A method for preparing a two-dimensional cuprous phosphide film
By growing cuprous phosphide crystals in an inert atmosphere and preparing cuprous phosphide two-dimensional films on silicon wafer substrates by chemical vapor deposition, the problem of preparing high-quality cuprous phosphide films in the prior art is solved, and the problem of achieving the High-quality and repetitive film preparation improves the performance and application research value of the material.
Patent Information
- Application Number
- CN202111490272.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-12-08
AI Technical Summary
It is difficult to effectively prepare high-quality copper phosphide two-dimensional films in the prior art, which affects its performance and application research.
Sodium hypophosphate and copper foil were used as precursors to grow cuprous phosphide crystals in an inert atmosphere, and a two-dimensional cuprous phosphide film was grown on the silicon wafer substrate of the oxide layer by chemical vapor deposition.
The preparation repeatability and crystallization quality of the two-dimensional cuprous phosphide two-dimensional film are improved, and the film thickness can reach 2-10nm, which significantly improves the performance and application potential of the material.
Smart Images

Figure CN114150291B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of material technology, and in particular relates to a method for preparing a two-dimensional cuprous phosphide thin film. Background Art
[0002] Two-dimensional materials often exhibit properties different from those of bulk materials, which arouses research interest. This patent prepares a two-dimensional cuprous phosphide film, which is helpful for the preparation, performance and application research of cuprous phosphide and other two-dimensional phosphide materials. Summary of the invention
[0003] In view of the deficiencies of the prior art, the present invention provides a method for preparing a two-dimensional cuprous phosphide film.
[0004] The present invention adopts sodium hypophosphite and copper foil as precursors, and grows cuprous phosphide crystals on the surface of the copper foil by heating in an inert atmosphere; then, using the copper foil with cuprous phosphide grown on the surface as a source and a silicon wafer (SiO2 / Si) with an oxide layer grown on the surface as a substrate, a two-dimensional cuprous phosphide film is grown on the surface of the substrate by chemical vapor deposition (CVD).
[0005] Preferably, the cuprous phosphide crystals are grown on the surface of the copper foil, specifically:
[0006] Step (1) sodium hypophosphite is placed in a corundum boat, and then the surface of the corundum boat is covered with 1-5 square centimeters and a copper foil with a thickness of 250-1000 microns;
[0007] Step (2) The corundum boat of step (1) is placed in a corundum tube, evacuated, filled with argon at 1 atmosphere, and then the ends of the corundum tube are sealed;
[0008] Step (3). The corundum tube of step (2) is heated to 280-300°C in a tube furnace at a heating rate of 10°C / min; after the temperature reaches 280-300°C, it is kept warm for 30-60min; then it is naturally cooled to room temperature, the corundum tube is evacuated to remove the residual gas in the tube, and then the copper foil with cuprous phosphide grown on the surface of the product is taken out.
[0009] Preferably, the copper foil with cuprous phosphide grown on the surface is used as the source, the silicon wafer (SiO2 / Si) with an oxide layer grown on the surface is used as the substrate, and a two-dimensional cuprous phosphide film is grown on the surface of the substrate by chemical vapor deposition, specifically:
[0010] Step (1). Place the copper foil with cuprous phosphide grown on the surface into a corundum boat, then transfer it into a corundum tube, and place a silicon wafer with an oxide layer grown on the surface at a 45° angle at the mouth of the corundum tube. Evacuate the tube, fill it with argon gas at 1 atmosphere, and then seal both ends of the corundum tube;
[0011] Step (2). The middle position of the corundum tube in step (1) is heated to 700-850°C in a tube furnace, the temperature of the corundum tube mouth is 550-700°C, and the heating rate is 10°C / min; after the temperature rises to 700-850°C, it is kept warm for 10-30min; then it is naturally cooled to room temperature, and then the product at the corundum tube mouth is taken out to obtain a two-dimensional cuprous phosphide film grown on the surface of the substrate.
[0012] Preferably, the substrate has a size of 2.5-3.5 cm×1.5-2.0 cm.
[0013] Preferably, the diameter of the corundum tube is 1 inch and the vacuum pumping device is equipped with an exhaust gas purification device.
[0014] Preferably, the size of the corundum boat is 0.8 cm×0.6 cm×6 cm.
[0015] The invention has the advantages that: using copper foil with cuprous phosphide grown on the surface as a source and silicon wafer (SiO2 / Si) with an oxide layer grown on the surface as a substrate, a two-dimensional cuprous phosphide film is grown on the surface of the substrate by chemical vapor deposition, the film preparation has good repeatability and high crystal quality. The thickness of the prepared two-dimensional cuprous phosphide film is 2-10nm. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is an atomic force microscope image of a two-dimensional cuprous phosphide film grown on a silicon wafer surface;
[0017] Figure 2 for Figure 1 The film height data corresponding to a total of 1 horizontal line segment is marked. DETAILED DESCRIPTION
[0018] Embodiment 1:
[0019] Step (1) The sodium hypophosphite 6g, placed in a corundum boat, the corundum boat surface covered with 5 square centimeters, a thickness of 1000 microns of copper foil;
[0020] Step (2) The corundum boat of step (1) is placed in a corundum tube, evacuated, filled with argon at 1 atmosphere, and then the ends of the corundum tube are sealed;
[0021] Step (3). The corundum tube of step (2) is heated to 300°C in a tube furnace at a heating rate of 10°C / min; the temperature is raised to 300°C and then kept warm for 60 min; then naturally cooled to room temperature, the corundum tube is evacuated (with exhaust gas purification equipment) to remove residual gas in the tube, and then the product is taken out: a copper foil with cuprous phosphide grown on the surface;
[0022] Step (4). Place the product prepared in step (3) into a new corundum boat, then transfer it into a corundum tube, and place a 2.8cm*1.5cm silicon wafer with an oxide layer grown on the surface at a 45° angle at the mouth of the corundum tube. Evacuate the tube, fill it with argon gas at 1 atmosphere, and then seal both ends of the corundum tube;
[0023] Step (5). The middle position of the corundum tube in step (4) is heated to 700°C in a tube furnace and then kept warm. The mouth of the corundum tube is heated to 550°C at a heating rate of 10°C / min; the holding time is 30min; then it is naturally cooled to room temperature, and then the product at the mouth of the corundum tube is taken out to obtain a two-dimensional cuprous phosphide film grown on the surface of the substrate, such as Figure 1 , Figure 2 As shown, Figure 2 The horizontal axis represents the horizontal position, and the vertical axis represents the vertical height. The horizontal line segment marked as 1 in the left figure has a width of 2 μm, the step is the edge of the film, and the film thickness is about 4 nm.
[0024] Embodiment 2:
[0025] Step (1) The sodium hypophosphite 3g, into a corundum boat, the corundum boat area of 0.8 cm × 0.6 cm × 6 cm, the corundum boat surface covered with 1 square centimeter, a thickness of 250 microns of copper foil;
[0026] Step (2) The corundum boat of step (1) is placed in a corundum tube, evacuated, filled with argon at 1 atmosphere, and then the ends of the corundum tube are sealed;
[0027] Step (3). The corundum tube of step (2) is heated to 290°C by a tube furnace at a heating rate of 10°C / min; the temperature is raised to 290°C and then kept warm for 30 min; then naturally cooled to room temperature, the corundum tube is evacuated (with exhaust gas purification equipment) to remove the residual gas in the tube, and then the product is taken out: a copper foil with cuprous phosphide grown on the surface;
[0028] Step (4). Place the product prepared in step (3) into a new corundum boat, then transfer it into a corundum tube, and place a 2.5cm*1.8cm silicon wafer with an oxide layer grown on the surface at a 45° angle at the mouth of the corundum tube. Evacuate the tube, fill it with argon gas at 1 atmosphere, and then seal both ends of the corundum tube;
[0029] Step (5). The middle position of the corundum tube in step (4) is heated to 750°C by a tube furnace and then kept warm. The mouth of the corundum tube is heated to 600°C for 30 minutes; then naturally cooled to room temperature, and then the product at the mouth of the corundum tube is taken out to obtain a two-dimensional cuprous phosphide film grown on the surface of the substrate;
[0030] Embodiment three:
[0031] Step (1) The sodium hypophosphite 5g, into a corundum boat, the corundum boat surface covered with 3 square centimeters, a thickness of 800 microns of copper foil;
[0032] Step (2) The corundum boat of step (1) is placed in a corundum tube, evacuated, filled with argon at 1 atmosphere, and then the ends of the corundum tube are sealed;
[0033] Step (3). The corundum tube of step (2) is heated to 280°C by a tube furnace at a heating rate of 10°C / min; the temperature is raised to 280°C and then kept warm for 40min; then naturally cooled to room temperature, the corundum tube is evacuated (with exhaust gas purification equipment) to remove the residual gas in the tube, and then the product is taken out: a copper foil with cuprous phosphide grown on the surface;
[0034] Step (4). Place the product prepared in step (3) into a new corundum boat, then transfer it into a corundum tube, and place a 3.5cm*2.0cm silicon wafer with an oxide layer grown on the surface at a 45° angle at the mouth of the corundum tube. Evacuate the tube, fill it with argon gas at 1 atmosphere, and then seal both ends of the corundum tube;
[0035] Step (5). The middle position of the corundum tube in step (4) is heated to 800°C in a tubular furnace and then kept warm. The mouth of the corundum tube is heated to 700°C and kept warm for 30 minutes. Then the tube is naturally cooled to room temperature, and the product is taken out. The product at the mouth of the corundum tube is then taken out to obtain a two-dimensional cuprous phosphide film grown on the surface of the substrate.
Claims
1. A method for preparing a two-dimensional cuprous phosphide film, characterized in that: The method is specifically as follows: sodium hypophosphite and copper foil are used as precursors, and cuprous phosphide crystals are grown on the surface of the copper foil by heating in an inert atmosphere; Then, a copper foil with cuprous phosphide grown on the surface is used as a source, and a silicon wafer with an oxide layer grown on the surface is used as a substrate, and a two-dimensional cuprous phosphide film is grown on the surface of the substrate by chemical vapor deposition, specifically: Step (1) placing a copper foil with cuprous phosphide grown on the surface into a corundum boat, then transferring it into a corundum tube, tilting the corundum tube, and placing a silicon wafer with an oxide layer grown on the surface into the corundum tube mouth; evacuating the tube, filling it with argon at 1 atmosphere, and then sealing both ends of the corundum tube; Step (2). The middle position of the corundum tube in step (1) is heated to 700-850°C in a tube furnace, the temperature of the corundum tube mouth is 550-700°C, and the heating rate is 10°C / min; after the temperature rises to 700-850°C, it is kept warm for 10-30min; then it is naturally cooled to room temperature, and then the product at the corundum tube mouth is taken out to obtain a two-dimensional cuprous phosphide film grown on the surface of the substrate.
2. The method for preparing a two-dimensional cuprous phosphide film according to claim 1, characterized in that: Sodium hypophosphite and copper foil are used as precursors, and cuprous phosphide crystals are grown on the surface of the copper foil by heating in an inert atmosphere; specifically: Step (1) sodium hypophosphite is placed in a corundum boat, and then the surface of the corundum boat is covered with 1-5 square centimeters and a copper foil with a thickness of 250-1000 microns; Step (2) The corundum boat of step (1) is placed in a corundum tube, evacuated, filled with argon at 1 atmosphere, and then the ends of the corundum tube are sealed; Step (3). The corundum tube of step (2) is heated to 280-300°C in a tube furnace at a heating rate of 10°C / min; after the temperature reaches 280-300°C, it is kept warm for 30-60min; then it is naturally cooled to room temperature, the corundum tube is evacuated to remove the residual gas in the tube, and then the copper foil with cuprous phosphide grown on the surface of the product is taken out.
3. The method for preparing a two-dimensional cuprous phosphide film according to claim 1, characterized in that: The size of the substrate is 2.5-3.5 cm×1.5-2.0 cm.
4. The method for preparing a two-dimensional cuprous phosphide film according to claim 2 or 3, characterized in that: The diameter of the corundum tube is 1 inch and the vacuum device is equipped with tail gas purification equipment.