LCP extruded film, flexible laminate using the same, and method for producing the same

By using the LCP extruded film of aromatic polyester-based liquid crystal polymer and adjusting its crystallization state and dissolution rate, thermal compression bonding at a lower temperature is achieved, which solves the problem of insufficient temperature control in the existing technology and improves the efficiency The productivity and peel strength of flexible laminates maintain the excellent properties of liquid crystal polymers.

CN113993702BActive Publication Date: 2024-10-29DENKA CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202080040729.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-06-19
Publication Date
2024-10-29
Estimated Expiration
2040-06-19

AI Technical Summary

Technical Problem

In the existing technology, when manufacturing flexible laminates, imprecise temperature control leads to insufficient productivity and dimensional accuracy, and high-temperature thermocompression bonding can damage the mechanical and electrical properties of liquid crystal polymers and increase production costs.

Method used

LCP extruded film containing aromatic polyester liquid crystal polymer is used. By adjusting its crystallization state and dissolution rate, thermal compression bonding at a lower temperature can be achieved to improve process margin and peel strength.

Benefits of technology

While maintaining the excellent properties of the liquid crystal polymer, the productivity and economy of the flexible laminate are improved, the manufacturing process is simplified, and high peel strength and good reproducibility are obtained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113993702B_ABST
    Figure CN113993702B_ABST
Patent Text Reader

Abstract

The present invention provides an LCP extruded film, etc., which can improve the process margin when manufacturing a flexible laminate without excessively damaging the excellent basic properties of the liquid crystal polymer. The present invention provides an LCP extruded film, etc., which can easily obtain a flexible laminate with high peel strength with a metal foil even under milder manufacturing conditions than the prior art. The LCP extruded film 11 contains an aromatic polyester-based liquid crystal polymer, and the aromatic polyester-based liquid crystal polymer has at least one selected from the group consisting of p-hydroxybenzoic acid, terephthalic acid, isophthalic acid, 6-naphthalene dicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybiphenol, ethylene terephthalate and their derivatives and 6-hydroxy-2-naphthoic acid and its derivatives as monomer components, and the solubility of the LCP extruded film 11 in pentafluorophenol at 60°C is 25% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an LCP extruded film, a flexible laminate using the same, a method for producing the same, and the like. Background Art

[0002] Liquid crystal polymer (LCP) is a polymer that exhibits liquid crystal properties in a molten state or a solution state. In particular, thermotropic liquid crystal polymers that exhibit liquid crystal properties in a molten state have excellent properties such as high strength, high heat resistance, high insulation, low water absorption, and high gas barrier properties. Therefore, their practical application in electronic material applications and electrical insulating material applications is progressing rapidly.

[0003] In addition, liquid crystal polymers have excellent high-frequency characteristics and low dielectric properties, and therefore are also attracting attention as insulating materials for flexible printed circuit boards (FPCs) and other materials in the fifth-generation mobile communication systems (5G) and millimeter-wave radars that will be developed in the future.

[0004] As a method for manufacturing a flexible laminate using a liquid crystal polymer, for example, Patent Document 1 discloses a method for manufacturing a flexible laminate, which is characterized in that it includes a heat pressing step of continuously supplying an insulating film and a metal foil formed by a liquid crystal polymer between a pair of annular belts, and heat pressing the insulating film and the metal foil between the annular belts to form a flexible laminate, in which the maximum temperature of the flexible laminate is within a range of not less than 45°C lower than the melting point of the liquid crystal polymer constituting the insulating film and not more than 5°C lower than the melting point, and the flexible laminate is slowly cooled in a range of not less than 235°C lower than the melting point of the liquid crystal polymer constituting the insulating film and not more than 100°C lower than the melting point when the flexible laminate is unloaded from the annular belt.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2016-129949 Summary of the invention

[0008] Problems to be solved by the invention

[0009] However, it is known that in the manufacturing method described in Patent Document 1, if precise temperature control is not performed in the thermal compression bonding process, problems such as failure to operate continuously or failure to obtain a flexible laminate with high dimensional accuracy will occur at a high frequency (see

[0047] of Patent Document 1).

[0010] In addition, in Patent Document 1, an LCP film obtained by inflation film forming is used as an insulating film, and it is also shown that the peel strength can be improved by performing heat pressing at a temperature above the melting point (335°C) of the LCP film (see Comparative Examples 11 and 12 of Patent Document 1). However, it is recorded that if this operation is performed, the dimensional accuracy will be significantly deteriorated, and therefore the desired purpose cannot be achieved (see

[0048] of Patent Document 1). In addition, it is easy to imagine that if heat pressing is performed at a temperature exceeding the melting point of the LCP film, the production cost of the resulting flexible laminate will be higher than that of a laminate that is not the case, and basic properties such as mechanical strength will be reduced.

[0011] As described above, the manufacturing method of Patent Document 1 has insufficient process margin from the perspective of continuous production of high-quality flexible laminates, and is insufficient in productivity and versatility from an industrial perspective. That is, there is a technical limit to only precise temperature control in the thermal compression bonding process, and a new design policy that can break through such a technical level is required.

[0012] The present invention is made in view of the above problems. The purpose of the present invention is to provide an LCP extruded film that can improve the process margin when manufacturing a flexible laminate without excessively damaging the excellent basic properties of liquid crystal polymers such as mechanical properties, electrical properties, high frequency properties, heat resistance, and hygroscopicity.

[0013] In addition, another object of the present invention is to provide an LCP extruded film that can easily obtain a flexible laminate having a high peel strength with a metal foil even under milder manufacturing conditions than the prior art. In addition, another object of the present invention is to provide a flexible laminate having a high peel strength with a metal foil and excellent productivity and economy, and a manufacturing method that can easily obtain such a flexible laminate with good reproducibility.

[0014] Means for solving problems

[0015] In order to solve the above-mentioned problems, the inventors of the present application conducted in-depth research focusing on the characteristics and crystallization states of various LCP extruded films. As a result, they found that the above-mentioned problems can be solved by using LCP extruded films in which aromatic polyester-based liquid crystal polymers have a specified crystallinity, thereby completing the present invention.

[0016] That is, the present invention provides various specific aspects shown below.

[0017] (1) An LCP extruded film comprising an aromatic polyester-based liquid crystal polymer, wherein the aromatic polyester-based liquid crystal polymer has at least one selected from the group consisting of p-hydroxybenzoic acid, terephthalic acid, isophthalic acid, 6-naphthalene dicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybiphenol, ethylene terephthalate and their derivatives and 6-hydroxy-2-naphthoic acid and its derivatives as monomer components, and the solubility of the LCP extruded film in pentafluorophenol at 60°C is not less than 25%.

[0018] (2) The LCP extruded film as described in (1), which has a melting point of 250 to 360°C.

[0019] (3) The LCP extruded film according to (1) or (2), wherein the content of 6-hydroxy-2-naphthoic acid in the aromatic polyester-based liquid crystal polymer is 10 mol% or more and less than 70 mol%.

[0020] (4) The LCP extruded film according to any one of (1) to (3), wherein the film thickness is 10 μm or more and less than 500 μm.

[0021] (5) A method for producing a flexible laminate, which comprises at least the following steps: a step of preparing one or more LCP extruded films, wherein the LCP extruded films contain an aromatic polyester-based liquid crystal polymer, wherein the aromatic polyester-based liquid crystal polymer has at least one selected from the group consisting of p-hydroxybenzoic acid, terephthalic acid, isophthalic acid, 6-naphthalene dicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybiphenol, ethylene terephthalate and their derivatives and 6-hydroxy-2-naphthoic acid and its derivatives as monomer components, and the solubility of the LCP extruded film in pentafluorophenol at 60°C is not less than 25%; a step of laminating the LCP extruded film with one or more metal foils; and a step of heating the obtained laminate to a temperature that is 50°C lower than the melting point of the aromatic polyester-based liquid crystal polymer and below the melting point, and performing heat compression bonding.

[0022] (6) The method for producing a flexible laminate according to (5), wherein the LCP extruded film has a melting point of 250 to 360°C.

[0023] (7) The method for producing a flexible laminate according to (5) or (6), wherein the content of 6-hydroxy-2-naphthoic acid in the aromatic polyester-based liquid crystal polymer is 10 mol% or more and less than 70 mol%.

[0024] (8) The method for producing a flexible laminate according to any one of (5) to (7), wherein the LCP extruded film has a thickness of 10 μm or more and less than 500 μm.

[0025] (9) The method for producing a flexible laminate according to any one of (5) to (8), wherein the metal foil is one or more selected from the group consisting of copper foil, aluminum foil, stainless steel foil, and alloy foil of copper and aluminum.

[0026] (10) The method for producing a flexible laminate according to any one of (5) to (9), wherein the obtained flexible laminate has a peel strength between the LCP extruded film and the metal foil of 1.0 (N / mm) or more.

[0027] (11) A flexible laminate, characterized in that it comprises: one or more LCP extruded films, wherein the LCP extruded films contain an aromatic polyester-based liquid crystal polymer, wherein the aromatic polyester-based liquid crystal polymer has at least one selected from the group consisting of p-hydroxybenzoic acid, terephthalic acid, isophthalic acid, 6-naphthalene dicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybiphenol, ethylene terephthalate and their derivatives and 6-hydroxy-2-naphthoic acid and its derivatives as monomer components, and the solubility of the LCP extruded film in pentafluorophenol at 60°C is not less than 25%; and one or more metal foils, wherein the metal foils are arranged on the surface of at least one side of the LCP extruded film.

[0028] (12) The flexible laminate according to (11), wherein the LCP extruded film has a melting point of 250 to 360°C.

[0029] (13) The flexible laminate according to (11) or (12), wherein the content of 6-hydroxy-2-naphthoic acid in the aromatic polyester-based liquid crystal polymer is 10 mol% or more and less than 70 mol%.

[0030] (14) The flexible laminate according to any one of (11) to (13), wherein the peel strength between the LCP extruded film and the metal foil is 1.0 (N / mm) or more.

[0031] (15) The flexible laminate according to any one of (11) to (14), wherein the LCP extruded film has a thickness of 10 μm or more and less than 500 μm.

[0032] Effects of the Invention

[0033] According to the present invention, it is possible to provide an LCP extruded film that can improve the process margin when manufacturing a flexible laminate without excessively damaging the excellent basic properties of liquid crystal polymers such as mechanical properties, electrical properties, high-frequency properties, heat resistance, and hygroscopicity. In addition, according to a preferred embodiment of the present invention, it is possible to provide an LCP extruded film that can easily obtain a flexible laminate with high peel strength with a metal foil even under manufacturing conditions that are milder than those of the prior art. In addition, according to another preferred embodiment of the present invention, it is possible to provide a flexible laminate with high peel strength with a metal foil and excellent productivity and economy, as well as a manufacturing method that can easily obtain such a flexible laminate with good reproducibility. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] [ Figure 1 ] is a schematic diagram showing an LCP extruded film 11 according to one embodiment.

[0035] [ Figure 2 ] is a schematic diagram showing a flexible laminate 31 according to one embodiment. DETAILED DESCRIPTION

[0036] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. It should be noted that, with respect to positional relationships such as up, down, left, and right, unless otherwise specified, the positional relationships shown in the accompanying drawings shall be taken as a reference. In addition, the dimensional ratios of the accompanying drawings are not limited to the ratios shown in the drawings. Among them, the following embodiments are examples for illustrating the present invention, and the present invention is not limited to these. That is, the present invention can be implemented with arbitrary changes within the scope of the gist thereof. It should be noted that in this specification, the expression of a numerical range such as "1 to 100" includes both its lower limit "1" and upper limit "100". In addition, the expression of other numerical ranges is the same.

[0037] (LCP extruded film)

[0038] Figure 1 The schematic diagram of the LCP extruded film 11 of the present embodiment is shown. The LCP extruded film 11 of the present embodiment is characterized in that it contains an aromatic polyester-based liquid crystal polymer, the aforementioned aromatic polyester-based liquid crystal polymer has 6-hydroxy-2-naphthoic acid and its derivatives (hereinafter, sometimes referred to as "monomer component B") as a basic structure, and has at least one selected from the group consisting of p-hydroxybenzoic acid, terephthalic acid, isophthalic acid, 6-naphthalene dicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybiphenol, ethylene terephthalate and their derivatives (hereinafter, sometimes referred to as "monomer component A") as a monomer component, and the solubility of the aforementioned LCP extruded film in pentafluorophenol at 60°C is 25% or more.

[0039] The above-mentioned aromatic polyester-based liquid crystal polymer containing monomer component A and monomer component B has linear chains of molecules arranged regularly in a molten state to form an anisotropic melt phase, typically showing thermotropic liquid crystal properties, and has excellent basic properties in terms of mechanical properties, electrical properties, high-frequency properties, heat resistance, hygroscopicity, etc. It should be noted that the properties of the anisotropic melt phase of the above-mentioned aromatic polyester-based liquid crystal polymer can be confirmed by known methods such as polarized light inspection using orthogonal polarizers. More specifically, the confirmation of the anisotropic melt phase can be implemented in the following manner: using a Leitz polarizing microscope, a sample placed on a Leitz hot stage is observed at a magnification of 40 times in a nitrogen atmosphere.

[0040] The above-mentioned aromatic polyester-based liquid crystal polymer can have any structure as long as it has monomer component A and monomer component B as essential units. For example, it can have more than two monomer components A, or it can have more than three monomer components A. In addition, the above-mentioned aromatic polyester-based liquid crystal polymer can also contain other monomer components other than monomer components A and monomer component B. That is, the aromatic polyester-based liquid crystal polymer can be a condensation product of more than two monomer components formed only by monomer components A and monomer component B, or it can be a condensation product of more than three monomer components formed by monomer components A, monomer component B and other monomer components. As other monomer components (hereinafter, sometimes referred to as "monomer component C"), monomer components other than the above-mentioned monomer components A and monomer component B can be cited, specifically aromatic or aliphatic dihydroxy compounds and their derivatives; aromatic or aliphatic dicarboxylic acids and their derivatives; aromatic hydroxycarboxylic acids and their derivatives; aromatic diamines, aromatic hydroxyamines or aromatic aminocarboxylic acids and their derivatives; etc., but are not particularly limited to these.

[0041] It should be noted that in this specification, "derivatives" refer to monomer components (hereinafter sometimes referred to as "monomer components having substituents") in which a halogen atom (e.g., fluorine atom, chlorine atom, bromine atom, iodine atom), an alkyl group having 1 to 5 carbon atoms (e.g., methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, etc.), an aryl group such as phenyl, a hydroxyl group, an alkoxy group having 1 to 5 carbon atoms (e.g., methoxy, ethoxy, etc.), a carbonyl group, -O-, -S-, -CH2-, etc., is introduced into a part of the above-mentioned monomer components. Here, the "derivatives" may be ester-forming monomers such as acylates, ester derivatives, or acyl halides of the monomer components A and B that may have the above-mentioned modifying groups.

[0042] Preferred aromatic polyester liquid crystal polymers include: binary polycondensates of p-hydroxybenzoic acid and its derivatives and 6-hydroxy-2-naphthoic acid and its derivatives; ternary or higher polycondensates of p-hydroxybenzoic acid and its derivatives, 6-hydroxy-2-naphthoic acid and its derivatives and monomer component C; polycondensates of p-hydroxybenzoic acid and its derivatives, 6-hydroxy-2-naphthoic acid and its derivatives and a monomer component C selected from terephthalic acid, isophthalic acid, 6-naphthalene dicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-diphenol A ternary or higher polycondensate formed from one or more of the group consisting of hydroxydiphenol, ethylene terephthalate and their derivatives; a quaternary or higher polycondensate formed from one or more of p-hydroxybenzoic acid and its derivatives, 6-hydroxy-2-naphthoic acid and its derivatives, terephthalic acid, isophthalic acid, 6-naphthalene dicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxydiphenol, ethylene terephthalate and their derivatives, and one or more monomer components C. These can be obtained as polymers having a lower melting point than, for example, homopolymers of p-hydroxybenzoic acid, and therefore, LCP extruded films using these are excellent in molding processability during thermal compression bonding with an adherend.

[0043] From the viewpoint of lowering the melting point of the aromatic polyester-based liquid crystal polymer, improving the molding processability during the thermocompression bonding of the LCP extruded film and the adherend, or obtaining high peel strength during the thermocompression bonding of the LCP extruded film and the metal foil, the molar ratio content of the monomer component A relative to the aromatic polyester-based liquid crystal polymer is preferably 30 mol% or more and less than 90 mol%, more preferably 50 mol% or more and less than 90 mol%, further preferably 60 mol% or more and less than 90 mol%, more preferably 70 mol% or more and less than 85 mol%. Similarly, the molar ratio content of the monomer component B relative to the aromatic polyester-based liquid crystal polymer is preferably 10 mol% or more and less than 70 mol%, more preferably 10 mol% or more and less than 50 mol%, further preferably 10 mol% or more and less than 40 mol%, more preferably 15 mol% or more and less than 30 mol%.

[0044] The content of the monomer component C in the aromatic polyester-based liquid crystal polymer is preferably 10% by mass or less, more preferably 8% by mass or less, further preferably 5% by mass or less, and preferably 3% by mass or less in terms of molar ratio.

[0045] The method for producing the aromatic polyester-based liquid crystal polymer can be a known method, and is not particularly limited. A known polycondensation method for forming an ester bond based on the above-mentioned monomer components, such as melt polymerization, melt acid hydrolysis, slurry polymerization, etc., can be applied. When these polymerization methods are applied, an acylation or acetylation step can be performed according to a conventional method.

[0046] The LCP extruded film can be obtained by forming a molten resin composition containing the above-mentioned aromatic polyester-based liquid crystal polymer into a film using a known melt film forming method such as a T-die method and an inflation method.

[0047] The LCP extruded film preferably contains the above-mentioned aromatic polyester-based liquid crystal polymer as a main component as a resin component. Here, the term "containing an aromatic polyester-based liquid crystal polymer as a main component" means that the film contains 80 parts by mass or more, preferably 90 parts by mass or more, more preferably 95 parts by mass or more, particularly preferably 97 parts by mass or more, and 100 parts by mass or less of the aromatic polyester-based liquid crystal polymer relative to 100 parts by mass of the total amount of the resin component of the LCP extruded film.

[0048] In addition, for LCP extruded film, in addition to the above-mentioned resin components, additives known in the industry, such as higher fatty acids with carbon atoms of 10 to 25, higher fatty acid esters, higher fatty acid amides, higher fatty acid metal salts, polysiloxanes, fluororesins and other mold release improvers, dyes, pigments, carbon black and other colorants, organic fillers, inorganic fillers, antioxidants, heat stabilizers, ultraviolet absorbers, antistatic agents, surfactants, etc. can be included in the molten resin composition during the film formation of the LCP extruded film. These additives can be used alone or in combination of two or more. The content of the additive is not particularly limited, but from the viewpoint of molding processability, thermal stability, etc., it is preferably 0.01 to 10% by mass, more preferably 0.1 to 7% by mass, and further preferably 0.5 to 5% by mass relative to the total amount of the LCP extruded film.

[0049] The melting point of the LCP extruded film is not particularly limited, but from the viewpoints of heat resistance and processability of the film, it is preferably 200 to 400° C., and especially from the viewpoint of improving the thermal compression bonding with the metal foil, it is preferably 250 to 360° C., more preferably 260 to 355° C., further preferably 270 to 350° C., and particularly preferably 275 to 345° C. It should be noted that in this specification, the melting point of the LCP extruded film refers to the melting peak temperature in differential scanning calorimetry (DSC) when the film for compression bonding is heated at a heating rate of 20° C. / min (first heating).

[0050] In addition, one feature of the LCP extruded film of the present embodiment is that the solubility in pentafluorophenol at 60°C is 25% or more. If the solubility of the LCP extruded film in pentafluorophenol at 60°C is 25% or more, preferably 30% or more, and more preferably 40% or more, a high peel strength with the metal foil can be obtained even when the film is thermocompressed with the metal foil at a temperature below the melting point of the film. Moreover, by thermocompressing such an LCP extruded film at a temperature below the melting point of the film, the process margin when manufacturing a flexible laminate can be improved without excessively damaging the excellent basic properties of the liquid crystal polymer.

[0051] The technical concept of the present invention is described in detail below. In the case of using an LCP extruded film having a low solubility at 60°C in pentafluorophenol, if the film is hot-pressed with a metal foil at a temperature below the melting point of the film, it is difficult to obtain a high peel strength with the metal foil. It is therefore believed that when hot-pressing is performed at a temperature below the melting point, the melting of the liquid crystal portion is not fully performed. Therefore, due to the fact that the internal strain is not relaxed, the amount of the crystalline portion that remains unmelted is large, or the spherulites are large in size and there are many remaining spherulites, the close contact state during pressing is prone to unevenness, so high peel strength cannot be obtained. That is, it is believed that when hot-pressing with a metal foil at a temperature below the melting point of the film, the crystalline state of the LCP extruded film itself strongly affects the peel strength with the metal foil.

[0052] Moreover, according to the view of the inventor of the present application, it is found that in order to obtain high peel strength by hot pressing with metal foil at a temperature below the melting point of the film, it is necessary to use an LCP extruded film in a crystalline state in which the internal strain is small, the amount of the remaining crystalline part that is not melted is small, or the spherulite size is small and the remaining spherulites are few. Here, for the crystalline state of the LCP extruded film, in addition to the type of the aromatic polyester-based liquid crystal polymer used, it also changes according to the thermal history such as heat treatment when manufacturing raw material pellets, heat treatment when manufacturing LCP extruded film, and post-heating treatment (annealing treatment) of the LCP extruded film after manufacturing. Moreover, if it is an LCP extruded film in a crystalline state in which the internal strain is small, the amount of the remaining crystalline part that is not melted is small, or the spherulite size is small and the remaining spherulites are few, then even if it is hot pressed with metal foil at a temperature below the melting point of the film, high peel strength can be obtained. That is, in other words, it can be said that the present invention adopts the solubility rate in pentafluorophenol as an indicator of the LCP extruded film having the crystalline state adjusted in this way.

[0053] It should be noted that, in this specification, the solubility rate of the LCP extruded film in pentafluorophenol refers to: after immersing 10 mg of the LCP extruded film in 10 g of pentafluorophenol and placing it at 60° C. for 15 minutes under stirring to dissolve it, the undissolved and residual resin solid matter is taken out and calculated. The solubility rate of the LCP extruded film in pentafluorophenol can be appropriately adjusted by the type of aromatic polyester-based liquid crystal polymer used, the heat treatment conditions when manufacturing the raw material pellets containing it, the heat treatment conditions when manufacturing the LCP extruded film, the annealing treatment conditions of the LCP extruded film after manufacturing, etc.

[0054] The thickness of the LCP extruded film can be appropriately set according to the required performance, and is not particularly limited. Considering the operability and productivity during melt extrusion molding, it is preferably 5 μm or more and less than 1000 μm, more preferably 10 μm or more and less than 500 μm, further preferably 20 μm or more and less than 300 μm, and further preferably 30 μm or more and less than 250 μm.

[0055] The LCP extruded film of the present embodiment can be an unstretched film or a stretched film. Regardless of which one, usually, due to the presence of the anisotropic melt phase of the aromatic polyester-based liquid crystal polymer during melt extrusion, it is easy to obtain an oriented LCP extruded film. Therefore, the linear thermal expansion coefficient (CTE) of the film MD direction of the LCP extruded film is preferably -40 to 0 ppm / K, and the linear thermal expansion coefficient of the film TD direction is preferably 0 to 120 ppm / K. In addition, the linear thermal expansion coefficient in the film thickness direction is preferably 300 ppm / K or more.

[0056] For example, an unstretched film can be obtained by a melt film forming method using a T die. In this case, usually, due to the presence of a melt phase for the anisotropy of the aromatic polyester-based liquid crystal polymer during melt extrusion, an unstretched film with high orientation can be obtained. In the case where the LCP extruded film is an unstretched film, the linear thermal expansion coefficient in the MD direction of the film is preferably -40 to 0 ppm / K, and the linear thermal expansion coefficient in the TD direction of the film is preferably 0 to 120 ppm / K. In addition, the linear thermal expansion coefficient in the thickness direction of the film is preferably 300 ppm / K or more.

[0057] On the other hand, for example, a stretched film can be obtained by a blown melt film method. In this case, due to the flow during molding, a stretched film with low orientation can be obtained. In the case where the LCP extruded film is a stretched film, the linear thermal expansion coefficient in the MD direction of the film is preferably 0 to 40 ppm / K, and the linear thermal expansion coefficient in the TD direction of the film is preferably 0 to 40 ppm / K. In addition, the linear thermal expansion coefficient in the thickness direction of the film is preferably less than 300 ppm / K.

[0058] In addition, for the above-mentioned unstretched film or stretched film, heat treatment (heat treatment, cooling treatment) can be further performed, so that the orientation of the polymer chain is relaxed, thereby improving the film dimensional stability in advance. These heat treatments are performed using methods known in the industry, such as contact heat treatment, non-contact heat treatment, etc., and their types are not particularly limited. For example, known equipment such as non-contact heaters, baking ovens, blowing devices, hot rollers, cooling rollers, hot presses, double belt hot presses can be used to perform heat setting. At this time, as required, a stripping film and a porous film known in the industry can be configured on the surface of the LCP extruded film and heat treated. In addition, in the case of performing this heat treatment, from the viewpoint of the control of orientation, it is also preferred to use the following method: a stripping film and a porous film are configured on the surface and back of the LCP extruded film, and hot pressing is performed while the endless belt of the double belt press is clamped between, and thereafter the stripping film and the porous film are removed. For the heat treatment at this time, in order to control the crystallization state of the LCP extruded film, it is preferably carried out at a temperature higher than the melting point of the aromatic polyester-based liquid crystal polymer and below a temperature 70°C higher than the melting point. The heat pressing conditions at this time can be appropriately set according to the desired performance, and are not particularly limited. For example, when using a double-belt press, it is preferably carried out at a surface pressure of 0.5 to 10 MPa under a heating temperature of 250 to 430°C. On the other hand, when using a non-contact heater or an oven, it is preferably carried out at 200 to 320°C for 1 to 20 hours. Moreover, the linear thermal expansion coefficient of the treated LCP extruded film in the MD direction of the film is preferably 0 to 40 ppm / K, and the linear thermal expansion coefficient in the TD direction of the film is preferably 0 to 40 ppm / K. In addition, the linear thermal expansion coefficient in the thickness direction of the film is preferably less than 120 ppm / K.

[0059] (Flexible laminate)

[0060] Figure 2 The flexible laminate 31 of the present embodiment is schematically shown. The flexible laminate 31 (metal laminate film) of the present embodiment comprises the above-mentioned LCP extruded film 11 and one or more metal foils 21, wherein the metal foils 21 are disposed on the surface of at least one side of the LCP extruded film 11. Here, in the present specification, the so-called "disposed on the surface side of one side (the other side) of ~" not only includes a method in which the metal foil 21 is disposed only on the surface 11a of one side of the LCP extruded film 11, but also includes any method in which the metal foil 21 is disposed on the surface 11b of the other side of the LCP extruded film 11, and the metal foil 21 is disposed on the surfaces 11a and 11b on both sides of the LCP extruded film 11.

[0061] The material of the metal foil is not particularly limited, and gold, silver, copper, copper alloy, nickel, nickel alloy, aluminum, aluminum alloy, iron, iron alloy, etc. can be cited. Among these, copper foil, aluminum foil, stainless steel foil, and alloy foil of copper and aluminum are preferred, and copper foil is more preferred. As the copper foil, any copper foil manufactured by rolling method or electrolysis method can be used, but electrolytic copper foil and rolled copper foil with large surface roughness are preferred. The thickness of the metal foil can be appropriately set according to the desired performance and is not particularly limited. It is usually preferably 1.5 to 1000 μm, more preferably 2 to 500 μm, further preferably 5 to 150 μm, and particularly preferably 7 to 100 μm. It should be noted that as long as the effect of the present invention is not impaired, the metal foil may also be subjected to surface treatments such as chemical surface treatments such as acid cleaning.

[0062] The method of providing the metal foil on the surface of the LCP extruded film can be carried out according to conventional methods, and is not particularly limited. It can be any of the following methods: a method of laminating a metal foil on the LCP extruded film and bonding or pressing the two layers; a physical method (dry method) such as sputtering and evaporation; a chemical method (wet method) such as electroless plating or electrolytic plating after electroless plating; a method of applying a metal paste, etc.

[0063] As a preferred lamination method, the following method can be cited: superimposing an LCP extruded film and a metal foil to form a laminated body with a metal foil placed on the LCP extruded film, and performing heat pressing while clamping the laminated body between a pair of endless belts of a double-belt press. As described above, the LCP extruded film used in the present embodiment can obtain a higher peel strength with the metal foil than before, even when it is heat pressed with the metal foil at a temperature below the melting point of the film. Therefore, by performing heat pressing under the temperature conditions described above, such an LCP extruded film is heat pressed at a temperature below the melting point of the film, thereby improving the process margin when manufacturing a flexible laminated body without excessively damaging the excellent basic properties of the liquid crystal polymer, and being able to easily achieve a flexible laminated body with excellent productivity and economy with good reproducibility.

[0064] At this time, the temperature range during hot pressing can be a range in which the LCP extruded film is substantially non-melting, that is, a temperature above 50°C lower than the melting point of the aromatic polyester-based liquid crystal polymer and below the melting point. By performing hot pressing at a lower temperature, the process margin when manufacturing the flexible laminate can be improved without excessively damaging the excellent basic properties of the liquid crystal polymer, and a flexible laminate with excellent productivity and economy can be easily achieved with good reproducibility. In addition, by performing hot pressing on the higher temperature side, there is a tendency for the peel strength between the LCP extruded film and the metal foil to be further improved. It should be noted that the LCP extruded film of the present embodiment can also be hot pressed with the metal foil at a temperature exceeding the melting point of the film. Since an LCP extruded film in a crystalline state suitable for hot pressing is used, even in this case, there is a tendency to obtain a higher peel strength than before.

[0065] The temperature during heat pressing can be appropriately set according to the required performance based on these viewpoints, and is not particularly limited, but is preferably a temperature 50°C lower than the melting point of the aromatic polyester liquid crystal polymer and below the melting point, more preferably a temperature 40°C lower than the melting point and below the melting point, further preferably a temperature 30°C lower than the melting point and below the melting point, and particularly preferably a temperature 20°C lower than the melting point and below the melting point. It should be noted that the temperature during heat pressing is a value measured in the form of the surface temperature of the LCP extruded film of the aforementioned laminate. In addition, the pressing conditions at this time can be appropriately set according to the desired performance, and are not particularly limited. For example, when using a double-belt press, it is preferably carried out at a surface pressure of 0.5 to 10 MPa under a heating temperature of 200 to 360°C.

[0066] The flexible laminate of this embodiment only needs to have a double-layer structure of LCP extruded film and metal foil, and may also have a further laminated structure. For example, it can be made into a three-layer structure such as metal foil / LCP extruded film / metal foil, LCP extruded film / metal foil / LCP extruded film; a five-layer structure such as metal foil / LCP extruded film / metal foil / LCP extruded film / metal foil; or a multi-layer structure having at least the above double-layer structure. In addition, multiple (for example, 2 to 50) flexible laminates can be stacked and thermally pressed.

[0067] In the flexible laminate of the present embodiment, the peel strength between the LCP extruded film and the metal foil is not particularly limited, but from the viewpoint of having a higher peel strength, it is preferably 1.0 (N / mm) or more, more preferably 1.1 (N / mm) or more, and further preferably 1.2 (N / mm) or more. It should be noted that in this specification, "peel strength" refers to the value measured using the method and conditions described in the embodiments described later. As described above, in the flexible laminate of the present embodiment, a higher peel strength can be achieved compared to the prior art, and therefore, the peeling of the LCP extruded film and the metal foil can be suppressed in, for example, the heating process of substrate manufacturing. In addition, when obtaining a peel strength equivalent to that of the prior art, a mild manufacturing condition can be applied, and therefore, the degradation of the basic performance of the liquid crystal polymer can be suppressed while maintaining the same degree of peel strength as before.

[0068] For the flexible laminate of the present embodiment, at least a portion of the metal foil can be pattern-etched, etc., and used as a raw material for electronic circuit substrates, multilayer substrates, etc., and can also be used for high heat dissipation substrates, antenna substrates, optoelectronic hybrid substrates, IC packaging, etc. In addition, the flexible laminate of the present embodiment can be made into a laminate with excellent high-frequency characteristics and low dielectric properties, excellent adhesion between the LCP extruded film and the metal foil, and good dimensional stability, and therefore, it becomes a particularly useful raw material as an insulating material for flexible printed wiring boards (FPCs) and the like in fifth-generation mobile communication systems (5G), millimeter-wave radars, etc.

[0069] Example

[0070] The following examples and comparative examples are given to more specifically illustrate the features of the present invention, but the present invention is not subject to any limitation thereof. That is, the material, usage, ratio, processing content, processing steps etc. shown in the following examples can be appropriately changed, as long as they do not depart from the gist of the present invention. In addition, the values ​​of the various manufacturing conditions and evaluation results in the following examples have the meaning of the preferred upper limit or the preferred lower limit in the embodiment of the present invention, and the preferred numerical range can be the scope specified by the combination of the aforementioned upper limit or lower limit and the value of the following examples or the values ​​of the examples each other.

[0071] (Example 1)

[0072] In a reaction tank equipped with a stirrer and a vacuum distillation apparatus, p-hydroxybenzoic acid (74 mol%), 6-hydroxy-2-naphthoic acid (26 mol%), and acetic anhydride in an amount of 1.025 times the total amount of the monomers were charged, and the reaction tank was heated to 150°C under a nitrogen atmosphere, and maintained for 30 minutes. Then, the temperature was rapidly raised to 190°C while distilling off acetic acid produced as a by-product, and maintained for 1 hour to obtain an acetylated reaction product. The obtained acetylated reaction product was heated to 320°C over 3.5 hours, and then the pressure was reduced to 2.7 kPa over about 30 minutes to perform melt polycondensation, and then the pressure was gradually reduced to normal pressure to obtain a polymer solid. The obtained polymer solid was crushed and granulated at 300°C using a twin-screw extruder to obtain pellets of an aromatic polyester-based liquid crystal polymer (molar ratio of 74:26) composed of p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid. The obtained pellets were used to form a film by a T-die casting method, thereby obtaining an LCP extruded film having a melting point of 280° C. and a thickness of 50 μm.

[0073] (Example 2)

[0074] In a reaction tank equipped with a stirrer and a vacuum distillation apparatus, p-hydroxybenzoic acid (80 mol%), 6-hydroxy-2-naphthoic acid (19 mol%), terephthalic acid (1 mol%), and acetic anhydride in an amount of 1.025 times the total amount of the monomers were charged, and the reaction tank was heated to 150°C under a nitrogen atmosphere, and maintained for 30 minutes. Then, the temperature was rapidly raised to 190°C while distilling off acetic acid produced as a by-product, and maintained for 1 hour to obtain an acetylated reaction product. The obtained acetylated reaction product was heated to 330°C over 3.5 hours, and then the pressure was reduced to 2.7 kPa over about 30 minutes to perform melt polycondensation, and then the pressure was gradually reduced to normal pressure to obtain a polymer solid. The obtained polymer solid was crushed and granulated at 330°C using a twin-screw extruder to obtain pellets of an aromatic polyester-based liquid crystal polymer (molar ratio of 80:19:1) composed of p-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid and terephthalic acid. The obtained pellets were used to form a film by a T-die casting method, thereby obtaining an LCP extruded film having a melting point of 310° C. and a thickness of 50 μm.

[0075] (Example 3)

[0076] In a reaction tank equipped with a stirrer and a vacuum distillation apparatus, p-hydroxybenzoic acid (22 mol%), 6-hydroxy-2-naphthoic acid (49 mol%), terephthalic acid (16 mol%), 4,4'-biphenol (13 mol%), and acetic anhydride in an amount of 1.025 times the total amount of the monomers were charged, and the reaction tank was heated to 150° C. in a nitrogen atmosphere, and maintained for 30 minutes, and then the temperature was rapidly raised to 190° C. while distilling off acetic acid generated as a by-product, and maintained for 1 hour to obtain an acetylated reaction product. The obtained acetylated reaction product was heated to 360° C. over 4 hours, and then the pressure was reduced to 2.7 kPa over about 30 minutes to perform melt polycondensation, and then the pressure was gradually reduced to normal pressure to obtain a polymer solid. The obtained polymer solid was crushed and granulated at 360°C using a twin-screw extruder to obtain pellets of an aromatic polyester liquid crystal polymer (molar ratio of 22:49:16:13) composed of p-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, terephthalic acid and 4,4'-biphenol. The obtained pellets were used to form a film using a T-die casting method to obtain an LCP extruded film having a melting point of 340°C and a thickness of 50 μm.

[0077] (Example 4)

[0078] The LCP extruded film of Example 1 was subjected to contact heat treatment at 320° C. for 30 seconds using a double belt heat press, thereby obtaining an LCP extruded film having a melting point of 280° C.

[0079] (Example 5)

[0080] The LCP extruded film of Example 1 was subjected to non-contact heat treatment at 260°C for 2 hours in an oven and then to non-contact heat treatment at 280°C for 4 hours to obtain an LCP extruded film having a melting point of 290°C.

[0081] (Comparative Example 1)

[0082] The LCP extruded film of Example 1 was subjected to non-contact heat treatment at 260°C for 2 hours and further to non-contact heat treatment at 290°C for 20 hours in an oven to obtain an LCP extruded film having a melting point of 310°C and a thickness of 50 μm.

[0083] (Comparative Example 2)

[0084] In a reaction tank equipped with a stirrer and a vacuum distillation apparatus, p-hydroxybenzoic acid (72 mol%), 6-hydroxy-2-naphthoic acid (27 mol%), terephthalic acid (1 mol%), and acetic anhydride in an amount of 1.025 times the total amount of the monomers were charged, and the reaction tank was heated to 150°C in a nitrogen atmosphere, and maintained for 30 minutes. Then, the temperature was rapidly raised to 190°C while distilling off acetic acid produced as a by-product, and maintained for 1 hour to obtain an acetylated reaction product. The obtained acetylated reaction product was heated to 320°C over 3.5 hours, and then the pressure was reduced to 2.7 kPa over about 30 minutes to perform melt polycondensation, and then the pressure was gradually reduced to normal pressure to obtain a polymer solid. The obtained polymer solid was crushed and granulated at 300°C using a twin-screw extruder to obtain pellets of an aromatic polyester-based liquid crystal polymer (molar ratio of 72:27:1) composed of p-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid and terephthalic acid. The obtained pellets were used to form a film by an inflation method, and then non-contact heat treatment was performed in an oven at 260°C for 2 hours and further at 290°C for 6 hours to obtain an LCP extruded film having a melting point of 335°C and a thickness of 50 μm.

[0085] <Dissolution rate>

[0086] The dissolution rate of the LCP extruded film was measured under the following conditions.

[0087] 10 mg of the freeze-crushed LCP extruded film was immersed in 10 g of pentafluorophenol at 60°C and allowed to stand for 15 minutes under stirring to dissolve it. The undissolved and residual resin solid matter was filtered out using a 400-mesh metal mesh and dried. The dissolution rate of the LCP extruded film was calculated based on the mass of the metal mesh before and after the filtration separation.

[0088] Dissolution rate (%) = (LCP extruded film mass - (metal mesh mass after filtration separation and drying - metal mesh mass before filtration separation)) / LCP extruded film mass × 100

[0089] <Peel Strength>

[0090] The peel strength of the flexible laminate was measured under the following conditions.

[0091] Under the temperature conditions described in Tables 1 and 2, the LCP extruded film to be measured and the electrolytic copper foil (TQ-M7VSP, manufactured by Mitsui Kinzoku Co., Ltd.) were heat-pressed for 1 minute at a surface pressure of 5 MPa, thereby obtaining a flexible laminate formed of the LCP extruded film and the copper foil. From the obtained flexible laminate, a test piece with a width of 10 mm was cut out in a long strip shape, and a tensile tester (Strograph) VE1D (manufactured by Toyo Seiki Seisaku-sho Co., Ltd.) was used to peel the copper foil in a 180-degree direction at a tensile speed of 50 mm / min under an environment of a temperature of 23°C and a relative humidity of 50%, and the peel strength of the copper foil was measured and evaluated according to the following criteria.

[0092] ◎Material damage (cannot be peeled off) exceeds the measurement limit, about 1.5N / mm or more

[0093] ○Peeling 1.0N / mm or more

[0094] × Peeling less than 1.0N / mm

[0095] Tables 1 and 2 show the results.

[0096] [Table 1]

[0097]

[0098] [Table 2]

[0099]

[0100] Industrial Applicability

[0101] For the LCP extruded film of the present invention, it is not only excellent in the excellent basic properties of liquid crystal polymers such as mechanical properties, electrical properties, high-frequency properties, heat resistance, and hygroscopicity, but also can easily obtain a flexible laminate with high peel strength with metal foil, and in addition, it can improve the process margin when manufacturing the flexible laminate. Therefore, the LCP extruded film of the present invention can be widely and effectively used in electronic circuit substrates, multi-layer substrates, high heat dissipation substrates, antenna substrates, optoelectronic hybrid substrates, IC packaging and other uses, especially due to the excellent high-frequency properties and low dielectric properties, so it can be used as the fifth generation mobile communication system (5G), millimeter wave radar and other flexible printed wiring board (FPC) and other insulating materials and is particularly widely and effectively used.

[0102] Description of Reference Numerals

[0103] 11···LCP extrusion film

[0104] 21···Metal foil

[0105] 31···Flexible laminate

Claims

1. An LCP extruded film comprising an aromatic polyester-based liquid crystal polymer, wherein the aromatic polyester-based liquid crystal polymer comprises at least a monomer component A and a monomer component B, The monomer component A is one or more selected from the group consisting of p-hydroxybenzoic acid, terephthalic acid, isophthalic acid, 6-naphthalene dicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybiphenol, ethylene terephthalate and derivatives thereof, The monomer component B is selected from 6-hydroxy-2-naphthoic acid and its derivatives, The molar ratio of the monomer component A to the aromatic polyester liquid crystal polymer is 60 mol% or more and less than 90 mol%, and the molar ratio of the monomer component B to the aromatic polyester liquid crystal polymer is 10 mol% or more and less than 40 mol%. The solubility of the LCP extruded film in pentafluorophenol at 60° C. is greater than 25%.

2. The LCP extruded film of claim 1, having a melting point of 250 to 360°C.

3. The LCP extruded film of claim 1, wherein The film thickness is 10 μm or more and less than 500 μm.

4. A method for producing a flexible laminate, comprising at least the following steps: A step of preparing one or more LCP extruded films, wherein the LCP extruded films contain an aromatic polyester-based liquid crystal polymer, wherein the aromatic polyester-based liquid crystal polymer has at least a monomer component A and a monomer component B, wherein the monomer component A is one or more selected from the group consisting of p-hydroxybenzoic acid, terephthalic acid, isophthalic acid, 6-naphthalene dicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybiphenol, ethylene terephthalate and derivatives thereof, and the monomer component B is selected from 6-hydroxy-2-naphthoic acid and derivatives thereof, wherein the solubility of the LCP extruded film in pentafluorophenol at 60° C. is 25% or more, and the content ratio of the monomer component A in terms of molar ratio is 60 mol% or more and less than 90 mol% relative to the aromatic polyester-based liquid crystal polymer, and the content ratio of the monomer component B in terms of molar ratio is 10 mol% or more and less than 40 mol%; The step of laminating the LCP extruded film with one or more metal foils; and The obtained laminate is heated to a temperature not less than 50° C. lower than the melting point of the aromatic polyester-based liquid crystal polymer and not more than the melting point, and then subjected to thermocompression bonding.

5. The method for producing a flexible laminate according to claim 4, wherein: The LCP extruded film has a melting point of 250 to 360°C.

6. The method for producing a flexible laminate according to claim 4, wherein: The LCP extruded film has a thickness of 10 μm or more and less than 500 μm.

7. The method for producing a flexible laminate according to claim 4, wherein: The metal foil is one or more selected from the group consisting of copper foil, aluminum foil, stainless steel foil, and alloy foil of copper and aluminum.

8. The method for producing a flexible laminate according to claim 4, wherein: A flexible laminate having a peel strength between the LCP extruded film and the metal foil of 1.0 (N / mm) or more is obtained.

9. A flexible laminate, characterized in that: have: One or more LCP extruded films, the LCP extruded films containing an aromatic polyester liquid crystal polymer, the aromatic polyester liquid crystal polymer having at least a monomer component A and a monomer component B, the monomer component A being at least one selected from the group consisting of p-hydroxybenzoic acid, terephthalic acid, isophthalic acid, 6-naphthalene dicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, 4,4-dihydroxybiphenol, ethylene terephthalate and derivatives thereof, the monomer component B being selected from 6-hydroxy-2-naphthoic acid and derivatives thereof, the solubility of the LCP extruded film in pentafluorophenol at 60° C. being at least 25%, the content ratio of the monomer component A in terms of molar ratio being at least 60 mol % and less than 90 mol %, and the content ratio of the monomer component B in terms of molar ratio being at least 10 mol % and less than 40 mol %; and, One or more metal foils are provided on at least one surface of the LCP extruded film.

10. The flexible laminate according to claim 9, wherein: The LCP extruded film has a melting point of 250 to 360°C.

11. The flexible laminate according to claim 9, wherein: The peel strength between the LCP extruded film and the metal foil is 1.0 (N / mm) or more.

12. The flexible laminate according to claim 9, wherein: The LCP extruded film has a thickness of 10 μm or more and less than 500 μm.

Citation Information

Patent Citations

  • Flexible laminate and method for manufacturing flexible laminate

    JP2016129949A

  • Flexible laminated board and multilayer circuit board

    CN107107555A

  • Wholly aromatic polyester capable of forming anisotropic molten phase

    JP1986157527A

  • Polyester of 6-hydroxy-2-naphthoic acid and para-hydroxy benzoic acid capable of readily undergoing melt processing

    US4161470A

  • Polyester of 6-hydroxy-2-naphthoic acid, para-hydroxy benzoic acid, aromatic diol, and aromatic diacid capable of readily undergoing melt processing