A resource processing method for by-products of sodium chloride and sodium bisulfate
By mixing dried sodium chloride and sodium bisulfate with sodium persulfate for oxidation reaction, organic matter is removed and sodium sulfate is generated under high temperature conditions, the problems of high temperature treatment cost and equipment corrosion in the prior art are solved, and the problem of high temperature treatment in the prior art is realized. Resource treatment of sodium chloride and sodium bisulfate and high-quality sodium sulfate production.
Patent Information
- Application Number
- CN202111298515.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-04
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-11-04
AI Technical Summary
In the prior art, when dealing with by-product salts of sodium chloride and sodium bisulfate, the high-temperature treatment method is costly, complicated to operate and difficult to meet the standards of the chlor-alkali industry, and the use of sulfuric acid is corrosive to the equipment.
By mixing dried sodium chloride and sodium bisulfate with sodium persulfate for oxidation reaction, organic matter is removed and reaction is carried out under high temperature conditions to produce sodium sulfate and hydrochloric acid, which meets the national standard requirements and reduces the risk of equipment corrosion.
The resource treatment of sodium chloride and sodium bisulfate is achieved, which reduces the risk of equipment corrosion, simplifies the process flow, improves economic benefits, and ensures that the product quality meets the national standard Class II qualified products.
Smart Images

Figure CN113998711B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a comprehensive resource treatment method for industrial by-product salt, in particular to a resource treatment method for by-product sodium chloride and sodium bisulfate, and belongs to the technical field of waste resource recovery. Background Art
[0002] The chemical, pharmaceutical, pesticide, printing and dyeing industries produce a large amount of by-product salts, such as chlorides, sulfuric acid, nitrates, etc. As the country's requirements for environmental protection are getting higher and higher and the management of hazardous wastes is getting stricter, companies are facing the pressure of a large amount of waste salt and waste residue that cannot be disposed of and the high cost of disposal. In the pesticide field, for example, the production process of dicamba produces a large amount of by-product sodium bisulfate monohydrate, and the production process of dimethyl tetrachlorophenoxyacetic acid and 2,4-D produces a large amount of by-product sodium chloride.
[0003] Realizing the resource utilization of salt, removing impurities such as organic matter contained in salt and then using it for downstream product preparation is the way for enterprises to survive. The technologies for treating organic matter in by-product salt include high-temperature treatment methods such as pyrolysis, rotary kiln incineration, graded critical carbonization, advanced oxidation, membrane separation technology, etc., or other combined processes. These existing treatment methods, whether using high-temperature treatment methods such as cracking and pyrolysis, or combined processes such as advanced oxidation, all face problems such as large investment, high cost, and complex operation, and most of them do not meet the standards for entering the chlor-alkali industry.
[0004] Patent CN108217696A introduces a resource recovery method for sodium chloride containing organic matter, which is as follows: 1) heating the sodium chloride containing organic matter in a pyrolysis furnace to pyrolyze the organic matter in the sodium chloride to obtain pyrolyzed sodium chloride; 2) adding the pyrolyzed sodium chloride to a stirring synthesis furnace and adding sulfuric acid, heating to obtain sodium sulfate and hydrogen chloride gas. This method uses high-temperature pyrolysis to treat the sodium chloride byproduct, which is expensive, is completed in two steps, is not easy to transfer, and uses sulfuric acid, which is corrosive to the equipment. Summary of the invention
[0005] The purpose of the present invention is to provide a resource treatment method for by-products of sodium chloride and sodium bisulfate. The method mixes by-product sodium chloride and sodium bisulfate, can remove organic matter in the two by-product salts, and can obtain sodium sulfate and hydrochloric acid by-products. The obtained sodium sulfate meets the requirements of Class II qualified products of the national standard (GBT6009-2014), and the resource treatment of the two by-product salts of sodium chloride and sodium bisulfate is realized at the same time.
[0006] The specific technical solutions of the present invention are as follows:
[0007] A method for recycling by-products of sodium chloride and sodium bisulfate, the method comprising the following steps:
[0008] (1) drying and dehydrating the sodium chloride by-product and sodium bisulfate or sodium bisulfate monohydrate by-product;
[0009] (2) mixing the dried sodium chloride byproduct, sodium bisulfate byproduct and sodium persulfate, heating them for oxidation reaction, and removing organic matter from the byproduct;
[0010] (3) subjecting the mixture from step (2) after removing the organic matter to a high temperature reaction to obtain sodium sulfate;
[0011] (4) The tail gas generated in the reaction of step (3) is absorbed by water to obtain a hydrochloric acid solution.
[0012] Further, the sodium chloride by-product and the sodium bisulfate or sodium bisulfate monohydrate by-product are by-products generated from industrial production, and can come from the chemical, pharmaceutical, pesticide, printing and dyeing industries. The sodium chloride by-product has sodium chloride as the main component, and also contains water, organic matter and some other small impurities. The sodium bisulfate or sodium bisulfate monohydrate by-product has sodium bisulfate or sodium bisulfate monohydrate as the main component, and also contains water, organic matter and some other small impurities.
[0013] Furthermore, in step (1), the by-product is first dehydrated. This is because in the subsequent high-temperature reaction stage, the reaction of sodium chloride and sodium bisulfate will release hydrogen chloride gas. If the by-product contains a lot of water, hydrochloric acid will be formed. Under high temperature conditions, hydrochloric acid is easy to corrode the equipment and has extremely high requirements for the equipment. Therefore, removing the water in the by-product first can reduce the requirements of the reaction on the equipment material.
[0014] Furthermore, in step (1), dehydration is performed until the water content is ≤ 0.5 wt%. The sodium bisulfate monohydrate byproduct needs to be dehydrated separately because sodium bisulfate monohydrate has a low melting point and changes in the state of the material during the dehydration process, requiring a special stirring device for dehydration.
[0015] Furthermore, in step (1), the dehydration of sodium chloride and sodium bisulfate can be carried out by conventional drying methods, such as dehydration and drying at room temperature or at a slightly elevated temperature, or dehydration and drying under reduced pressure. The dehydration temperature can be controlled below 100°C or above 100°C.
[0016] Preferably, the dehydration of sodium bisulfate monohydrate is carried out under reduced pressure, the dehydration temperature is 80 to 140°C, and the pressure is -0.05 MPa to -0.08 MPa. The dehydration time varies depending on the water content in the by-product, and the dehydration can be carried out until the water content is ≤ 0.5 wt%. Dehydration at high temperature and reduced pressure can shorten the dehydration time and improve efficiency.
[0017] Furthermore, in step (2), the molar ratio of sodium chloride to sodium bisulfate is 0.91:1 to 0.97:1, and the amount of sodium chloride is controlled to be slightly insufficient. The reason is that although the reaction process of sodium chloride and sodium bisulfate is equimolar, due to uneven mass transfer and thermal decomposition of sodium bisulfate, a small amount of sodium chloride will not react completely, affecting product quality.
[0018] Furthermore, the purpose of adding sodium persulfate is to remove organic matter in the by-product salt. Sodium persulfate has strong oxidizing properties and undergoes redox reaction when in contact with organic matter. The final product of sodium persulfate is sodium sulfate, and no new impurities are introduced. The amount of sodium persulfate added is related to the content of organic matter in the by-product salt. The amount of sodium persulfate added can be controlled to be 4 to 8 times the mass of TOC in the by-product salt. Sodium chloride, sodium persulfate and sodium bisulfate are mixed evenly.
[0019] Furthermore, in step (2), the reaction temperature is 150-200°C, and the reaction time is 30-120 min. Preferably, the reaction temperature is 180-190°C, and the reaction time is 40-70 min.
[0020] Furthermore, in step (3), the high temperature reaction can cause sodium chloride and sodium bisulfate to react to form sodium sulfate and hydrogen chloride. At the same time, the high temperature reaction can also completely remove the remaining organic matter that has not been completely oxidized. The sodium sulfate finally obtained meets the requirements of Class II qualified products of the national standard (GBT6009-2014) and has good quality.
[0021] Furthermore, in step (3), the reaction temperature is 500-800°C, and the reaction time is 60-240 min. Preferably, the reaction temperature is 500-600°C, and the reaction time is 110-200 min.
[0022] Furthermore, in step (3), the hydrogen chloride gas produced by the reaction of sodium chloride and sodium bisulfate is absorbed by water to obtain hydrochloric acid, which can be recycled as a by-product.
[0023] The present invention has the following advantages:
[0024] 1. The present invention adds sodium persulfate to the by-products of sodium chloride and sodium bisulfate, which can remove part of the organic matter in the by-products under relatively low temperature conditions, and then reacts the by-product sodium chloride and sodium bisulfate under high temperature conditions, so that sodium sulfate can be obtained and the organic matter can be further removed, thereby realizing the resource processing of the two salts.
[0025] 2. The present invention dehydrates the by-product sodium chloride and sodium bisulfate monohydrate or sodium bisulfate to prevent the product hydrogen chloride from combining with water to form hydrochloric acid which may corrode the equipment at high temperature, thereby reducing the requirements of the reaction on the equipment material.
[0026] 3. In the present invention, sodium persulfate is added to oxidize organic matter in by-product salt under medium temperature (150-200°C). The reduction product and decomposition product of sodium persulfate are both sodium sulfate, which can oxidize and remove organic matter without introducing new impurities, achieving two goals at one stroke and being easy to operate.
[0027] 4. The present invention allows sodium chloride and sodium bisulfate to react at high temperature to obtain sodium sulfate as a by-product, and simultaneously removes incompletely reacted organic matter by high-temperature cracking, thereby realizing resource processing of the two waste salts, which has the advantages of simple process and high economic benefit.
[0028] 5. The reaction of sodium chloride and sodium bisulfate is a high-temperature (500-800°C) anaerobic reaction, which can decompose organic matter and avoid the production of dioxins. The process is simple and the quality of sodium sulfate is high.
[0029] 6. The hydrogen chloride produced by the reaction of sodium chloride and sodium bisulfate is absorbed by water to obtain hydrochloric acid, which meets the standards of industrial-grade hydrochloric acid and can be sold as a by-product with high economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The present invention discloses a process flow chart of a method for recycling by-products of sodium chloride and sodium bisulfate. DETAILED DESCRIPTION
[0031] In order to better illustrate the technical solution of the present invention, the following examples are given, but the present invention is not limited to the following examples. In order to avoid too many unnecessary details, the well-known structures or functions will not be described in detail in the following examples. Unless otherwise defined, the technical and scientific terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs.
[0032] Unless otherwise specified, the following concentrations are all mass percentages.
[0033] In the following examples, the by-product sodium chloride used was produced by Shandong Weifang Runfeng Chemical Co., Ltd., and was produced by multiple-effect evaporation of wastewater. The sodium bisulfate monohydrate used was produced by Shandong Weifang Runfeng Chemical Co., Ltd., and was a by-product of the production process of dicamba.
[0034] Example 1
[0035] 1. Dry the sodium chloride produced by multi-effect evaporation at 50°C until the moisture content is 0.4% and TOC = 2200 mg / kg;
[0036] 2. Take 403.7g of by-product sodium bisulfate monohydrate and place it in a four-necked flask for decompression dehydration at a temperature of 140°C, a pressure of -0.05MPa, and a time of 56min. After dehydration, the moisture content is 0.43% and TOC is 633mg / kg;
[0037] 3. Take 155.32g of dried sodium chloride, 346.3g of dehydrated sodium bisulfate and 2.24g of sodium persulfate respectively and add them into a four-necked flask, mix them evenly, raise the temperature to 180°C, react for 42 minutes under uniform stirring to remove organic matter in the by-product salt. After the medium-temperature reaction, the sample TOC is 521.34mg / kg;
[0038] 4. The mixed salt after removing the organic matter in step 3 was subjected to high temperature reaction to prepare sodium sulfate at a temperature of 500°C for 155 min. The obtained product had a sodium sulfate content of 97.83%, a sodium chloride content of 0.53%, a sodium bisulfate content of 0.98%, and TOC of 44.2 mg / kg. No characteristic pollutants were detected, meeting the requirements of Class II qualified products of the national standard (GBT6009-2014);
[0039] 5. The tail gas produced in step 4 is absorbed by water to prepare dilute hydrochloric acid.
[0040] Example 2
[0041] 1. Dry the sodium chloride produced by multi-effect evaporation at 50°C until the moisture content is 0.45% and TOC = 1957 mg / kg;
[0042] 2. Take 401.4 g of by-product sodium bisulfate monohydrate and place it in a four-necked flask for decompression dehydration at a temperature of 120°C, a pressure of -0.065 MPa, and a time of 74 min. After dehydration, the moisture content is 0.3% and TOC = 650 mg / kg;
[0043] 3. Take 154.91g of dried sodium chloride, 341.68g of dehydrated sodium bisulfate and 3.15g of sodium persulfate respectively and add them into a four-necked flask, mix them evenly, raise the temperature to 195°C, react for 52 minutes under uniform stirring to remove organic matter in the by-product salt. After the medium-temperature reaction, the sample TOC is 378.66mg / kg;
[0044] 4. The mixed salt after removing the organic matter in step 3 was continued to react at high temperature to prepare sodium sulfate, the temperature was 600°C, the time was 117 minutes, the obtained product had a sodium sulfate content of 98.41%, a sodium chloride content of 0.28%, a sodium bisulfate content of 0.73%, TOC = 26.67 mg / kg, and no characteristic pollutants were detected, meeting the requirements of Class II qualified products of the national standard (GBT6009-2014);
[0045] 5. The tail gas produced in step 4 is absorbed by water to prepare dilute hydrochloric acid.
[0046] Example 3
[0047] 1. Dry the sodium chloride produced by multi-effect evaporation at 50°C until the moisture content is 0.3% and TOC = 2689 mg / kg;
[0048] 2. Take 400.8g of by-product sodium bisulfate monohydrate and place it in a four-necked flask for decompression dehydration at a temperature of 130°C, a pressure of -0.06MPa, and a time of 63min. After dehydration, the moisture content is 0.41% and TOC is 656mg / kg;
[0049] 3. Take 155.51g of dried sodium chloride, 343g of dehydrated sodium bisulfate and 5.2g of sodium persulfate respectively and add them into a four-necked flask, mix them evenly, raise the temperature to 185°C, react for 62 minutes under uniform stirring to remove organic matter in the by-product salt. After the medium-temperature reaction, the sample TOC = 148.25mg / kg;
[0050] 4. The mixed salt after removing the organic matter in step 3 was subjected to high temperature reaction to prepare sodium sulfate at a temperature of 500°C for 195 min. The obtained product had a sodium sulfate content of 98.55%, a sodium chloride content of 0.25%, a sodium bisulfate content of 0.87%, and TOC of 15.23 mg / kg. No characteristic pollutants were detected, meeting the requirements of Class II qualified products of the national standard (GBT6009-2014);
[0051] 5. The tail gas produced in step 4 is absorbed by water to prepare dilute hydrochloric acid.
[0052] Comparative Example
[0053] 1. Dry the sodium chloride produced by multi-effect evaporation at 50°C until the moisture content is 0.3% and TOC = 2689 mg / kg;
[0054] 2. Take 400.6g of by-product sodium bisulfate monohydrate and place it in a four-necked flask for decompression dehydration at a temperature of 125°C, a pressure of -0.065MPa, and a time of 61min. After dehydration, the moisture content is 0.1% and TOC is 679mg / kg.
[0055] 3. Take 151.93g of dried sodium chloride and 338.75g of dehydrated sodium bisulfate, add them into a four-necked flask, mix them evenly, raise the temperature to 183°C, react for 60 minutes under uniform stirring, remove organic matter in the by-product salt, and the sample TOC after medium-temperature reaction is 938.3mg / kg;
[0056] 4. The mixed salt after removing the organic matter in step 3 was continued to react at high temperature to prepare sodium sulfate, the temperature was 500°C, the time was 190 min, and the obtained product had a sodium sulfate content of 97.53%, a sodium chloride content of 0.67%, and a sodium bisulfate content of 0.94%, and TOC = 187.66 mg / kg. The TOC exceeded the standard and could not meet the national standard requirements;
[0057] 5. The tail gas produced in step 4 is absorbed by water to prepare dilute hydrochloric acid.
Claims
1. A method for recycling by-products of sodium chloride and sodium bisulfate, characterized in that The following steps are involved: (1) drying and dehydrating the sodium chloride by-product and sodium bisulfate or sodium bisulfate monohydrate by-product respectively; (2) mixing the dried sodium chloride byproduct, sodium bisulfate byproduct and sodium persulfate, heating them for oxidation reaction, and removing organic matter from the byproduct; (3) subjecting the mixture from step (2) after removing the organic matter to a high temperature reaction to obtain sodium sulfate; (4) absorbing the tail gas formed in the reaction of step (3) with water to obtain a hydrochloric acid solution; In step (1), dehydration is performed to a moisture content of ≤0.5wt%; In step (2), the molar ratio of sodium chloride to sodium bisulfate is 0.91:1 to 0.97:1; In step (2), the reaction temperature of the oxidation reaction is 150-200°C, and in step (3), the reaction temperature is 500-800°C.
2. The resource recovery method according to claim 1, characterized in that: In step (1), the dehydration pressure is -0.05 MPa to -0.08 MPa, and the dehydration temperature is 80 to 140°C.
3. The resource recovery method according to claim 1, characterized in that: In step (2), the amount of sodium persulfate added is 4-8 times the mass of TOC in the mixture.
4. The resource recovery method according to claim 1 or 3, characterized in that: In step (2), the oxidation reaction time is 30 to 120 minutes.
5. The resource recovery method according to claim 1, characterized in that: In step (3), the reaction time is 60 to 240 minutes.
Citation Information
Patent Citations
Recycling method for sodium chloride containing organisms
CN108217696A
Method for producing HCl (hydrogen chloride) from NaCl
CN109384198A
System and method for resourceful treatment of high-salt organic wastewater
CN112225377A
Resource utilization method for treating industrial mixed waste salt by using sulfuric acid
CN113149038A