Method for preparing ultra-thin metal foil
By forming a removable transition layer on the surface of the carrier and performing metal vapor deposition, the problems of low yield and low yield of ultra-thin metal foil preparation are solved, and an efficient and low-cost preparation process is achieved, suitable for large-scale production and environmentally friendly Require.
Patent Information
- Application Number
- CN202111335008.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-11
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-11-11
AI Technical Summary
The existing ultra-thin metal foil preparation technology has the problems of low yield, low yield, high production cost and high difficulty, and it is impossible to achieve large-scale industrial preparation.
Using movable carrier and removable transition layer technology, by forming a transition layer on the surface of the carrier and performing vapor deposition of metal on it, followed by natural separation and shedding, simplifying the process flow and reducing equipment costs, using soluble materials or iodine as transition layer materials To improve preparation efficiency and yield.
It significantly improves the preparation efficiency and yield of ultra-thin metal foil, reduces equipment and material costs, simplifies the process flow, realizes large-scale mass production, and conforms to the characteristics of green chemical industry.
Smart Images

Figure CN114086120B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal materials, and in particular relates to a method for preparing an ultra-thin metal foil. Background Art
[0002] Metal foil is a thin sheet of metal products, such as copper foil, which is usually made of copper and a certain proportion of other metals. The copper content of commercially available copper foil is generally 80 wt% or 90 wt%, corresponding to 80 foil and 90 foil respectively. In the past market environment, its most widely used use is as a decorative material, because it has low surface oxygen characteristics, can be attached to a variety of different substrates, such as metals, insulating materials, etc., and has a wide temperature range of use.
[0003] However, with the development of metal foil, the market has generated a variety of demands. For example, in the field of copper foil, the high-purity electronic-grade copper foil with a copper content of ≥99.7 wt% has been widely used in electronic equipment due to its excellent conductivity and electromagnetic shielding effect. Electronic-grade copper foil is one of the basic materials of the electronics industry. With the rapid development of the electronic information industry, the use of electronic-grade copper foil is increasing. The products are widely used in industrial calculators, communication equipment, QA equipment, lithium-ion copper foil, copper foil sub-batteries, civilian televisions, video recorders, CD players, copiers, telephones, air conditioners, automotive electronic components, game consoles, etc. The demand for electronic-grade copper foil, especially high-performance electronic-grade copper foil, in the domestic and foreign markets is increasing.
[0004] Similarly, copper foil is also an indispensable part of the 5G communication and chip industries that the country is vigorously developing. Compared with conventional electronic-grade copper foil, the copper foil used in chips has higher quality requirements, and it usually needs to reach an ultra-thin and extremely low surface roughness state of about 5 to 8 μm, or even 1 to 3 μm. In addition to the representative copper foil, the demand for various types of ultra-thin metal foils is also increasing. For example, in the fields of catalysts, ultra-thin metal foils also have huge room for development. The traditional calendering and electrolytic methods for the preparation of ultra-thin metal foils can no longer meet the high performance requirements of the above-mentioned fields.
[0005] The preparation of ultra-thin metal foil by vapor deposition can solve the above problems, but there is still the problem of difficulty in stripping the metal foil. Therefore, how to improve the yield rate of ultra-thin metal foil prepared by vapor deposition is one of the core issues of current technology development. Summary of the invention
[0006] In order to solve the problems of low yield and low yield of existing ultra-thin metal foils, high requirements for equipment, high production cost and difficulty, and inability to achieve large-scale industrial preparation and promotion, the present invention provides a method for preparing ultra-thin metal foil.
[0007] The objects of the present invention are:
[0008] 1. Improve the preparation efficiency of ultra-thin metal foil;
[0009] 2. Improve the yield rate of ultra-thin metal foil;
[0010] 3. Reduce process costs and equipment costs;
[0011] 4. Reduce the difficulty of preparation and simplify the preparation process.
[0012] To achieve the above objectives, the present invention adopts the following technical solutions.
[0013] A method for preparing an ultra-thin metal foil,
[0014] The method comprises:
[0015] 1) A movable carrier is provided, at least one side of the carrier is a load surface, and at least one load area is provided in the movable area of the carrier;
[0016] 2) The carrier activity area before the carrier moves to the loading area is the upstream area. When the carrier is in the upstream area, the loading surface of the carrier is covered with transition material to form a transition layer;
[0017] 3) When the carrier moves in the loading area, the metal is vapor-deposited on the surface of the transition layer to form a metal foil;
[0018] 4) The carrier activity area after the carrier moves away from the loading area is the downstream area, and the transition layer is removed in the downstream area to achieve separation of the metal foil and the carrier;
[0019] 5) Collect the separated metal foil.
[0020] The technical solution of the present invention is still based on the existing vapor deposition method to prepare metal foil. The preparation of metal foil is different from conventional metal vapor deposition. The purpose of conventional metal vapor deposition is to stably cover and adhere the metal, while the purpose of vapor deposition used in the preparation of metal foil is to form and peel off. Therefore, after referring to and testing a large number of existing metal foil vapor deposition process methods, the inventor found that it could not effectively improve the peelability of the prepared metal foil, and had no practical reference value for the preparation of ultra-thin metal foil. However, the inventor pioneered the reference to the traditional "lost foam casting" technology and effectively improved the preparation technology of metal foil.
[0021] In the improved metal foil preparation process, a removable transition layer is formed first, and then the metal foil is prepared on the surface of the transition layer, so that the metal foil and the carrier do not contact each other. After the transition layer is removed, the metal foil and the carrier can be naturally separated and detached, and the metal foil can be separated. Compared with the traditional tearing method for demolding, the natural separation of the present invention can more effectively maintain the complete morphology of the metal foil, which has a significant effect on improving the yield rate of ultra-thin metal foil. In addition, the application of dedicated ultra-thin metal foil tearing equipment is reduced, which can reduce equipment costs and simplify the process.
[0022] As a preference,
[0023] Step 1) The carrier is kept flat and performs translational motion in the loading area.
[0024] Since ultra-thin metal foil has strict requirements on the thickness and flatness of the metal foil, controlling the translational movement of the carrier in the load area can effectively maintain the metal foil certificate and ensure high uniformity of the metal foil thickness.
[0025] As a preference,
[0026] Step 2) the transition material is a soluble material;
[0027] The soluble material is soluble in water and / or an organic solvent;
[0028] The transition layer formed by the soluble material is removed by dissolving in the downstream zone of step 4).
[0029] Removing the transition layer by solvent dissolution is simple and efficient. No special equipment is required. The transition layer can be removed by soaking the three-layer structure of the carrier, the transition layer and the metal foil in a solvent or by using a solvent, so that the metal foil falls off naturally. In addition, the transition layer prepared by the above-mentioned soluble material is restored to a soluble material after dissolution, which can be recycled and reused, significantly reducing material costs and improving material utilization, reducing the energy loss required for the peeling equipment to work, and conforming to the characteristics of green chemical industry.
[0030] As a preference,
[0031] The soluble material is PMMA.
[0032] PMMA is a common polymer material that can be effectively dissolved in organic solvents such as toluene. It can also be easily recycled after being dissolved.
[0033] As a preference,
[0034] The soluble material is starch.
[0035] Compared with PMMA, starch is a more common and low-cost organic material, and the starch used in the present invention is water-soluble. Therefore, after the transition layer is prepared using starch, it can be easily removed by water-soluble means.
[0036] As a preference,
[0037] The transition material is iodine.
[0038] As the most unique transition material of the present invention, iodine is utilized for its special physical property of being able to sublime directly. In the traditional metal foil vapor deposition preparation process, after the metal foil is deposited and loaded on the carrier surface, it is quickly cooled to ≤35°C by liquid cooling and / or air cooling. The test shows that iodine can remain relatively stable during the metal deposition loading process in the loading area, and then in the downstream area, it can be removed by heating and sublimation.
[0039] As a preference,
[0040] The iodine is covered on the loading surface of the carrier by vapor deposition to form a transition layer.
[0041] The use of iodine vapor circulation can effectively improve the utilization rate of iodine and energy.
[0042] As a preference,
[0043] The transition layer formed by iodine is removed in the downstream area by thermal sublimation.
[0044] In combination with the above, the transition layer formed by iodine is removed in the downstream area by thermal sublimation to form iodine vapor, and the formed iodine vapor is directly introduced into the upstream area through the gas circulation system and loaded on the loading surface of the carrier again, which can effectively realize the efficient utilization of energy and reduce the solid transportation steps of iodine, thereby greatly improving the efficiency of the overall process.
[0045] In summary, whether it is prepared by soluble materials or iodine, it has the characteristics of efficient preparation of transition layers and efficient removal of transition layers, which has a very significant improvement in the production efficiency of ultra-thin metal foils. In addition, experiments have shown that not all materials are suitable for the vapor deposition preparation of metal foils. Although the temperature is actually highly controllable, the biggest influence on the vapor deposition preparation of metal foils is the adhesion of the transition layer material to the metal foil. Poor adhesion can easily lead to a decrease in the yield rate or even the inability to prepare.
[0046] As a preference,
[0047] Step 3) The metal is deposited on the surface of the transition layer by evaporation to form a metal foil.
[0048] For example, evaporation to prepare ultra-thin electronic-grade high-purity copper foil is the most commonly used method of vapor deposition to prepare copper foil. The process is relatively mature and stable, and can achieve effective temperature control.
[0049] The beneficial effects of the present invention are:
[0050] 1) The preparation efficiency and yield rate of ultra-thin metal foils are significantly improved;
[0051] 2) Can significantly reduce equipment costs, process costs and material costs;
[0052] 3) The difficulty of production and preparation is significantly reduced, which facilitates large-scale batch production and preparation;
[0053] 4) Materials can be recycled and reused, which is in line with the characteristics of green chemistry. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 The process flow chart of the method of the present invention is shown in FIG. DETAILED DESCRIPTION
[0055] The present invention is further described in detail below in conjunction with specific embodiments and the accompanying drawings. A person of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by a person of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.
[0056] In the description of the present invention, it should be understood that the terms "thickness", "upper", "lower", "horizontal", "top", "bottom", "inner", "outer", "circumferential" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In the description of the present invention, "multiple" means at least two, such as two, three, etc., unless otherwise clearly and specifically defined, and "several" means one or more.
[0057] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection, an electrical connection, or communication with each other; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0058] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.
[0059] Unless otherwise specified, the carriers used in the embodiments of the present invention are all metal aluminum strips.
[0060] Unless otherwise specified, the embodiments of the present invention all take the preparation of copper foil as an example, which is a typical representative of the preparation of metal foil.
[0061] Example
[0062] A method for preparing ultra-thin copper foil, the specific process is combined with Figure 1 Provide explanation.
[0063] from Figure 1 It can be seen that in Figure 1 Before the four steps shown, a movable carrier is first set up and its loading surface is determined, and the loading area of Step 2 is set up. Step 1: Upstream means that in the upstream area, the transition layer is loaded on the surface of the loading surface of the carrier, and the transition layer material is gradually deposited on the loading surface to form a transition layer. Then, it enters Step 2: Chemical loading to prepare the deposition loading of copper foil. The embodiment of the present invention mainly adopts the evaporation method for preparation, so copper foil is formed by copper vapor in Step 2, and then enters Step 3: Downstream, and the transition layer is removed in the downstream area. The transition layer is removed to form a separated transition material (Transition material after separation), and then enters the cycle of Step 1. The copper foil is separated and recovered in the Step 4: Separate process, and the carrier re-enters the cycle of Step 1.
[0064] The overall process realizes the effective circulation of materials, the material utilization rate can theoretically reach 100%, and the copper foil is basically intact after separation.
[0065] Specifically, the following specific production and preparation examples are provided.
[0066] Production and Preparation Example 1
[0067] The specific steps are:
[0068] 1) A movable carrier is provided, at least one side of the carrier is a load surface, and at least one load area is provided in the active area of the carrier, and the carrier translates in the load area;
[0069] 2) The carrier activity area before the carrier moves to the loading area is the upstream area. When the carrier is in the upstream area, the loading surface of the carrier is covered with a transition material to form a transition layer. The transition material used in this example is PMMA. A saturated PMMA solution is prepared and a PMMA solution film is formed on the loading surface of the carrier by a coating method, which is dried and solidified to form a PMMA transition layer.
[0070] 3) When the carrier moves in the loading area, the metal copper is vapor-deposited on the surface of the transition layer to form a copper foil, specifically, copper vapor is prepared and then evaporated on the surface of the transition layer;
[0071] 4) The carrier activity area after the carrier moves away from the loading area is the downstream area, and the transition layer is removed in the downstream area to achieve the separation of the copper foil and the carrier. In this example, the three-layer structure of the carrier, the transition layer and the copper foil is passed through a toluene solvent, and PMMA is removed by dissolving the toluene, and then concentrated to a saturated state and reused for the preparation of the transition layer in step 2);
[0072] 5) Collecting the separated copper foil, specifically, the copper foil naturally falls off after the transition layer is taken out, collecting the fallen copper foil and re-entering the carrier into step 2) to achieve cyclic preparation.
[0073] Production and Preparation Example 2
[0074] The specific steps are:
[0075] 1) A movable carrier is provided, at least one side of the carrier is a load surface, and at least one load area is provided in the active area of the carrier, and the carrier translates in the load area;
[0076] 2) The carrier activity area before the carrier moves to the loading area is the upstream area. When the carrier is in the upstream area, the loading surface of the carrier is covered with a transition material to form a transition layer. The transition material used in this example is water-soluble amylose, and a saturated water-soluble amylose solution is prepared to form a starch solution film on the loading surface of the carrier by a coating method, which is dried and solidified to form a starch transition layer;
[0077] 3) When the carrier moves in the loading area, the metal copper is vapor-deposited on the surface of the transition layer to form a copper foil, specifically, copper vapor is prepared and then evaporated on the surface of the transition layer;
[0078] 4) The carrier activity area after the carrier moves away from the loading area is the downstream area, and the transition layer is removed in the downstream area to achieve separation of the copper foil and the carrier. In this example, the three-layer structure of the carrier, the transition layer and the copper foil is passed through boiling water, and the starch transition layer is removed by dissolving the boiling water, and then concentrated to a saturated state and reused for the preparation of the transition layer in step 2);
[0079] 5) Collecting the separated copper foil, specifically, the copper foil naturally falls off after the transition layer is taken out, collecting the fallen copper foil and re-entering the carrier into step 2) to achieve cyclic preparation.
[0080] Production and Preparation Example 3
[0081] The specific steps are:
[0082] 1) A movable carrier is provided, at least one side of the carrier is a load surface, and at least one load area is provided in the active area of the carrier, and the carrier translates in the load area;
[0083] 2) The carrier activity area before the carrier moves to the loading area is the upstream area. When the carrier is in the upstream area, the loading surface of the carrier is covered with a transition material to form a transition layer. The transition material used in this example is elemental iodine. The elemental iodine is heated to sublime to form iodine vapor that is evaporated on the loading surface of the carrier to form an iodine transition layer;
[0084] 3) When the carrier moves in the loading area, the metal copper is vapor-deposited on the surface of the transition layer to form a copper foil. Specifically, copper vapor is prepared and then evaporated on the surface of the transition layer. This process requires increasing the cooling speed. In this example, air cooling combined with water cooling is used to achieve ultra-high-speed cooling, so that the iodine loss rate during the copper evaporation process is less than 1% (the loss rate is determined by the recovery rate of iodine during the actual cycle process);
[0085] 4) The carrier activity area after the carrier moves away from the loading area is the downstream area, and the transition layer is removed in the downstream area to achieve the separation of the copper foil and the carrier. In this example, the three-layer structure of the carrier, the transition layer and the copper foil is heated to 80°C, and the hot steam is collected for the evaporation preparation of the iodine transition layer in step 2);
[0086] 5) Collecting the separated copper foil, specifically, the copper foil naturally falls off after the transition layer is taken out, collecting the fallen copper foil and re-entering the carrier into step 2) to achieve cyclic preparation.
[0087] Production and preparation comparative example
[0088] The specific steps are:
[0089] 1) A movable carrier is provided, at least one side of the carrier is a load surface, and at least one load area is provided in the active area of the carrier, and the carrier translates in the load area;
[0090] 2) When the carrier moves to the loading area, vapor deposition of metallic copper is performed on the loading surface of the carrier to form copper foil, specifically, copper vapor is prepared and then evaporated on the surface of the transition layer;
[0091] 3) peeling off the copper foil prepared on the carrier surface by a peeling method;
[0092] 5) Collect the separated copper foil and put the carrier back into step 2) to achieve cyclic preparation.
[0093] Yield detection test
[0094] The batch preparation test was carried out by the method described in Example 1, Example 2, Example 3 and the comparative example. Ten pieces of copper metal foil with a size of 80×100 cm were prepared respectively. A judgment area of 5×5 cm was divided. If there were bad points (including deformation, obvious folds, scratches, holes, obvious corrosion marks, or obvious dirt that was difficult to remove, etc.) in the judgment area, the area was judged to be damaged. If it was at the boundary of several judgment areas, only one judgment area was counted as damaged.
[0095] The yield rate is calculated based on this. The results are shown in the following table.
[0096]
[0097] It can be clearly seen from the above table that the method of the present invention can effectively improve the yield rate of metal foil. Compared with Example 1, a small amount of pitting corrosion occurs on the surface of part of the copper metal foil in Example 2. Therefore, although Example 2 has a higher demoulding efficiency, the pitting corrosion phenomenon exists, indicating that the water dissolution method has certain defects. The damage of Example 1 is mainly due to the fact that part of the PMMA is solidified on the surface of the metal foil, and removal easily causes mechanical damage to the metal foil and is not easy to remove.
[0098] The damage of the test group of Comparative Example 1 was mainly caused by various mechanical damages produced during the tearing process.
[0099] In contrast, the test group of Example 3, which uses iodine isolation transition, has the highest demoulding efficiency and the highest yield rate, and basically does not cause damage to the metal foil. The three damages are all caused by collision damage during the shedding process.
[0100] In addition, compared with the traditional tearing method, the demoulding method of the present invention can more effectively realize batch demoulding. The traditional tearing method requires special stripping equipment for tearing and demoulding, and each device can demould a limited number of pieces at the same time. The method of the present invention does not require special demoulding equipment, has basically no obvious requirements for the equipment, and can perform large-scale and continuous demoulding, which is more suitable for the existing batch evaporation preparation of metal foil.
[0101] Further, a small-scale production trial run was carried out.
[0102] A four-month large-scale trial production will be carried out from September to December 2020.
[0103] Four production lines of equal scale are set up, namely A, B, C, and D, wherein production line A adopts PMMA transition layer in combination with the method of the present invention for production, which is specifically the same as production and preparation example 1, production line B adopts starch transition layer in combination with the method of the present invention for production, which is specifically the same as production and preparation example 2, production line C adopts iodine transition layer in combination with the method of the present invention for production, which is specifically the same as production and preparation example 3, and production line D adopts traditional method for production and preparation, which is specifically the same as production and preparation comparison example.
[0104] After four months of small-scale production trial operation, the output, yield rate, profit rate, etc. of the products were compared horizontally. Based on the yield rate and profit rate of production line D, the yield rate of production line A increased by about 26.1%, the yield rate of production line B increased by about 22.8%, and the yield rate of production line C increased by about 30.2%. The output of production lines A, B, and C increased by more than 20 times, and the profit rate can reach more than 40 times. The production efficiency and economic benefits have been significantly improved, and it has broad prospects for application and promotion.
Claims
1. A method for preparing an ultra-thin metal foil, characterized in that: The method comprises: 1) A movable carrier is provided, at least one side of the carrier is a load surface, and at least one load area is provided in the movable area of the carrier; 2) The carrier activity area before the carrier moves to the loading area is the upstream area. When the carrier is in the upstream area, the loading surface of the carrier is covered with transition material to form a transition layer; 3) When the carrier moves in the loading area, the metal is vapor-deposited on the surface of the transition layer to form a metal foil; 4) The carrier activity area after the carrier moves away from the loading area is the downstream area, and the transition layer is removed in the downstream area to achieve separation of the metal foil and the carrier; 5) Collect the separated metal foil; Step 2) the transition material is iodine; The transition material is removed in the downstream area, recycled and reused, and then enters the upstream area again for forming the transition layer; The iodine is covered on the loading surface of the carrier by vapor deposition to form a transition layer; The transition layer formed by iodine is removed in the downstream area by thermal sublimation; Step 3) After the metal foil is deposited and loaded on the carrier surface, the temperature is rapidly cooled to ≤35° C. by liquid cooling and / or air cooling.
2. The method for preparing an ultra-thin metal foil according to claim 1, characterized in that: Step 1) The carrier is kept flat and performs translational motion in the loading area.
3. The method for preparing an ultra-thin metal foil according to claim 1, characterized in that: Step 3) The metal is deposited on the surface of the transition layer by evaporation to form a metal foil.
Citation Information
Patent Citations
Method for preparing metal foil by electroless plating
CN101717925A
Process for producing microbeads and microbeads
CN102165317A
Manufacturing method of flexible and transferable electronic device
CN109285946A
Preparation method of flexible Ag / MoS2 / Cu RRAM (Resistive Random Access Memory)
CN110379922A
Method for accurately transferring two-dimensional material and application thereof
CN111874896A
Cited By
Zero-stress electrolytic metal foil preparation method and application of system and method used by zero-stress electrolytic metal foil preparation method
CN115717255A
A method for preparing zero-stress electrolytic metal foil and applications of the system and method used therefor
CN115717255B