thereby obtaining Adhesive 3 for polarizing plates.

[0209] (Manufacturing of Polarizing Plates 21 and 22)

[0210] Polarizing plates 21 and 22 were obtained in the same manner as for polarizing plate 3 except that PVA-based adhesive 1 was replaced with PVA-based adhesive 2 and PVA-based adhesive 3, respectively.

[0211] (Production of Polarizing Plate 23)

[0212] A polarizing plate 23 was obtained in the same manner as the polarizing plate 12 except that the PVA-based adhesive 1 was replaced with the PVA-based adhesive 2 .

[0213] Optical layered bodies 21 to 23 were obtained in the same manner as in the optical layered body 1 except that the polarizing plate 1 was replaced with the polarizing plates 21 to 23, respectively. These samples were evaluated in the same manner as in the optical layered body 1, and the obtained results are shown in Table 2.

[0214] [Table 2]

[0215]

[0216] From the results shown in Table 2, the following conclusions can be drawn.

[0217] 1. The polarizing plate of the present invention containing a urea compound in the polarizing film and the adhesive can suppress a decrease in single-body transmittance even when exposed to a high-temperature environment for a long time when used in an image display device having an interlayer filler structure.

[0218] Another example is given. This example is a method in which a polarizing film not containing a urea compound is first prepared, and after a drying step, a coating liquid containing a urea compound is applied. This example is also not limited to or restricted by the following example.

[0219] A 0.5% solution of methyl urea was prepared as a coating solution. The 0.5% solution of methyl urea was applied to one side of the polarizing film 12 prepared above using a bar coater so that the wet coating amount was 10 μm, and dried at 60° C. for 5 minutes to obtain a polarizing film 31. The obtained polarizing film 31 contained methyl urea.

[0220] As a comparative example, pure water was applied to one side of the polarizing element produced above using a bar coater so that the wet coating amount was 10 μm, and the mixture was dried at 60° C. for 5 minutes to obtain a polarizing film 32 .

[0221] Regarding the polarizing plate 1 , the polarizing plates 31 and 32 were obtained in the same manner except that the polarizing film 1 was replaced with the polarizing film 31 and the polarizing film 32 , respectively.

[0222] Optical layered bodies 31 and 32 were obtained in the same manner as in the optical layered body 1 except that polarizing plate 1 was replaced with polarizing plate 31 and polarizing plate 32, respectively. These samples were evaluated in the same manner as in the optical layered body 1. Table 3 shows the obtained results.

[0223] [Table 3]

[0224]

[0225] From the results shown in Table 3, the following conclusions can be drawn.

[0226] 1. The polarizing plate of the present invention, which has a polarizing film produced by coating a solution containing a urea compound on at least one surface of the polarizing film and drying the solution, can suppress the decrease in single-body transmittance even when exposed to a high-temperature environment for a long time when used in an image display device composed of interlayer filling.

[0227] Description of Reference Numerals

[0228] 10 comprises a raw material film of a polyvinyl alcohol-based resin, 11 a raw material roll, 13 a swelling bath, 15 a dyeing bath, 17a a first cross-linking bath, 17b a second cross-linking bath, 19 a cleaning bath, 21 a drying section, 23 a polarizing film, 30 to 48, 60, 61 guide rollers, 50 to 52, 53a, 53b, 54, 55 clamping rollers.

Claims

1. A polarizing plate, characterized in that: A polarizing plate comprising a polyvinyl alcohol-based resin polarizing film formed by absorbing and orienting iodine, and a protective film formed on at least one surface of the polarizing film. The polarizing film contains at least one urea compound selected from urea derivatives and thiourea derivatives. The urea derivative is selected from the group consisting of methyl urea, ethyl urea, propyl urea, butyl urea, isobutyl urea, N-octadecyl urea, 2-hydroxyethyl urea, hydroxyurea, acetyl urea, allyl urea, 2-propynyl urea, cyclohexyl urea, phenyl urea, 3-hydroxyphenyl urea, (4-methoxyphenyl) urea, benzyl urea, benzoyl urea, o-tolyl urea, p-tolyl urea, 1,1-dimethyl urea, 1,3-dimethyl urea, 1,1-diethyl urea, 1,3-diethyl urea, 1,3-bis(hydroxymethyl) urea, 1,3-tert-butyl urea. butyl urea, 1,3-dicyclohexyl urea, 1,3-diphenyl urea, 1,3-di(4-methoxyphenyl)urea, 1-acetyl-3-methyl urea, 2-imidazolidinone (ethylene urea), tetrahydro-2-pyrimidinone (propylene urea), tetramethyl urea, 1,1,3,3-tetraethyl urea, 1,1,3,3-tetrabutyl urea, 1,3-dimethoxy-1,3-dimethyl urea, 1,3-dimethyl-2-imidazolidinone, 1,3-dimethyl-3,4,5,6-tetrahydro-2(1H)-pyrimidinone, The thiourea derivative is selected from N-methylthiourea, ethylthiourea, propylthiourea, isopropylthiourea, 1-butylthiourea, cyclohexylthiourea, N-acetylthiourea, N-allylthiourea, (2-methoxyethyl)thiourea, N-phenylthiourea, (4-methoxyphenyl)thiourea, N-(2-methoxyphenyl)thiourea, N-(1-naphthyl)thiourea, (2-pyridyl)thiourea, o-tolylthiourea, p-tolylthiourea, 1,1-dimethylthiourea, 1,3-dimethylthiourea, 1,1-diethylthiourea, Thiourea, 1,3-diethylthiourea, 1,3-dibutylthiourea, 1,3-diisopropylthiourea, 1,3-dicyclohexylthiourea, N,N-diphenylthiourea, N,N'-diphenylthiourea, 1,3-di(o-tolyl)thiourea, 1,3-di(p-tolyl)thiourea, 1-benzyl-3-phenylthiourea, 1-methyl-3-phenylthiourea, N-allyl-N'-(2-hydroxyethyl)thiourea, ethylenethiourea, trimethylthiourea, tetramethylthiourea, 1,1,3,3-tetraethylthiourea.

2. The polarizing plate according to claim 1, wherein The polarizing plate is used in an image display device having an interlayer filling structure.

3. A method for manufacturing a polarizing plate, characterized in that: A method for manufacturing a polarizing plate having a protective film, The method provides a polyvinyl alcohol-based resin to a swelling step, a dyeing step, a cross-linking step, and a washing step in sequence to produce a polarizing film. The method comprises the steps of contacting a polyvinyl alcohol resin film with a solution containing at least one urea compound selected from urea, urea derivatives, thiourea and thiourea derivatives. The contact treatment step is performed together with the cross-linking step or the washing step.

4. The method for manufacturing a polarizing plate according to claim 3, wherein: The urea compound is a urea derivative and / or a thiourea derivative.

5. The method for manufacturing a polarizing plate according to claim 3, wherein: The contact treatment step is performed after the dyeing treatment step.

6. The method for producing a polarizing plate according to any one of claims 3 to 5, wherein: The contact treatment step includes a step of immersing the polyvinyl alcohol-based resin film in a solution containing the urea-based compound.

7. The method for producing a polarizing plate according to any one of claims 3 to 5, wherein: The contact treatment step includes a step of applying a solution containing the urea compound to the polyvinyl alcohol-based resin film.

8. An image display device, characterized in that: have: An image display panel having the polarizing plate according to claim 1 or 2 bonded to a visible side surface of an image display unit via an adhesive layer, and A transparent member bonded to the viewing side polarizing plate surface of the image display panel via an adhesive layer.

9. The image display device according to claim 8, characterized in that: The transparent member is a glass plate or a transparent resin plate.

10. The image display device according to claim 8, characterized in that The transparent component is a touch panel.