A sulfidation type hydrodesulfurization catalyst and its preparation method and application

By using solvothermal deposition and roasting processes combined with tetraalkylthiuram disulfide in the preparation of hydrodesulfurization catalysts, the problem of interaction between active metals and carriers is solved, the degree of sulfurization and dispersion of the catalyst is improved, and high efficiency is achieved Hydrodesulfurization activity and simplified process flow.

CN114073970BActive Publication Date: 2024-10-29PETROCHINA CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202010840189.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-19
Publication Date
2024-10-29
Estimated Expiration
2040-08-19

AI Technical Summary

Technical Problem

During the preparation process of existing hydrodesulfurization catalysts, the strong interaction between the active metal and the carrier makes it difficult to completely sulfide the active metal, reducing the activity and utilization of the catalyst. The preparation process is complex and poses environmental and safety risks.

Method used

By heating and refluxing the active metal-containing compound and the vulcanizing agent in a solvent to generate the active metal sulfide, and performing solvothermal deposition on the carrier, combined with the use of tetraalkylthiuram disulfide as the vulcanizing agent during the roasting process, reactivity is avoided. The strong interaction between metal and carrier improves the degree of sulfidation and dispersion of active metals.

Benefits of technology

It achieves high sulfidation and good dispersion of active metals, improves the activity of hydrodesulfurization catalysts, simplifies the preparation process, reduces environmental protection and safety risks, and improves the utilization rate of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114073970B_ABST
    Figure CN114073970B_ABST
Patent Text Reader

Abstract

The present invention provides a sulfidation type hydrodesulfurization catalyst and a preparation method and application thereof. The catalyst comprises a carrier, an active metal and an auxiliary metal. The preparation method comprises the following steps: step 1, adding a compound containing an active metal and a sulfiding agent into a first solvent, heating and refluxing to obtain an active metal sulfide; step 2, dispersing the active metal sulfide on a carrier, then impregnating a compound solution containing an auxiliary metal, and roasting to obtain a sulfidation type hydrodesulfurization catalyst. The catalyst obtained by the method of the present invention can omit the sulfidation process and be directly used for oil hydrodesulfurization, and the method of the present invention can avoid the strong interaction between the active metal and the carrier. In the prepared catalyst, the active metal has a high degree of sulfidation and dispersion, so it has a high removal activity for thiophene sulfur-containing compounds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts and relates to a sulfidation-type hydrodesulfurization catalyst and a preparation method and application thereof. Background Art

[0002] With the increasing development of the national economy, the production, sales and ownership of automobiles in my country have increased rapidly since the beginning of the new century, and the resulting environmental pollution problems have become increasingly serious. To this end, my country has formulated more stringent standards for automotive gasoline, especially strict restrictions on the sulfur content therein. Therefore, the production of ultra-clean gasoline has become an inevitable trend in the gasoline processing industry. Hydrodesulfurization technology is the main means of producing ultra-clean gasoline, and the development of highly active hydrodesulfurization catalysts is the key to achieving an efficient hydrodesulfurization process.

[0003] The hydrodesulfurization catalyst widely used in industry at present uses γ-Al2O3 as carrier, Mo or W as active metal, and Ni or Co as promoter. Usually, in the newly prepared hydrodesulfurization catalyst, Mo, W, Ni and Co exist in the form of oxidation state, and the hydrodesulfurization activity is very low. During use, it is necessary to perform presulfurization to convert it into the sulfurized state to have high hydrodesulfurization activity. The presulfurization process can be divided into in-situ sulfurization and ex-situ sulfurization. Traditional hydrodesulfurization catalysts often use in-situ sulfurization technology, that is, first load the oxidized catalyst into the reactor, and then heat up to introduce hydrogen and sulfurizing agent for sulfurization. There are usually two ways of ex-situ sulfurization. The first is to place the oxidized catalyst on a special presulfurization device for sulfurization, which is no different from in-situ sulfurization; the second is to introduce the sulfurizing agent (such as organic sulfide, elemental sulfur, vegetable oil, sulfone and sulfoxide, etc.) into the gap of the oxidized hydrodesulfurization catalyst by impregnation, melting or sublimation, and then heat up in an inert gas to sulfurize the catalyst. In the actual operation of in-situ sulfidation, the sulfiding agent used is flammable and toxic, which can easily cause environmental pollution. The added sulfiding agent and the water and hydrogen sulfide generated by the reaction can easily cause corrosion to the device and damage the equipment. The process is complicated and time-consuming. Although ex-situ sulfidation can avoid the corrosion of the reaction device during the sulfidation process, its preparation process is complicated. At the same time, the use of a large amount of sulfiding agent will bring certain environmental and safety risks. Most importantly, whether it is ex-situ sulfidation or in-situ sulfidation, the catalyst has a strong interaction between the active metal and the carrier, generating a large number of Al-O-Mo(W) bonds, making it difficult for the active metal to be completely sulfided, reducing the utilization rate of the active metal.

[0004] To address the above problems, the researchers combined the catalyst preparation process with the sulfurization process so that the active components of the catalyst do not exist in an oxidized form during the preparation process, but are converted into a sulfurized form, avoiding strong interactions between the active metal and the carrier and facilitating the full sulfurization of the active metal.

[0005] CN104707629A discloses a method for preparing a hydrodesulfurization catalyst, which uses thiomolybdenum (tungstate) acid salt as a precursor, introduces it into a carrier by an impregnation method, dries and roasts it in an inert atmosphere, then impregnates Ni or Co salt, and roasts it again to obtain a sulfided hydrodesulfurization catalyst. This method effectively avoids the strong interaction between the active metal and the carrier, and improves the sulfidation degree of the active metal. However, due to the weak interaction between the active metal and the carrier, the active metal is easily aggregated during the roasting process, resulting in low utilization of the active metal, which is not conducive to improving the hydrodesulfurization activity of the catalyst.

[0006] In order to improve the dispersion of active metals in hydrodesulfurization catalysts prepared using thiomolybdenum (tungstate) salts as precursors, Alonso et al. (G Alonso, G Berhault, A Aguilar, V Collins, C Ornelas, S Fuentes, R R Chianelli. Characterization and HDS activity of mesoporous MoS2 catalysts prepared by in situ activation of tetraalkylammonium thiomolybdates. Journal of Catalysis, 2002, 208 (2): 359-369) promoted the dispersion of active metals by adding a chelating agent to thiomolybdenum (tungstate) salts, thereby improving the dispersion of active metals. However, the addition of the chelating agent causes incomplete decomposition of thiomolybdenum (tungstate) salts to generate Mo(W)S3, which reduces the utilization rate of active metals and limits the improvement of the hydrodesulfurization activity of the catalyst.

[0007] In summary, there is an urgent need in the art to develop a new sulfurized hydrodesulfurization catalyst, in order to achieve a high degree of sulfurization of the active metal in the hydrodesulfurization catalyst while having a high degree of dispersion of the active metal, thereby improving the activity of the hydrodesulfurization catalyst. Summary of the invention

[0008] The main purpose of the present invention is to provide a sulfided hydrodesulfurization catalyst and a preparation method and application thereof, wherein the active metal in the catalyst has a high degree of sulfidation and good dispersion performance, and thus has a high hydrodesulfurization activity.

[0009] In order to achieve the above object, the present invention provides a method for preparing a sulfidation-type hydrodesulfurization catalyst, the catalyst comprising a carrier, an active metal and an additive metal, and the preparation method comprises the following steps:

[0010] Step 1, adding a compound containing an active metal and a sulfiding agent into a first solvent, heating and refluxing, to obtain an active metal sulfide;

[0011] Step 2: dispersing the active metal sulfide on a carrier, then impregnating a compound solution containing a promoter metal, and calcining to obtain a sulfided hydrodesulfurization catalyst.

[0012] The method for preparing a sulfided hydrodesulfurization catalyst of the present invention comprises the following steps: the active metal-containing compound is molybdenum hexacarbonyl and / or tungsten hexacarbonyl; the sulfiding agent is tetraalkylthiuram disulfide; and / or the active metal-containing compound is calculated based on the active metal, the sulfiding agent is calculated based on sulfur, and the molar ratio of the sulfiding agent to the active metal-containing compound is (1-6):1.

[0013] The method for preparing the sulfidation-type hydrodesulfurization catalyst of the present invention, wherein the tetraalkylthiuram disulfide is one or more of tetramethylthiuram disulfide, tetraethylthiuram disulfide and tetrabutylthiuram disulfide.

[0014] The preparation method of the sulfidation-type hydrodesulfurization catalyst of the present invention, wherein the method of dispersing the active metal sulfide on the carrier is: adding the active metal sulfide and the carrier into a second solvent to carry out a solvent thermal deposition reaction; the carrier is γ-Al2O3; and the mass ratio of the active metal sulfide to the carrier is 0.10-0.25.

[0015] The method for preparing the sulfidation-type hydrodesulfurization catalyst of the present invention, wherein the method for dispersing the active metal sulfide on the carrier is: dissolving the active metal sulfide in a second solvent, then adding the carrier, and performing a solvent thermal deposition reaction.

[0016] The method for preparing the sulfidation-type hydrodesulfurization catalyst of the present invention comprises the following steps: the solvent thermal deposition reaction is carried out in a closed container, the reaction temperature is 160-240° C., and the reaction time is 10-24 hours.

[0017] In the method for preparing the sulfidation-type hydrodesulfurization catalyst of the present invention, the closed container is a high-pressure reactor, and the closed container is in a constant temperature and rotating state.

[0018] The preparation method of the sulfidation type hydrodesulfurization catalyst of the present invention, wherein the auxiliary metal is nickel and / or cobalt; the molar ratio of the auxiliary metal to the active metal is 0.2-0.4; the calcination is carried out in an inert atmosphere, the calcination temperature is 400-500°C, and the calcination time is 4-8h.

[0019] The method for preparing the sulfided hydrodesulfurization catalyst of the present invention comprises the following steps: the heating and reflux in step 1 is carried out under an inert atmosphere; the heating and reflux temperature is 50-100° C., and the heating and reflux time is 1-6 hours.

[0020] In order to achieve the above-mentioned object, the present invention also provides a sulfided hydrodesulfurization catalyst, which includes a carrier, an active metal and an auxiliary metal, wherein the active metal is molybdenum and / or tungsten, the auxiliary metal is nickel and / or cobalt, and the carrier is Al2O3; based on the total mass of the catalyst, the loading amount of the active metal is 15-25%, and the sulfidation degree of the active metal is 85-95%.

[0021] In order to achieve the above object, the present invention further provides the use of the above-mentioned sulfidation-type hydrodesulfurization catalyst in a gasoline desulfurization process.

[0022] Beneficial effects of the present invention:

[0023] (1) The present invention uses an active metal sulfide generated by the reaction of an active metal compound with a sulfiding agent as a precursor and loads it on a carrier to prepare a sulfided hydrodesulfurization catalyst, thereby avoiding the use of an oxygen-containing metal compound as a precursor, reducing the interaction between the active metal and the carrier, and increasing the sulfidation degree of the active metal, which is conducive to the generation of more type II active phases.

[0024] (2) In the catalyst preparation method of the present invention, tetraalkylthiuram disulfide is used as a sulfiding agent, and the synthesized active metal sulfide precursor contains a certain amount of nitrogen, which will interact with the oxygen-containing functional groups on the surface of the carrier during the solvent thermal deposition process to improve the dispersion of the active metal on the carrier. At the same time, in the subsequent calcination process, the tetraalkylthiuram disulfide contained in the active metal sulfide precursor will decompose into residual carbon, inhibit the aggregation of the active metal, further improve the dispersion of the active metal, and expose more active sites of the catalyst, thereby improving the desulfurization activity of the prepared hydrodesulfurization catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a HRTEM photo of the catalyst prepared in Example 2 of the present invention;

[0026] Figure 2 This is the HRTEM photo of the catalyst prepared in Comparative Example 2. DETAILED DESCRIPTION

[0027] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be understood as limiting the scope of the present invention. In the embodiments, all raw reagent materials are commercially available unless otherwise specified, and the experimental methods without specific conditions are conventional methods and conventional conditions well known in the art, or according to the conditions recommended by the instrument manufacturer.

[0028] The present invention provides a method for preparing a sulfidation-type hydrodesulfurization catalyst, wherein the catalyst comprises a carrier, an active metal and an auxiliary metal, and the preparation method comprises the following steps:

[0029] Step 1, adding a compound containing an active metal and a sulfiding agent into a first solvent, heating and refluxing, to obtain an active metal sulfide;

[0030] Step 2: dispersing the active metal sulfide on a carrier, then impregnating a compound solution containing a promoter metal, and calcining to obtain a sulfided hydrodesulfurization catalyst.

[0031] The present invention uses active metal sulfide generated by the reaction of active metal compounds and sulfiding agents as a precursor, and loads the active metal sulfide on a carrier to prepare a sulfided hydrodesulfurization catalyst, which avoids the use of oxygen-containing metal compounds as precursors, reduces the interaction between the active metal and the carrier, increases the sulfidation degree of the active metal, and is conducive to generating more type II active phases.

[0032] In one embodiment, the active metal of the present invention is molybdenum and / or tungsten, and the compound containing the active metal is molybdenum hexacarbonyl and / or tungsten hexacarbonyl. The sulfiding agent is tetraalkylthiuram disulfide. In another embodiment, the sulfiding agent is tetraalkylthiuram disulfide, which is one or more of tetramethylthiuram disulfide, tetraethylthiuram disulfide and tetrabutylthiuram disulfide. The active metal-containing compound is calculated based on the active metal, and the sulfiding agent is calculated based on sulfur, and the molar ratio of the sulfiding agent to the active metal-containing compound is (1-6):1.

[0033] The present invention does not particularly limit the order in which the active metal-containing compound and the sulfiding agent are added to the first solvent, and they can be added simultaneously or sequentially. In one embodiment, step 1 is to dissolve the active metal-containing compound in the first solvent, and then add the sulfiding agent. In one embodiment, the first solvent is an organic solvent, which can increase the solubility of the active metal-containing compound and the sulfiding agent. The present invention does not particularly limit the organic solvent, for example, acetone, chloroform, etc.

[0034] In one embodiment, a compound containing an active metal and a sulfiding agent are added to a first solvent, and heated to reflux under an inert atmosphere, the heating reflux temperature is, for example, 50-100° C., and the heating reflux time is, for example, 1-6 hours. The present invention does not specifically limit the inert atmosphere, for example, it is a nitrogen atmosphere, an argon atmosphere, or a helium atmosphere. Then, after post-treatment operations such as filtration, washing, drying, and calcination, a precipitate, i.e., an active metal sulfide, is obtained. Among them, the calcination is performed, for example, under a vacuum environment.

[0035] Then, the active metal sulfide is dispersed on the support. In one embodiment, the support is Al2O3, and in another embodiment, the support is γ-Al2O3. The mass ratio of the active metal sulfide to the support is 0.10-0.45, and in another embodiment, the mass ratio of the active metal sulfide to the support is 0.10-0.25.

[0036] The method for dispersing the active metal sulfide on the carrier can be: adding the active metal sulfide and the carrier to a second solvent, and performing a solvothermal deposition reaction. In another embodiment, the method for dispersing the active metal sulfide on the carrier is: dissolving the active metal sulfide in a second solvent, then adding the carrier, and performing a solvothermal deposition reaction. In yet another embodiment, the active metal sulfide is added to the second solvent and subjected to ultrasonic treatment to enhance the dispersibility or solubility of the active metal sulfide.

[0037] In one embodiment, the active metal sulfide is Mo(Et2NCS2)4. In another embodiment, the second solvent is an organic solvent, which can increase the solubility of the active metal sulfide. The present invention does not specifically limit the organic solvent, such as anhydrous acetonitrile.

[0038] In one embodiment, the solvent thermal deposition reaction is carried out in a closed container, the reaction temperature is, for example, 160-240° C., and the reaction time is, for example, 10-24 hours. The closed container is, for example, a high-pressure reactor, and another example is a stainless steel reactor lined with polytetrafluoroethylene. In another embodiment, the closed container is in a constant temperature and rotating state, for example, the closed reactor is placed in a rotating constant temperature oven, so that the solvent thermal deposition reaction is carried out dynamically, thereby making the active metal sulfide deposited on the carrier uniform and dispersed.

[0039] After the solvent thermal deposition reaction is completed, operations such as cooling, filtering, washing and drying are performed to obtain a carrier with active metal sulfide deposited thereon.

[0040] Finally, the carrier on which the active metal sulfide is deposited is impregnated with a compound solution containing the promoter metal, and then calcined to obtain a sulfidation-type hydrodesulfurization catalyst.

[0041] In one embodiment, the auxiliary metal is nickel and / or cobalt, the compound containing the auxiliary metal is a soluble salt of nickel and / or cobalt, such as nickel nitrate and / or cobalt nitrate, and the compound solution containing the auxiliary metal is, for example, a solution formed by dissolving nickel nitrate and / or cobalt nitrate in water. In another embodiment, the molar ratio of the auxiliary metal to the active metal is 0.2-0.4. The present invention does not specifically limit the impregnation method, such as equal volume impregnation, excess impregnation, etc.

[0042] After impregnation, post-treatment is performed, such as drying, calcination, etc. to obtain a sulfided hydrodesulfurization catalyst. In one embodiment, drying is performed under a vacuum environment, and calcination is performed under an inert environment, such as an environment formed by one or more of nitrogen, argon and helium. The calcination temperature is, for example, 400-500° C., and the calcination time is, for example, 4-8 hours.

[0043] The catalyst obtained by the above preparation method of the present invention omits the sulfurization process before use and can be directly used for oil hydrodesulfurization. In addition, the above preparation method of the present invention can also avoid the strong interaction between the active metal and the carrier. In the prepared catalyst, the active metal has a high degree of sulfurization and dispersion, so it has a high removal activity for thiophene sulfur-containing compounds.

[0044] Thus, the present invention obtains a sulfided hydrodesulfurization catalyst, which includes a carrier, an active metal and an auxiliary metal, wherein the active metal is molybdenum and / or tungsten, the auxiliary metal is nickel and / or cobalt, and the carrier is Al2O3; based on the total mass of the catalyst, the loading amount of the active metal is 15-25%, and the sulfidation degree of the active metal is 85-95%.

[0045] The sulfurized hydrodesulfurization catalyst obtained by the invention is suitable for the hydrodesulfurization of high-sulfur oil products and can realize ultra-deep desulfurization of gasoline.

[0046] The technical solution of the present invention will be further described below through specific embodiments.

[0047] Example 1

[0048] This embodiment provides a method for preparing a sulfided hydrodesulfurization catalyst, which comprises the following steps:

[0049] Step 1: First, weigh 1.06g of molybdenum hexacarbonyl (Mo(CO)6) and 2.37g of tetraethylthiuram disulfide and dissolve them in 40mL of acetone. Place the solution in a nitrogen atmosphere, heat and reflux at 58°C for 2.5h, cool to room temperature and let stand for 5h, filter and wash with n-pentane, and dry the obtained pink powder in a vacuum oven at 120°C for 8h to obtain metal sulfide Mo(Et2NCS2)4 powder.

[0050] Step 2: weigh 1.89 g of Mo(Et2NCS2)4 and dissolve it in 80 mL of anhydrous acetonitrile, ultrasonicate for 30 min, then add 2.00 g of 20-40 mesh γ-Al2O3 particles to obtain a suspension, transfer the above suspension to a stainless steel reactor lined with polytetrafluoroethylene, place the reactor in a 220°C rotary oven to react for 12 hours, take out after the reaction is completed, cool, filter and wash with ethanol, and dry the obtained sample in a vacuum oven at 80°C for 6 hours to obtain Mo(Et2NCS2)4 / γ-Al2O3.

[0051] Step three, weigh 1.00g Mo(Et2NCS2)4 / γ-Al2O3, impregnate nickel nitrate (Ni(NO3)2·6H2O) according to Ni / (Ni+Mo)=0.3, dry the obtained sample at room temperature for 12h, then place the sample in a vacuum oven at 80°C and dry it for 12h, finally, calcine it at 450°C in a nitrogen atmosphere for 4h to obtain a sulfided hydrodesulfurization catalyst.

[0052] Comparative Example 1

[0053] This comparative example provides a method for preparing a hydrodesulfurization catalyst, which is prepared by the following steps:

[0054] Weigh 0.48 g of ammonium heptamolybdate tetrahydrate ((NH4)6Mo7O 24 ·4H2O) was dissolved in deionized water and impregnated with an equal volume on 2.00g 20-40 mesh γ-Al2O3 particles. The obtained sample was air-dried at room temperature for 12h, and then dried in a vacuum oven at 80℃ for 12h. Then, it was calcined at 450℃ in a nitrogen atmosphere for 4h to obtain MoO3 / γ-Al2O3; 1.00g MoO3 / γ-Al2O3 was weighed and impregnated with nickel nitrate (Ni(NO3)2·6H2O) according to Ni / (Ni+Mo)=0.3. The obtained sample was air-dried at room temperature for 12h, and then dried in a vacuum oven at 80℃ for 12h. Finally, it was calcined at 450℃ in a nitrogen atmosphere for 4h to obtain a reference catalyst. The obtained reference catalyst was dried at 120°C for 2 h under H2 conditions, and then a sulfiding agent (3 wt.% CS2 in n-heptane) was introduced at a sulfiding pressure of 4.0 MPa and a liquid hourly space velocity of 8.0 h -1 , the volume ratio of hydrogen to oil was 300:1, and the temperature was raised to 360°C at a heating rate of 2°C / min and maintained for 6h to obtain a sulfurized reference catalyst.

[0055] The degree of sulfidation of the active metal Mo (W) in the hydrodesulfurization catalyst was determined by X-ray photoelectron spectroscopy (XPS). The degree of sulfidation was obtained by XPS data processing. For the specific processing method, see the literature (TKT Tinh, L. Massin, D. Laurenti, M. Vrinat. A new approach in the evaluation of the support effect for NiMo hydrodesulfurization catalysts. Applied Catalysis A: General, 2011, 407: 29-39.), wherein the XPS analysis was carried out on an ESCA Lab 250 X-ray photoelectron spectrometer (VG Company), the radiation source was AlKα, the resolution was 0.4 eV, and the C1s binding energy (284.5 eV) of the contaminated carbon was used as the internal standard.

[0056] Table 1 Metal content and metal sulfidation degree in catalyst

[0057] sample Mo (wt.%) Ni(wt.%) Mo sulfidation degree (%) Example 1 17.3 4.02 93.1 Comparative Example 1 17.5 4.04 62.5

[0058] Note: Metal content is calculated as sulfide, that is, Mo content is calculated as the mass fraction of MoS2, and Ni content is calculated as the mass fraction of NiS.

[0059] It can be seen from Table 1 that, under the condition of similar metal loading, the sulfidation degree of the active metal Mo in the hydrodesulfurization catalyst prepared by the method of the present invention is 49.0% higher than that of the catalyst prepared by using oxymolybdate.

[0060] Example 2

[0061] This embodiment is basically the same as Embodiment 1, except that "nickel nitrate (Ni(NO3)2·6H2O) is impregnated according to Ni / (Ni+Mo)=0.3" in Embodiment 1 is replaced by "nickel nitrate (Ni(NO3)2·6H2O) is impregnated according to Ni / (Ni+Mo)=0.4".

[0062] Comparative Example 2

[0063] This comparative example provides a method for preparing a sulfurized desulfurization catalyst, which comprises the following steps:

[0064] Weigh 0.71g of ammonium tetrathiomolybdate ((NH4)2MoS4) and dissolve it in ethanolamine, and impregnate an equal volume on 2.00g of 20-40 mesh γ-Al2O3 particles. Dry the obtained sample at room temperature for 12 hours, and then place the sample in a vacuum oven at 80°C for 12 hours to obtain (NH4)2MoS4 / γ-Al2O3; weigh 1.00g of (NH4)2MoS4 / γ-Al2O3, and impregnate nickel nitrate (Ni(NO3)2·6H2O) according to Ni / (Ni+Mo)=0.4. Dry the obtained sample at room temperature for 12 hours, and then place the sample in a vacuum oven at 80°C for 12 hours to obtain a reference catalyst.

[0065] The catalysts in Example 2 and Comparative Example 2 were analyzed using HRTEM. Figure 1 and Figure 2 They are HRTEM photos of the catalysts in Example 2 and Comparative Example 2, respectively. As can be seen from the figure, the difference in active metal precursors will affect the morphology of MoS2 lamellae in the catalyst. Most of the MoS2 lamellae in the catalyst prepared by using Mo sulfide assisted by tetraethylthiuram disulfide as a precursor are short in length and high in dispersion, while the MoS2 lamellae in the catalyst prepared by using (NH4)2MoS4 as a precursor are long and unevenly dispersed. This is because the Mo sulfide assisted by tetraethylthiuram disulfide contains a certain amount of nitrogen, which interacts with the oxygen-containing functional groups on the surface of the carrier during the solvent thermal deposition process, which is beneficial to the dispersion of the active metal precursor on the carrier. At the same time, in the subsequent roasting process, the tetraalkylthiuram disulfide contained in the Mo sulfide will decompose into residual carbon to inhibit the aggregation of active metals, further improving the dispersion of active metals. In comparative example 2, (NH4)2MoS4 is used as a precursor, and its interaction with the carrier is weak, and the active metal is unevenly dispersed on the carrier. High-temperature calcination causes serious agglomeration of the active components, resulting in poor dispersion of MoS2.

[0066] A desulfurization application experiment was carried out on the catalysts prepared in Example 2 and Comparative Example 2.

[0067] Thiophene (800 μg g -1 The reaction conditions were as follows: pressure 2.0 MPa, hydrogen oil volume ratio 300:1, temperature 270°C, volume space velocity 6.0 h -1 After the reaction was stable for 12 hours, samples were taken every 6 hours, and the catalyst evaluation results are shown in Table 2. As can be seen from the table, the desulfurization rates of the catalysts in Example 2 and Comparative Example 2 were 99.1% and 91.2%, respectively. The above results show that the catalyst prepared by the present invention has excellent desulfurization activity.

[0068] Table 2 Hydrodesulfurization performance of the catalysts prepared in Example 2 and Comparative Example 2

[0069] sample Total sulfur in raw materials (μg / g) Total sulfur of product (μg / g) Desulfurization rate (%) Example 2 800 7.2 99.1 Comparative Example 2 800 70.4 91.2

[0070] Finally, it should be noted that the above embodiments are only used to illustrate the implementation process and features of the present invention, rather than to limit the technical methods of the present invention. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in this field should understand that the present invention can still be modified or replaced by equivalents, and any modification or partial replacement that does not depart from the spirit and scope of the present invention should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a sulfidation-type hydrodesulfurization catalyst, characterized in that: The catalyst comprises a carrier, an active metal and an auxiliary metal, and the preparation method comprises the following steps: Step 1, adding a compound containing an active metal and a sulfiding agent into a first solvent, heating and refluxing, to obtain an active metal sulfide; Step 2, dispersing the active metal sulfide on a carrier, then impregnating a compound solution containing a promoter metal, and calcining to obtain a sulfided hydrodesulfurization catalyst; The method for dispersing the active metal sulfide on the carrier is as follows: adding the active metal sulfide and the carrier into a second solvent to perform a solvent thermal deposition reaction; The active metal-containing compound is molybdenum hexacarbonyl and / or tungsten hexacarbonyl; the vulcanizing agent is tetraalkylthiuram disulfide; the active metal-containing compound is calculated as active metal, the vulcanizing agent is calculated as sulfur, and the molar ratio of the vulcanizing agent to the active metal-containing compound is (1-6):1; the carrier is γ-Al2O3; the solvent thermal deposition reaction is carried out in a closed container, the reaction temperature is 160-240 °C, and the reaction time is 10-24 h; and the calcination is carried out under an inert atmosphere.

2. The method for preparing a sulfided hydrodesulfurization catalyst according to claim 1, characterized in that: The tetraalkylthiuram disulfide is one or more of tetramethylthiuram disulfide, tetraethylthiuram disulfide and tetrabutylthiuram disulfide.

3. The method for preparing a sulfided hydrodesulfurization catalyst according to claim 1, characterized in that: The mass ratio of the active metal sulfide to the carrier is 0.10-0.

25.

4. The method for preparing a sulfided hydrodesulfurization catalyst according to claim 1, characterized in that: The method for dispersing the active metal sulfide on the carrier is: dissolving the active metal sulfide in a second solvent, then adding the carrier to perform a solvent thermal deposition reaction.

5. The method for preparing a sulfided hydrodesulfurization catalyst according to claim 1, characterized in that: The sealed container is a high-pressure reactor, and the sealed container is in a constant temperature and rotating state.

6. The method for preparing a sulfided hydrodesulfurization catalyst according to claim 1, characterized in that: The auxiliary metal is nickel and / or cobalt; the molar ratio of the auxiliary metal to the active metal is 0.2-0.4; the calcination temperature is 400-500 °C, and the calcination time is 4-8 h.

7. The method for preparing a sulfided hydrodesulfurization catalyst according to claim 1, characterized in that: The heating reflux in step 1 is carried out under an inert atmosphere; the heating reflux temperature is 50-100 ° C, and the heating reflux time is 1-6 h.

8. The sulfided hydrodesulfurization catalyst obtained by the preparation method according to any one of claims 1 to 7, characterized in that: The catalyst comprises a carrier, an active metal and an auxiliary metal, wherein the active metal is molybdenum and / or tungsten, the auxiliary metal is nickel and / or cobalt, and the carrier is Al2O3; based on the total mass of the catalyst, the loading amount of the active metal is 15-25%, and the sulfidation degree of the active metal is 85-95%.

9. Use of the sulfided hydrodesulfurization catalyst according to claim 8 in a gasoline desulfurization process.

Citation Information

Patent Citations

  • Preparation method of hydrogenating catalyst for load type transition metal sulfide

    CN104707629A

  • Molybdenum sulfide catalyst with graphene-like structure and preparation method of molybdenum sulfide catalyst

    CN106111162A