Method for homogenizing oxide layer on fin structure surface

By forming grooves on the shallow isolation layer of the fin structure and performing side oxidation, the problem of inconsistent oxide layer thickness caused by oxidation rates of different crystal planes is solved, improving the uniformity of the oxide layer on the surface of the fin structure and the reliability of the device, and reducing reduce the risk of electrical leakage.

CN114121672BActive Publication Date: 2024-10-29SHANGHAI HUALI INTEGRATED CIRCUIT CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202111390525.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-23
Publication Date
2024-10-29
Estimated Expiration
2041-11-23

AI Technical Summary

Technical Problem

In the prior art, the thickness of the oxide layer on the upper part of the fin structure is inconsistent due to different oxidation rates of different crystal planes, which reduces the reliability of the device and generates leakage.

Method used

By performing chemical mechanical polishing on the shallow isolation layer of the fin structure, grooves are formed, and the grooves are oxidized on the side. The first hard mask layer is used to cover the top surface to offset the difference in oxidation rates of different crystal planes and ensure the oxidation layer. The thickness is consistent on the top surface and corners.

Benefits of technology

The uniformity of the oxide layer on the surface of the fin structure is achieved, improving the reliability of the device and reducing the possibility of leakage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114121672B_ABST
    Figure CN114121672B_ABST
Patent Text Reader

Abstract

The method for homogenizing the surface oxide layer of a fin structure comprises: S1: after the shallow isolation layer generated in the middle of the fin structure is exposed by the first chemical mechanical polishing after the first hard mask layer is exposed, the shallow isolation layer is continuously recessed and removed, and the bottom part of the first hard mask layer is removed to form a groove; S2: the groove is oxidized on the side, and the corner of the top surface-side surface of the fin structure corresponding to the groove is more easily oxidized than other parts. Accordingly, the groove is first oxidized on the side, and since the top surface is covered with the first hard mask layer, the part corresponding to the groove is oxidized, thereby offsetting the defect that the thickness at the corner of the fin is less than the thickness of the top surface due to the different oxidation rate effects at different crystal planes, so that the surface oxide layer finally generated is basically the same (the same on the top surface, corner, and side of the fin structure), the uniformity of the oxide layer is improved, the reliability of the device is improved, and the possibility of leakage is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of semiconductor processing methods, and in particular to a method for homogenizing an oxide layer on the surface of a fin structure. Background Art

[0002] Fin Field-Effect Transistor (FinFET) is a three-dimensional device with a fin structure. Figure 1 As shown, a schematic structural diagram of a fin field effect transistor includes a fin structure (Fin) 01, a channel 02 located between adjacent fin structures 01, an oxide layer 03, a silicon nitride layer 04, and a shallow trench isolation layer (STI) 05 in the channel 02, the oxide layer 03, the silicon nitride layer 04, and the shallow trench isolation layer (STI) 05 are ground to expose the upper part 06 of the fin structure, and the upper part 06 of the fin structure has a top surface 07 and a corner 08 structure.

[0003] In the prior art, since silicon crystals have different oxidation rates at different crystal planes, generally, the oxidation rate is: silicon crystal plane (100)>silicon crystal plane (110)>silicon crystal plane (111), so, usually, the oxide layer formed by the in-situ steam oxidation process (ISSG) on the upper part of the fin structure will have a thickness at the corner of the fin that is less than the thickness of the top surface. The oxide layer is used as an insulating material to isolate the fin structure and the upper layer structure of the fin. However, the inconsistent thickness of the oxide layer will lead to reduced reliability of the device and leakage.

[0004] The problem in the prior art is that the oxide layer generated on the upper part of the fin has inconsistent thickness due to different oxidation rates of different crystal planes, which reduces the reliability of the device and causes leakage. Summary of the invention

[0005] The technical problem to be solved by the present invention is: how to improve the uniformity of the thickness of the oxide layer on the upper part of the fin.

[0006] In order to solve the above technical problems, the present invention provides a method for homogenizing the surface oxide layer of a fin structure, the purpose of which is to make the thickness of the surface oxide layer on the upper part of the fin structure consistent at the top and the corners, thereby improving the reliability of the device and reducing leakage.

[0007] In order to achieve the above object, the present invention provides a method for homogenizing an oxide layer on the surface of a fin structure, comprising:

[0008] S1: After the shallow isolation layer generated in the middle of the fin structure is exposed by the first chemical mechanical polishing, the shallow isolation layer is continuously recessed and removed, and the bottom portion of the first hard mask layer is removed to form a groove;

[0009] S2: The groove is oxidized on the side. The corner of the top surface of the fin structure corresponding to the groove is more easily oxidized than other parts.

[0010] Preferably, before step S1, the method further comprises:

[0011] SP1: forming a pad oxide layer on a silicon substrate, forming a first hard mask layer on the pad oxide layer, patterning the first hard mask layer, and then etching to form a fin structure based on the patterned first hard mask layer;

[0012] SP2: depositing a first oxide layer on the sidewalls of the fin structure and the bottom of the grooves between the fin structures, and then depositing a second hard mask layer on the first oxide layer, the pad oxide layer, and the first hard mask layer;

[0013] SP3: Deposition to form a shallow trench isolation layer.

[0014] Preferably, after step S2, the method further comprises:

[0015] SR1: removing the first hard mask layer;

[0016] SR2: Perform a second chemical mechanical polishing on the shallow trench isolation layer, remove the pad oxide layer covering the fin structure - the first oxide layer, the second hard mask layer, and the shallow trench isolation layer to the same depth, until the fin structure is partially exposed to form a groove, and the shallow trench isolation layer, the first oxide layer, and the second hard mask layer that have not been removed exist at the bottom of the groove;

[0017] SR3: An oxidation process is performed on the exposed fin structure to form a surface oxide layer.

[0018] Preferably, after step SR3, the method further comprises:

[0019] SR4: Nitriding and annealing processes are used to drive nitrogen into the surface oxide layer and keep nitrogen in the surface oxide layer;

[0020] SR5: Polysilicon is deposited and patterned to form the gate structure.

[0021] Preferably, in step S1 , the fin structure is not exposed, the fin structure is covered with a first hard mask layer, and the groove is covered with a pad oxide layer and / or a first oxide layer.

[0022] Preferably, in step SP3, a shallow trench isolation layer is formed by deposition using a fluid chemical vapor deposition method.

[0023] Preferably, in step SR3, an in-situ water vapor oxidation process is adopted to grow and form a surface oxide layer.

[0024] Preferably, the first hard mask layer and the second hard mask layer are silicon nitride.

[0025] Preferably, in step SR4, a decoupled plasma nitridation process is adopted, followed by a post-nitridation annealing process, to implant plasma nitrogen into the surface oxide layer of the fin structure.

[0026] Preferably, two corner edges of the top of the formed fin structure are arc-shaped.

[0027] Compared with the prior art, the present invention provides a method for homogenizing the surface oxide layer of a fin structure, comprising: S1: after the shallow isolation layer generated in the middle of the fin structure is exposed by the first chemical mechanical polishing and the first hard mask layer is exposed, the shallow isolation layer is continuously recessed and removed, and the bottom part of the first hard mask layer is removed to form a groove; S2: the groove is oxidized on the side, and the groove corresponds to the top surface-side corner of the fin structure, which is easier to oxidize than other parts. Accordingly, the technical effect that can be achieved by the present invention is that the groove is first oxidized on the side, and since the top surface is covered with the first hard mask layer, the part corresponding to the groove is oxidized, thereby offsetting the defect that the thickness at the corner of the fin is less than the thickness of the top surface due to the different oxidation rate effects at different crystal planes, so that the surface oxide layer finally generated is basically the same (the same on the top surface, corner, and side of the fin structure), the uniformity of the oxide layer is improved, the reliability of the device is improved, and the possibility of leakage is reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 A fin structure form of the prior art is shown.

[0029] Figures 2A to 2G A schematic diagram showing the structural evolution of some steps of an embodiment of a method for homogenizing an oxide layer on the surface of a fin structure provided by the present invention is shown.

[0030] Figure 3 It is shown that the thickness of the surface oxide layer at the top surface and corner of the fin structure manufactured by the method for homogenizing the surface oxide layer of the fin structure provided by the present invention is consistent, and the shape of the corner is an arc.

[0031] Description of Figure Numbers.

[0032] Existing technology:

[0033] 01 Fin structure

[0034] 02 Channel

[0035] 03 Oxide layer

[0036] 04 Silicon Nitride Layer

[0037] 05 Shallow Trench Isolation Layer

[0038] 06 Upper part of the fin structure

[0039] 07 Top

[0040] 08 Corner;

[0041] The present invention:

[0042] 100 Silicon substrate

[0043] 101 Pad Oxide Layer

[0044] 102 first hard mask layer

[0045] 103 Fin structure

[0046] 104 First Oxide Layer

[0047] 105 second hard mask layer

[0048] 106 Shallow Trench Isolation Layer

[0049] 107 Grooves

[0050] 108 slots

[0051] 109 Surface oxide layer. DETAILED DESCRIPTION

[0052] The specific implementation modes of the present invention are described in detail below with reference to the accompanying drawings.

[0053] See also Figure 2C and 2D , an embodiment of a method for homogenizing an oxide layer on the surface of a fin structure provided by the present invention.

[0054] This method includes: See Figure 2C As shown, step S1: partially remove the shallow trench isolation layer 106 until the first hard mask layer 102 is exposed; continue to recess the shallow trench isolation layer 106, and remove the bottom portion of the first hard mask layer 102 to form a groove 107; refer to Figure 2D As shown, step S2 : performing an oxidation process on the exposed fin structure 103 to form a surface oxide layer 109 .

[0055] See also Figures 2A to 2G As shown, another embodiment of the method for homogenizing the oxide layer on the surface of the fin structure provided by the present invention.

[0056] See also Figure 2A As shown, a pad oxide layer 101 is formed on a silicon substrate 100 , a first hard mask layer 102 is formed on the pad oxide layer 101 , the first hard mask layer 102 is patterned, and then a fin structure 103 (Fin) is formed by etching based on the patterned first hard mask layer 102 .

[0057] See also Figure 2BAs shown, a first oxide layer 104 is deposited on the sidewalls of the fin structure 103 and the bottom of the grooves between the fin structures, and then a second hard mask layer 105 is deposited on the first oxide layer 104 , the pad oxide layer 101 , and the first hard mask layer 102 .

[0058] The first hard mask layer 102 and the second hard mask layer 105 are silicon nitride (SiN).

[0059] See also Figure 2B As shown, a shallow trench isolation layer 106 is deposited. The shallow trench isolation layer 106 may be formed by fluid chemical vapor deposition (FCVD).

[0060] The shallow trench isolation layer 103 is subjected to a first chemical mechanical polishing (CMP).

[0061] See also Figure 2C As shown in FIG. 1 , the shallow trench isolation layer 106 is partially removed until the first hard mask layer 102 is exposed. The shallow trench isolation layer 106 is further recessed and removed, and the bottom portion of the first hard mask layer 102 is removed to form a groove 107. The groove 107 is a concave surface composed of lines perpendicular to the observation plane in three dimensions. Figure 2C The viewing surface shown in .

[0062] Specifically, the fin structure 103 is not exposed, the fin structure 103 is covered with the first hard mask layer 102 , and the groove 107 is covered with the pad oxide layer 101 and / or the first oxide layer 104 .

[0063] Because Figure 2C For coverage shown, see Figure 2D As shown, the groove 107 is oxidized on the side surface, and the groove 107 corresponding to the top surface-side corner of the fin structure is more easily oxidized than other parts.

[0064] See also Figure 2E As shown, the first hard mask layer 102 is removed and the pad oxide layer 101 is exposed.

[0065] See also Figure 2F As shown, the shallow trench isolation layer 106 is subjected to a second chemical mechanical polishing (CMP) to remove the pad oxide layer 101-first oxide layer 104, the second hard mask layer 105, and the shallow trench isolation layer 106 covering the fin structure 103 to the same depth until the fin structure 106 is partially exposed to form a groove 108, and the shallow trench isolation layer 106, the first oxide layer 104, and the second hard mask layer 105 that have not been removed exist at the bottom of the groove.

[0066] See also Figure 2GAs shown, the exposed fin structure 103 is subjected to an oxidation process to form a surface oxide layer 109. Since, in the previous step, the top-side corner of the fin structure 106 corresponding to the groove 107 is more easily oxidized than other parts, and the oxide layer thickness at the corner is thinner than that on the top surface due to the different oxidation rates of different crystal planes of the crystal, the final surface oxide layer 109 has a uniform thickness.

[0067] An in-situ steam generation (ISSG) process is used to grow the surface oxide layer 109 .

[0068] See also Figure 3 As shown, a schematic diagram of the top of a fin structure surface oxide layer 109 formed by using the method for homogenizing the surface oxide layer of a fin structure provided by the present invention is shown. In the figure, the thickness of the surface oxide layer 109 at the top surface and the corners is the same, and the two corner edges of the top of the fin structure finally formed are arc-shaped.

[0069] The nitridation and annealing process is used to drive nitrogen into the surface oxide layer 109 and retain the nitrogen in the surface oxide layer.

[0070] Specifically, a decoupled plasma nitridation process (DPN) is used, followed by a post-nitridation annealing process (PNA), to inject plasma nitrogen into the surface oxide layer of the fin structure.

[0071] Polysilicon is deposited and patterned to form a gate structure.

[0072] The surface oxide layer 109 is used to isolate the gate from the top of the fin structure.

[0073] The above is a specific embodiment of the method for homogenizing the surface oxide layer of the fin structure provided by the present invention. Accordingly, the technical effect that can be achieved by the present invention is that the groove is first oxidized on the side, and because the top surface is covered with a first hard mask layer, the corresponding part of the groove is oxidized, thereby offsetting the defect that the thickness at the corner of the fin is less than the thickness on the top surface due to the different oxidation rate effects at different crystal planes, so that the surface oxide layer finally generated is basically the same (the same on the top surface, corners, and sides of the fin structure), the uniformity of the oxide layer is improved, the reliability of the device is improved, and the possibility of leakage is reduced.

[0074] The above specific embodiments and accompanying drawings are only used to illustrate the technical solutions and technical effects of the present invention, and are not used to limit the present invention. Any person skilled in the art who is familiar with the technology can modify or change the above embodiments within the scope of the claims without violating the technical principles and spirit of the present invention, and all of them belong to the scope of protection of the present invention.

Claims

1. A method for homogenizing an oxide layer on a fin structure surface, It is characterized in that The following steps are involved: SP1: forming a pad oxide layer on a silicon substrate, forming a first hard mask layer on the pad oxide layer, patterning the first hard mask layer, and then etching to form a fin structure based on the patterned first hard mask layer; SP2: depositing a first oxide layer on the sidewalls of the fin structure and the bottom of the grooves between the fin structures, and then depositing a second hard mask layer on the first oxide layer; SP3: Deposition to form a shallow trench isolation layer; S1: performing a first chemical mechanical polishing on the generated shallow trench isolation layer, exposing the first hard mask layer, and then continuing to remove the recess of the shallow trench isolation layer, and removing the shallow trench isolation layer, the second hard mask layer and a portion of the first oxide layer at the bottom of the first hard mask layer to form a groove; S2: The groove is oxidized on the side. The corner of the top surface of the fin structure corresponding to the groove is more susceptible to oxidation than other parts. SR1: removing the first hard mask layer; SR2: Perform a second chemical mechanical polishing on the shallow trench isolation layer to remove the pad oxide layer covering the fin structure - the first oxide layer, the second hard mask layer, and the shallow trench isolation layer to the same depth until the fin structure is partially exposed to form a groove, and the shallow trench isolation layer, the first oxide layer, and the second hard mask layer that have not been removed exist at the bottom of the groove; SR3: An oxidation process is performed on the exposed fin structure to form a surface oxide layer.

2. The method for homogenizing the oxide layer on the surface of the fin structure according to claim 1, It is characterized in that After step SR3, the method further includes: SR4: Nitriding and annealing processes are used to drive nitrogen into the surface oxide layer and keep nitrogen in the surface oxide layer; SR5: Polysilicon is deposited and patterned to form the gate structure.

3. The method for homogenizing the oxide layer on the surface of the fin structure according to claim 1, It is characterized in that In step S1 , the fin structure is not exposed, the fin structure is covered with a first hard mask layer, and the groove is covered with a pad oxide layer and / or a first oxide layer.

4. The method for homogenizing the oxide layer on the surface of the fin structure according to claim 1, It is characterized in that In step SP3, a shallow trench isolation layer is formed by deposition using a fluid chemical vapor deposition method.

5. The method for homogenizing the oxide layer on the surface of the fin structure according to claim 1, It is characterized in that In step SR3, an in-situ water vapor oxidation process is used to grow and form a surface oxide layer.

6. The method for homogenizing the oxide layer on the surface of the fin structure according to claim 1, It is characterized in that The first hard mask layer and the second hard mask layer are silicon nitride.

7. The method for homogenizing the oxide layer on the surface of the fin structure according to claim 2, It is characterized in that In step SR4 , a decoupled plasma nitridation process is adopted, followed by a post-nitridation annealing process, to implant plasma nitrogen into the surface oxide layer of the fin structure.

8. The method for homogenizing an oxide layer on a surface of a fin structure according to claim 1, It is characterized in that The two corner edges of the top of the formed fin structure are in arc shape.

Citation Information

Patent Citations

  • Plasma oxidizing method, plasma oxidizing apparatus, and storage medium

    CN101523576A

  • Method for improving performance of fin field-effect transistor

    CN107293489A

  • Method for manufacturing a semiconductor device

    KR100800918B1