Compositions for fuel cell catalysts and fuel cells comprising the same
By replacing the oxygen anions of C12A7 with fluorine or chloride anions and combining them with carbon materials, the problem of high cost of platinum catalysts in fuel cells is solved, and high catalytic activity and chemical stability are achieved, which is suitable for the practical use of fuel cells.
Patent Information
- Application Number
- CN202080050657.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-07-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-07-01
AI Technical Summary
The common use of precious metal platinum in existing fuel cell catalysts leads to high cost and limited reserves, and currently lacks materials that can replace platinum with high catalytic and chemical stability.
By replacing the oxygen anions of C12A7 with fluorine or chlorine anions, the formed halogen replaces C12A7 as a catalyst in the fuel cell and improves its catalytic action by specific heat treatment, combining carbon materials to enhance performance.
A catalyst without using rare elements is achieved, with chemical stability and high catalytic activity, suitable for practical use of fuel cells, and is relatively easy to manufacture, with catalytic performance exceeding that of electronic salting C12A7.
Smart Images

Figure CN114097120B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a composition for a fuel cell catalyst and a fuel cell comprising the composition. More specifically, the present disclosure relates to a composition for a fuel cell catalyst that does not require platinum, a fuel cell comprising the composition and a method for manufacturing the same. Background Art
[0002] In fuel cells such as polymer electrolyte fuel cells (PEFC) and phosphoric acid fuel cells (PAFC), platinum is usually used as a catalyst on both the anode and cathode sides. However, platinum, as a precious metal, is expensive and its reserves are limited, so it is desirable to eliminate or reduce the use of platinum in fuel cell catalysts. Therefore, it is required to develop a catalyst that can replace platinum.
[0003] As platinum alternative catalysts, iron phthalocyanine, nitrogen-containing carbon (carbon alloys), nitrogen-doped carbon, etc. have attracted attention, but at present, there is no catalyst that can catch up with platinum in terms of high catalyticity and chemical stability.
[0004] C12A7 (12CaO·7Al2O3) is an inorganic substance that exists as a natural mineral such as mayenite and is also a component of alumina cement. The crystals of C12A7 form a cage-like skeleton with an inner diameter of about 0.4nm, which is connected by sharing faces. Two of the 12 cages in the unit lattice contain oxygen ions O. 2- Patent Documents 1 and 2 describe that C12A7 is subjected to high temperature treatment to remove the oxygen in the crystal cage. 2- The anion is replaced by an electron e - The crystals obtained by electrification [Ca 24 Al 28 O 64 ] 4+ (4e - ). Patent Document 3 mentions the possibility of using a specific C12A7 compound as an electrode material for a solid electrolyte fuel cell, but to the best of the present inventors' knowledge, there is actually no document indicating that it can be used as a catalyst for a fuel cell to generate electricity.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2005 / 000741
[0008] Patent Document 2: International Publication No. 2007 / 060890
[0009] Patent Document 3: Japanese Patent Application Publication No. 2003-128415 Summary of the invention
[0010] Problems to be solved by the invention
[0011] The present disclosure provides a catalyst for a fuel cell that does not require platinum and a fuel cell including the catalyst.
[0012] Methods for solving problems
[0013] The inventors have found that C12A7 (ideal chemical formula is [Ca 24 Al 28 O 64 ] 4+ (O 2- )2)O 2- Substances in which anions are replaced by fluoride anions (expressed as C12A7:F - ; The ideal chemical formula is [Ca 24 Al 28 O 64 ] 4+ (4F - )) and the substance obtained by substitution with chloride anion (expressed as C12A7:Cl - ) have catalytic ability in the fuel electrode (anode) or air electrode (cathode) of a fuel cell, and can therefore be effectively used as a platinum alternative catalyst. It was further discovered that the catalytic effect can be further improved by subjecting these halogen-substituted C12A7 to heat treatment under specific conditions. The present invention is based on these findings.
[0014] The present disclosure includes the following embodiments. [1]
[0016] A fuel cell catalyst composition comprising C12A7:X having a structure in which oxygen anions of C12A7 are replaced by halogen (X) anions - . [2]
[0018] The fuel cell catalyst composition according to [1], wherein the halogen anion comprises C12A7:F - . [3]
[0020] The fuel cell catalyst composition according to [1] or [2], wherein the halogen anion comprises C12A7:Cl - . [4]
[0022] The fuel cell catalyst composition according to any one of [1] to [3], further comprising - Mixed carbon materials. [5]
[0024] The fuel cell catalyst composition according to [4], wherein the carbon material is carbon black. [6]
[0026] A fuel cell comprising an anode, an anode-side catalyst layer, an electrolyte, a cathode-side catalyst layer and a cathode stacked in sequence, wherein at least one of the anode-side catalyst layer and the cathode-side catalyst layer comprises the fuel cell catalyst composition described in any one of [1] to [5]. [7]
[0028] The fuel cell according to [6], wherein the electrolyte is a proton exchange solid polymer membrane or an aqueous phosphoric acid solution. [8]
[0030] The method for producing a fuel cell catalyst composition according to any one of [1] to [5] comprises: - A step of heat treating at 1000 to 1300° C. for 20 hours or more in a nitrogen atmosphere. [9]
[0032] The method according to [8] further comprises preparing the C12A7:X by calcining a mixture of CaCO3, Al2O3 and CaX2. - process.
[0033] Furthermore, the present disclosure includes the following embodiments. [1]
[0035] A fuel cell catalyst composition comprising C12A7:X having a structure in which oxygen anions of C12A7 are replaced by halogen (X) anions - Inorganic materials. [2]
[0037] The fuel cell catalyst composition according to [1], wherein the halogen anion is a fluoride anion, a chloride anion, or a combination of a fluoride anion and a chloride anion. [3]
[0039] The fuel cell catalyst composition according to [2], wherein the halogen anion is a fluoride anion (F - ) and chloride anion (Cl - ), F - :Cl -The molar ratio is 1:1 to 3:1. [4]
[0041] An inorganic material having a structure in which oxygen anions of C12A7 are replaced by halogen (X) anions: C12A7:X - A substance that is partially electronegated. [5]
[0043] A fuel cell catalyst composition comprising the inorganic material described in [4]. [6]
[0045] The fuel cell catalyst composition according to any one of [1] to [3] or [5], further comprising a carbon material mixed with the inorganic material. [7]
[0047] The fuel cell catalyst composition according to [6], wherein the carbon material is carbon black. [8]
[0049] A fuel cell comprising an anode, an anode-side catalyst layer, an electrolyte, a cathode-side catalyst layer and a cathode stacked in sequence, wherein at least one of the anode-side catalyst layer and the cathode-side catalyst layer comprises the fuel cell catalyst composition described in any one of [1] to [3] or [5] to [7]. [9]
[0051] The method for producing a fuel cell catalyst composition according to any one of [1] to [3] comprises: - A step of heat treating at 1000 to 1300° C. for 20 hours or more in a nitrogen atmosphere.
[10]
[0053] The method for producing the inorganic material described in [4] or the fuel cell catalyst composition described in [5] comprises: - The steps of placing the metal selected from calcium or titanium in the same reactor and sealing the reactor under vacuum; and heating the reactor to a temperature at which the metal is vaporized.
[0054] Effects of the Invention
[0055] The fuel cell catalyst composition of the present embodiment does not require the use of rare elements, can be produced from inexpensive raw materials, functions as a catalyst in both the anode and cathode of a fuel cell, and is chemically stable, and is therefore suitable for practical use in fuel cells.
[0056] The electron salting of C12A7 requires a long calcination process and is technically difficult. In contrast, the halogen-substituted C12A7 and its derivative materials disclosed in the present invention can be manufactured relatively easily. In addition, the fuel cell catalyst composition of the embodiment of the present disclosure can show catalytic activity exceeding that of the electron salted C12A7. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] [ Figure 1 ] Figure 1 Shows the C12A7:F that contains the "as-is" - Power generation when hydrogen is supplied to a fuel cell as a catalyst on the hydrogen electrode side (left) or the oxygen electrode side (right).
[0058] [ Figure 2 ] Figure 2 is shown with the use of as-is C12A7:F - Compared with the case of C12A7:F which was heat treated in a nitrogen atmosphere - Voltage-current curve showing improvement in fuel cell performance when used as a hydrogen-side catalyst.
[0059] [ Figure 3 ] Figure 3 is shown with the use of as-is C12A7:F - Compared with the case of C12A7:F which was heat treated in a nitrogen atmosphere - Power curve for improved fuel cell performance when used as a hydrogen-side catalyst.
[0060] [ Figure 4 ] Figure 4 The X-ray diffraction analysis of C12A7 and C12A7:F shows - result.
[0061] [ Figure 5 ] Figure 5 The analysis of C12A7 and C12A7:F by Raman spectroscopy is shown. - result.
[0062] [ Figure 6 ] Figure 6 (a) shows the - One embodiment of a reactor for subjecting a sample to electron salt treatment. (b) shows the blackening of the sample by electron salt treatment.
[0063] [ Figure 7 ] Figure 7 (a) shows that by C12A7:F -Data showing further improvement in performance as a fuel cell catalyst by electron salt treatment. The upper group shows the current-voltage (IV) curve and the current-power (IP) curve, and the lower group shows the graph of the maximum power.
[0064] (b) shows that such excellent catalytic performance is achieved on C12A7:X - This is unique to the case of electron salt treatment, and even if C12A7 is subjected to the same electron salt treatment, the effect is limited.
[0065] [ Figure 8 ] Figure 8 The electron-salted C12A7:F was analyzed by X-ray diffraction. - and the results of C12A7 subjected to the same electron salt treatment.
[0066] [ Fig. 9 ] Fig. 9 (a) shows C12A7:X containing fluorine (F) ions or chloride (Cl) ions dissolved as halogen (X) ions. - (b) Comparison of the use of F in complex anion substituted C12A7 - :Cl - (c) is a graph comparing the maximum power generation measured in the experiments of (a) and (b). (d) shows the power generation when the ratio of F2 to CaCl2 used in the calcination is changed between 1:2 and 3:1. - and / or Cl - C12A7:X - Lattice constants measured for inorganic materials. DETAILED DESCRIPTION
[0067] In the present disclosure, "to" indicating a numerical range means that the numerical values recorded before and after it are included as the lower limit and upper limit, respectively. In the case of multiple possible numerical ranges recorded separately such as "A to B", "C to D", it can be understood that it can also be a numerical range composed of the lower limit or upper limit of one side and the upper limit or lower limit of the other side (for example, "A to D", "C to B"). For example, a record such as "including" element E can be understood to include both a mode including not only element E but also other elements, and a mode not including other elements other than element E (i.e., consisting of element E).
[0068] In one aspect, the present disclosure provides a fuel cell catalyst composition comprising C12A7:X having a structure in which an oxygen anion of C12A7 is replaced by a halogen anion. - . X represents a halogen atom, X -In the present disclosure, for convenience, C12A7:X - Called C12A7:X - Inorganic materials, which are then mixed with the electron salt C12A7:X described below - Collectively referred to as C12A7:X - Inorganic material. Usually, C12A7 is prepared by calcining a mixture of CaCO3 and Al2O3, but C12A7:X can be prepared by adding CaX2 in a molar ratio to the mixture and calcining it. - (J. Phys. Chem. C 2008, 112, 19061-19068). Alternatively, even if CaX2 in a molar ratio is mixed with pre-generated C12A7 and then calcined, C12A7:X2 can be prepared. - (Journal of the Chemical Society of Japan, 1990, (3), p. 305-311). It is preferred that the number of X atoms per unit cell is 4, which is equivalent to C12A7. - CaX2 is included in the calcination at a theoretical molar ratio of . By these preparation methods, at least 80% or more (and 100% or less) of the oxygen anions of C12A7 can be replaced by halogen anions. - It is usually in the form of powder, usually white.
[0069] X is preferably fluorine or chlorine, and more preferably fluorine. That is, in the composition of this embodiment, C12A7:X - Preferably C12A7:F - 、C12A7:Cl - , or a combination thereof, more preferably C12A7:F - .
[0070] In other words, the halogen anion may be preferably a fluoride anion, a chloride anion, or a combination of a fluoride anion and a chloride anion. - ) and chloride anion (Cl - ) combination, F - :Cl - The molar ratio of F is more preferably 1:1 to 3:1, and particularly preferably 1:1 to 2.5:1. - and Cl - When the catalyst is calcined, the catalytic performance can be improved compared to the case where any one of them is contained alone. - The ratio of different CaX2 (CaF2 and CaCl2) contained in the solution can adjust the ratio of halogen anions in the solid solution.
[0071] In another aspect, the present disclosure provides a C12A7:X- The inorganic material is C12A7:X having a structure in which the oxygen anion of C12A7 is replaced by a halogen (X) anion. - The inorganic material obtained by partial electron saltization, i.e., C12A7:X - Partially electron-salted C12A7:X - The halogen anion may be a fluoride anion, a chloride anion, or a combination of a fluoride anion and a chloride anion. - In inorganic materials that have been partially electronized, although the anions are - Replace but X - Retention, at this point, with the formula [Ca 24 Al 28 O 64 ] 4+ (4e - ) represents the standard C12A7 electron salt phase. It is speculated that in C12A7:X - When the electron salt treatment of C12A7:X - The small amount of O contained in 2- Compared with other non-halogen anions - Prioritized by e - Replace, so X - At least part of it, or perhaps most of it, remains.
[0072] AS C12A7:X - The inorganic material of the partially electronized substance can be calcined in a vacuum in the presence of metal calcium or metal titanium at a temperature that vaporizes the metal to form C12A7:X - More specifically, first, C12A7:X - and metallic calcium are placed in the same reactor, and the reactor is sealed in vacuum (metal titanium can also be used instead of metallic calcium). - The method of disposing the metal in the reactor in a manner that the metal does not contact each other, that is, in a manner that the metal does not mix with each other, is preferred in terms of separating the target product. Figure 6 As shown in (a), C12A7:X is arranged in one tubular space of a reactor having two thick tubular spaces connected by a thin passage. - , place metal calcium in another tubular space, and then seal the entire reactor in a vacuum. In order to improve the reaction efficiency, C12A7:X - The sample preferably has a large surface area and is particularly preferably placed in the reactor in a powder state.
[0073] Next, the reactor is heated to a temperature at which the above metal is vaporized. The temperature at which the metal is vaporized under reduced pressure is known to those skilled in the art or can be appropriately determined by those skilled in the art. For example, in the case of metallic calcium, a heating temperature of 600 to 800°C may be preferred. 680 to 720°C is particularly preferred, and 700°C is most preferred. At temperatures below 1200°C, especially at temperatures below about 800°C, the halogen ions are relatively stable in the C12A7 crystals and are likely to remain, so this is preferred. The portion containing metallic calcium in the reactor is separated from the portion containing C12A7:X - When parts of the sample are sufficiently separated and can be heated at different temperatures, it is preferred to heat the former at a higher temperature such as 680-720°C (or 700°C) and the latter at 780-820°C (or 800°C), because this can suppress the unnecessary solidification of vaporized calcium near the sample.
[0074] In the same reactor, due to heating, C12A7:X - The released oxygen anions are spontaneously used in the oxidation of the vaporized metal, in C12A7:X - The side promotes the transition from anion to e - If the electron salt is fully carried out, the white C12A7:X - During the reaction with the metal vapor, the reaction efficiency can be further improved by shaking the reactor or the like to shuffle the sample while exposing it to the vapor.
[0075] Heating time of the reactor (sintering C12A7:X in vacuum and in the presence of metals) - The time) is typically 24 hours or more, for example, 40 to 240 hours, preferably 72 to 100 hours. The material and shape of the reactor can be appropriately selected by those skilled in the art based on common knowledge, for example Figure 6 A quartz tube with closed ends and a tapered center as shown in (a) is suitable. The quartz tube can be processed into any shape by being fired with a flame of a gas burner, and has heat resistance that allows it to withstand breakage at the typical reaction temperature described above.
[0076] AS C12A7:X - The inorganic material of the partially electron-salified substance can provide an excellent fuel cell catalyst. That is, in one embodiment, a fuel cell catalyst composition containing the inorganic material is provided. In addition, in another embodiment, a method is provided, which is a method for producing the inorganic material or a fuel cell catalyst composition containing the inorganic material, as described above, comprising calcining C12A7:X in a vacuum in the presence of a metal. -The inorganic material is obtained by the process.
[0077] The composition of the above different embodiments preferably further comprises any one of the above C12A7:X - A conductive carbon material mixed with an inorganic material. Examples of the carbon material include carbon black, mesocarbon microbeads, graphite, glassy carbon powder, carbon nanotubes, carbon nanohorns, and carbon nanofibers, but are not limited to these. These carbon materials are usually in a powder state. Carbon black is a particularly preferred carbon material. C12A7:X - The mixing weight ratio of the inorganic material to the carbon material can be, for example, 10:1 to 1:10, preferably 5:1 to 1:3, and more preferably 3:1 to 1:1. Therefore, in one aspect, the method for preparing a fuel cell catalyst composition may include: - The inorganic material is mixed with the carbon material as described in this paragraph.
[0078] On the other hand, the present disclosure provides a fuel cell, which comprises an anode, an anode-side catalyst layer, an electrolyte, a cathode-side catalyst layer and a cathode in a stacked manner. The basic structure of the fuel cell (also referred to as the stacked structure of MEA (Membrane Electrode Assembly: membrane-electrode assembly)) is widely known in the art, but the fuel cell of the present embodiment is characterized in that one or both of the anode-side catalyst layer and the cathode-side catalyst layer contain any of the above-mentioned fuel cell catalyst compositions. The catalyst layer of the other side, that is, the side that does not contain the fuel cell catalyst composition of the above-mentioned embodiment, may contain an existing catalyst such as carbon loaded with platinum. In addition, a combination of the fuel cell catalyst composition of the above-mentioned embodiment and an existing catalyst may also be included in the same catalyst layer.
[0079] The fuel of the fuel cell may be, for example, hydrogen, natural gas or methanol, with hydrogen being particularly preferred.
[0080] The electrolyte in this embodiment can be a proton exchange solid polymer membrane or an aqueous phosphoric acid solution. In the case of the former, it becomes a solid polymer fuel cell, and in the case of the latter, it becomes a phosphoric acid fuel cell. The fuel cell of this embodiment is more preferably a solid polymer fuel cell. A particularly preferred example of a proton exchange solid polymer membrane is a Nafion membrane. As is well known to those skilled in the art, Nafion is a substance having a tetrafluoroethylene skeleton and a perfluorinated side chain with a sulfonic acid group, and is a copolymer of tetrafluoroethylene and perfluoro[2-(fluorosulfonylethoxy)propyl vinyl ether]. The aqueous phosphoric acid electrolyte in a phosphoric acid fuel cell is usually incorporated into the above-mentioned stacked structure in a state of being impregnated in a solid matrix containing silicon carbide, etc.
[0081] Those skilled in the art know materials suitable for the anode and cathode of a fuel cell, respectively. For example, carbon paper or carbon fiber cloth is particularly suitable from the viewpoints of gas permeability, electrical conductivity, chemical stability, and the like.
[0082] In a specific example, the fuel cell involved in this embodiment can be manufactured by a method including the following process: - A fuel cell catalyst composition which is a mixture of an inorganic material and a carbon material (such as carbon black) in powder form is dispersed in a solvent (such as butyl acetate; Nafion solution may also be added) and coated on the surface of a piece of carbon paper. A fuel cell catalyst composition (or carbon loaded with platinum) which is similarly dispersed in a solvent is coated on the surface of another piece of carbon paper. A Nafion membrane is sandwiched between these two catalyst-coated carbon papers to form a stack (in this case, each coated side is facing the Nafion membrane), which are then heat-pressed together.
[0083] In another aspect, the present disclosure provides a method for making a fuel cell catalyst composition. One embodiment of the method comprises: - A process of heat treating at a temperature of 1000 to 1300° C. for more than 20 hours under a nitrogen atmosphere. The temperature of the heat treatment is preferably 1150 to 1250° C., or 1150 to 1200° C., and more preferably 1200±5° C. The time of the heat treatment may be, for example, 20 to 96 hours, preferably 24 to 72 hours, and more preferably 36 to 60 hours. In the environment of the heat treatment, it is preferred that alkali metals or alkaline earth metals are substantially absent. Substantially absent means that they are not intentionally added to the environment.
[0084] The method of this embodiment may further include treating C12A7:X under a nitrogen atmosphere as described above. - Before heat treatment or on C12A7:X - Before electron salting, the C12A7:X - Preparation of C12A7:X - This can be achieved by calcining a mixture of CaCO3, Al2O3 and CaX2. Considering the final C12A7:X - Ca, Al and X in -The theoretical molar ratio of CaCO3, Al2O3 and CaX2 in this process is preferably mixed in a molar ratio of 11:7:1, which means that, for example, when X is F, these materials are mixed in a weight ratio of 7.051g:4.571g:0.500g. The calcination temperature is preferably in the range of 1200°C or more and less than 1415°C, more preferably 1300-1400°C. The calcination time can be, for example, 2 to 96 hours, preferably 24 to 72 hours, and more preferably 36 to 60 hours. Alternatively, C12A7:X can be prepared by mixing pre-generated C12A7 with CaX2 and calcining. - .
[0085] The method of the present embodiment may further include a step of producing an MEA or a fuel cell using the fuel cell catalyst composition after producing the fuel cell catalyst composition as described above.
[0086] Example
[0087] Example 1
[0088] In this example, in order to study the structure of C12A7 in which the oxygen ion is replaced by the fluoride anion, that is, C12A7:F - As a platinum alternative catalyst, a catalyst layer containing C12A7:F - The power generation capacity of the solid polymer fuel cell was measured.
[0089] [C12A7:F - and generation of C12A7]
[0090] Powdered CaCO3, Al2O3 and CaF2 were mixed in a molar ratio of 11:7:1 (7.051 g:4.571 g:0.500 g) and stirred for 30 minutes using a stirrer. The mixture was calcined in air at 1350°C for 48 hours using a high-temperature muffle furnace to prepare C12A7:F2 as a white powder. - . Separately, a compound having a molar ratio of CaCO3 to Al2O3 of 12:7 (5.048 g:3.000 g) was similarly calcined to prepare C12A7. Still further, C12A7:Cl was prepared by using CaCl2 instead of the above-mentioned CaF2. - .
[0091] During the calcination, the temperature in the furnace reached 1350°C 4 hours after the start of the heating, and this temperature was maintained for 48 hours, and then cooled to room temperature by natural cooling. - The sample is said to be "as-is" in the sense that it remains in the state in which it was prepared.
[0092] The as-is sample was further heat treated at 1200°C for 24 hours or 48 hours in a nitrogen atmosphere to prepare a sample. The appearance of the sample heat treated in a nitrogen atmosphere also remained in a white powder state.
[0093] [Manufacturing of MEA and fuel cells]
[0094] A platinum-supported carbon catalyst (obtained from Tanaka Kikinzoku Kogyo) was used on the cathode (oxygen electrode) side, and the above-mentioned C12A7:F was used on the anode (fuel electrode) side. - A mixture of carbon black (weight ratio 1:1) is used as a catalyst layer, a Nafion membrane as a solid polymer electrolyte is sandwiched between the two catalyst layers, and carbon paper is used as the electrode stacked on the outside of the two catalyst layers. The whole is heat-pressed using a small hot press to produce a membrane / electrode assembly (MEA) as the core structure of the fuel cell. The area of the MEA is 23×23mm 2 .
[0095] The MEA was sandwiched between two silicone gaskets, which were further sandwiched between two carbon diaphragms, which were further sandwiched between two acrylic resin cell stack members to produce a fuel cell. In addition, a catalyst layer was also produced by mixing carbon with platinum on the oxygen electrode side and the fuel electrode side with C12A7:F - / fuel cell that replaces carbon black in reverse.
[0096] [Measurement of fuel cell activity]
[0097] At a hydrogen gas flow rate of 3 cc / min, the current was measured while changing the voltage applied to the fuel cell using a source meter, and the power was calculated from the measurement results. Figure 1 Shows the "as-is" C12A7:F - The current-voltage curve and power curve when used as a hydrogen electrode catalyst (left) and as an oxygen electrode catalyst (right). Thus, several mW of power was detected in this experimental system, confirming that C12A7:F - It functions as a catalyst on either the anode or cathode side of a fuel cell.
[0098] On the other hand, in this experimental system, the fuel cell using the conventional C12A7 without fluorine substitution as the catalyst failed to generate power. In this experimental system, the reference fuel cell using platinum catalyst on both electrode sides generated a maximum power of about 25mW. In addition, in a preliminary experiment, the C12A7:F -The fuel cell using the catalyst can show a cell performance that exceeds that of the fuel cell using the electron salt C12A7 as the catalyst under the same conditions. (The data are not shown in the figure. For the comparison with the electron salt C12A7, the results of other experiments conducted independently are recorded in Example 2).
[0099] As mentioned above, the as-is C12A7:F - It can also contribute to power generation as a catalyst, but it was observed that the catalytic activity was further improved by heat treatment of as-is C12A7:F in a nitrogen atmosphere. Figure 2 , Figure 3 The following shows the use of as-is C12A7:F - Compared with the case of C12A7:F - When used as a hydrogen electrode catalyst, the performance of fuel cells is improved. The mechanism of this improvement is not clear, but it is believed that the OH from attached water molecules during heat treatment - Increase (1 / 2O 2- +H2O→2OH - ) (see below) contribute to the possibility of increased catalytic activity and / or by heat treatment. 2- Or OH is replaced by e - , the possibility that its electrons contribute to the catalytic action, etc. Figure 2 , Figure 3 It is also shown that the power generation increases when the hydrogen supply time becomes longer. This result may be related to the increase in battery temperature, the increase in water content, etc. In the battery with the highest power generation, the power generation was about 1 / 4 times that of the reference battery using platinum catalyst for both the cathode and the anode.
[0100] Similarly, for the replacement F - And with Cl - C12A7:Cl - , and also confirmed that its power generation is better than F - The results of another experiment conducted independently are described in Example 3.
[0101] [C12A7:F - Structural analysis of
[0102] For the above C12A7:F in which the oxygen ion of C12A7 is replaced by the fluoride ion - , analyzed by X-ray diffraction and Raman spectroscopy. Figure 4 , Figure 5 In the figure, (a) represents the sample of as-is C12A7, and (b) represents the sample of as-is C12A7:F -(c) represents the C12A7:F obtained by heat treating (b) for 24 hours in a N2 atmosphere. - (d) represents the C12A7:F obtained by heat treating (b) for 48 hours in a N2 atmosphere. - Sample (e) represents C12A7:F - Theoretical simulation.
[0103] Figure 4 The X-ray diffraction patterns of each sample are shown. - The heat treatment in a nitrogen atmosphere causes a change in the arrangement of anions in the crystal cage, and as a result, a change is observed in the relative intensity of the Bragg peak.
[0104] Figure 5 The Raman spectrum is shown. Below 1000 cm -1 No significant differences were found in the spectra of the C12A7 sample at 1130 cm -1 The peaks appearing near 3570 cm correspond to the stretching vibration of O2. -1 The peaks near OH - The stretching vibration of C12A7:F - It can be confirmed that the Raman intensity becomes relatively larger with the heat treatment time in the nitrogen atmosphere.
[0105] Example 2
[0106] In this example, C12A7:F - Electron-salted C12A7:F - Inorganic materials are investigated for their ability to serve as catalysts for polymer electrolyte fuel cells.
[0107] First, the amount of calcium fluoride is calculated so that there are 4 F per C12A7 unit cell. - The solid solution was mixed with C12A7 and sintered at 800℃ for 4 hours to generate C12A7:F - X-ray diffraction and changes in lattice constants confirmed that C12A7:F - Based on the X-ray diffraction pattern, the lattice constant of the C12A7 sample was determined to be 11.980 ± 0.0007 Å, C12A7:F - The lattice constant of the sample was determined to be 11.964 ± 0.0010 angstroms.
[0108] Next, the quartz tube is processed by the flame of a gas burner so that Figure 6As shown in (a), a reactor having two tubular spaces connected by a thin passage is prepared, and C12A7:F is arranged in one of the spaces of the reactor. - The sample powder or C12A7 sample powder is placed with the same weight of metallic calcium in the space of another reactor so that the two are not mixed. The reactor is made into a vacuum state with a vacuum device, and the end of the reactor is directly cut off with a gas burner and vacuum sealed. Then, the reactor is heated in a three-zone electric furnace so that the part containing the above sample powder is 800°C and the part containing metallic calcium is 700°C, and sintered for 72 hours. The result is as follows Figure 6 (b) shows white C12A7:F - The powder and C12A7 powder turned black. This result is consistent with previous reports that the C12A7 sample turns black as the free oxygen ions of C12A7 are replaced by electrons, that is, as the C12A7 sample is oxidized by electrons.
[0109] In the catalyst layer on the fuel electrode side, the mass ratio of any of the above catalyst materials to acetylene black was set to 4:1, and the area of MEA was set to 20×20 mm 2 , except for the above, a fuel cell was produced in substantially the same manner as in Example 1. The hydrogen flow rate in the measurement of the fuel cell activity was set to 7 ml / min.
[0110] like Figure 7 (a) shows that C12A7:F - Compared with the fuel cell catalyst, C12A7:F - C12A7:F obtained by electron salt - The power generation of fuel cells using inorganic materials as catalysts has increased significantly. However, such excellent catalytic activity has not been found in materials obtained by electron salting C12A7 itself ( Figure 7 (b)), but its catalytic activity is lower than that of C12A7:F - (Compare Figure 7 (a) and (b)). In fact, C12A7:F - The inorganic material obtained by the electron salt treatment as described above has almost the same X-ray diffraction peak position but shows different relative peak intensity ratios ( Figure 8 ), suggesting that it is not a complete electron salt but that fluoride ions remain. It is believed that unlike oxygen ions, fluoride ions are difficult to be separated at the electron salt treatment temperature used above, so C12A7:F - During the electron salt treatment of the sample, the non-halogen anions present in small amounts are preferentially replaced by e - , fluoride ions remain.
[0111] Example 3
[0112] In this example, F - and Cl - Complex halogen substitutions in different ratios of solid solution C12A7:X - , their relative abilities as catalysts for solid polymer fuel cells were investigated.
[0113] In the same manner as in Example 1, a mixture of CaCO3, Al2O3 and CaX2 in a ratio of 11:7:1 was calcined to obtain C12A7:X - , but a mixture of CaF2 and CaCl2 was used as CaX2, and the calcination conditions were set to 1200°C and 12 hours. The molar ratio of CaF2 to CaCl2 was varied between 1:1, 2:1, 1:2 and 3:1. The same re-calcination experiment in a nitrogen atmosphere as in Example 1 (re-calcination time was 48 hours) and the same electron salt treatment experiment as in Example 2 (treatment time was 72 hours or 96 hours) were also conducted. In addition to setting the area of the MEA to 20×20 mm 2 Fuel cells containing these samples as catalysts on the fuel electrode side were prepared in substantially the same manner as in Example 1. The hydrogen flow rate in the measurement of the fuel cell activity was set at 7 ml / min.
[0114] With different F - :Cl - C12A7:X - showed similar X-ray diffraction patterns (not shown), but it was confirmed that F - The larger the ratio, the smaller the lattice constant ( Fig. 9 (d)). This is consistent with F - The ionic radius is smaller than that of Cl - In addition, Fig. 9 The results shown in (a) to (c) indicate that by regulating C12A7:X - F - With Cl - The ratio of catalytic performance can be adjusted. The F that shows the highest power generation is selected. - With Cl - The ratio of C12A7:X is 2:1 - , and further calcination or electron salt treatment was performed in a nitrogen atmosphere. As in the previous example, further improvement in power generation was observed. In the calcination in a nitrogen atmosphere, the maximum power generation increased to about 210%, and in the 96-hour electron salt treatment, the maximum power generation increased to about 222% (not shown).
Claims
1. A fuel cell catalyst composition comprising C12A7:X having a structure in which an oxygen anion of C12A7 is replaced by a halogen (X) anion - Inorganic material, the C12A7 is [Ca 24 Al 28 O 64 ] 4+ (O 2- ) 2, the halogen anion is a fluoride anion (F - ) and chloride anion (Cl - ) combination.
2. The fuel cell catalyst composition according to claim 1, wherein F - :Cl - The molar ratio is 1:1 to 3:
1.
3. An inorganic material, which is C12A7:X having a structure in which the oxygen anion of C12A7 is replaced by a halogen (X) anion - A partially electron-salified substance, wherein C12A7 is [Ca 24 Al 28 O 64 ] 4+ (O 2- )2, in the partially electron-salified C12A7:X - In the - Replace X - reserve. 4 . A fuel cell catalyst composition comprising the inorganic material according to claim 3 . 5 . The fuel cell catalyst composition according to claim 1 , further comprising a carbon material mixed with the inorganic material.
6. The fuel cell catalyst composition according to claim 5, wherein The carbon material is carbon black.
7. A fuel cell comprising an anode, an anode-side catalyst layer, an electrolyte, a cathode-side catalyst layer and a cathode stacked in sequence, wherein at least one of the anode-side catalyst layer and the cathode-side catalyst layer comprises the fuel cell catalyst composition according to any one of claims 1 to 2 or 4 to 6.
8. A method for producing a fuel cell catalyst composition according to any one of claims 1 to 2, comprising: - A step of heat treating at 1000 to 1300° C. for 20 hours or more in a nitrogen atmosphere.
9. A method for producing the inorganic material according to claim 3 or the fuel cell catalyst composition according to claim 4, comprising: C12A7:X - The steps of placing the metal selected from calcium or titanium in the same reactor and sealing the reactor under vacuum; and heating the reactor to a temperature at which the metal is vaporized.
10. The manufacturing method according to claim 9, wherein the C12A7:X - The metal is arranged in the reactor in a manner that the metal does not contact with the reactor.
Citation Information
Patent Citations
12cao-7al2o3 compound and method for preparing the same
JP2003128415A
ELECTROCONDUCTIVE 12CaO·7Al2O3 AND COMPOUND OF SAME TYPE, AND METHOD FOR PREPARATION THEREOF
WO2005000741A1
METALLIC ELECTROCONDUCTIVE 12Cao·7Al2O3 COMPOUND AND PROCESS FOR PRODUCING THE SAME
WO2007060890A1
Process for producing conductive mayenite compound
CN101184697A
Process for producing an oxide
CN102171150A