Silver nanoparticles and preparation method thereof

By controlling the reaction conditions in a reducing gas atmosphere, silver nanoparticles are prepared, which solves the problems of poor dispersion of silver nanoparticles in organic solvents and high decomposition temperature of the surface coating layer in traditional methods, and achieves uniformity and uniformity of silver nanoparticles. Improved dispersion and lowered decomposition temperature.

CN114226711BActive Publication Date: 2024-10-29JIANGSU NANOMEIDA OPTOELECTRONICS TECH CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202111673240.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-31
Publication Date
2024-10-29
Estimated Expiration
2041-12-31

AI Technical Summary

Technical Problem

In the traditional preparation method of silver nanoparticles, silver nanoparticles are difficult to disperse in organic solvents, and the decomposition temperature of the surface organic coating layer is high, making the particles difficult to decompose.

Method used

A mixed solution of silver nitrate, dodecanoic acid, polyvinylpyrrolidone and organic solvent is used to heat up the reaction in a reducing gas atmosphere, control the reaction pressure and temperature, and reduce the cross-linking degree of the surface organic coating layer of the silver nanoparticles to achieve their Decomposes at low temperatures.

Benefits of technology

The prepared silver nanoparticles have uniform size, no agglomeration, and good dispersion in organic solvents. The surface organic coating layer can decompose at relatively low temperatures to avoid high-temperature cross-linking problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114226711B_ABST
    Figure CN114226711B_ABST
Patent Text Reader

Abstract

The present invention relates to a silver nanoparticle and a preparation method thereof. The preparation method of the silver nanoparticle comprises the following steps: uniformly mixing silver nitrate, dodecanoic acid, polyvinyl pyrrolidone and an organic solvent to obtain a mixed solution; and heating the mixed solution to 80°C to 100°C in a reducing gas atmosphere, maintaining a reaction pressure of 0.5MPa to 3.0MPa, performing solid-liquid separation after sufficient reaction and retaining solids to obtain silver nanoparticles. Experimental verification shows that the silver nanoparticles prepared by the preparation method of the above silver nanoparticles of the technical solution of the present invention are uniform in size, non-agglomerated, easy to disperse, and have good dispersibility in organic solvents. At the same time, the preparation method of the silver nanoparticles of the technical solution of the present invention introduces a reducing gas as a reducing agent, and the reaction does not need to be carried out at a high temperature of more than 150°C, which reduces the crosslinking degree of the organic coating on the surface of the silver nanoparticles, thereby achieving that the organic coating layer on the surface can be decomposed at a relatively low temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nano material preparation, in particular to silver nano particles and a preparation method thereof. Background Art

[0002] Silver nanoparticles have attracted more and more attention due to their excellent electrical properties and catalytic performance. Due to the high surface energy brought by the nano-size effect, silver nanoparticles tend to agglomerate in solvents and are difficult to disperse. Therefore, the traditional method for preparing silver nanoparticles is to use organic reagents with low reducing properties as solvents (such as ethanol and saturated fatty acids) to control the nucleation rate of the reaction process and reduce the surface energy of the particles.

[0003] However, in the traditional method for preparing silver nanoparticles, even if ethanol is used as a solvent to react with silver carbonate to prepare silver nanoparticles, it is difficult to disperse a sufficient amount of silver nanoparticles in solvents such as cyclohexane. In addition, due to the low reducibility of alcohols and fatty acids, the reaction often needs to be carried out at a high temperature above 150°C, resulting in a high degree of crosslinking of the organic coating on the surface of the silver nanoparticles, which is not easy to decompose. Therefore, when using alcohols and fatty acids as reducing agents, there is also the problem of high temperature decomposition temperature of the organic coating on the surface of the silver nanoparticles. Summary of the invention

[0004] Based on this, it is necessary to provide a silver nanoparticle and a preparation method thereof to improve the dispersibility in an organic solvent and reduce the decomposition temperature of the surface coating layer.

[0005] A method for preparing silver nanoparticles comprises the following steps:

[0006] Mixing silver nitrate, dodecanoic acid, polyvinyl pyrrolidone and an organic solvent uniformly to obtain a mixed solution; and

[0007] The mixed solution is heated to 80° C. to 100° C. in a reducing gas atmosphere, and the reaction pressure is maintained at 0.5 MPa to 3.0 MPa. After sufficient reaction, solid-liquid separation is performed and the solid is retained to obtain silver nanoparticles.

[0008] Experimental verification shows that compared with the traditional method for preparing silver nanoparticles, the silver nanoparticles prepared by the method for preparing silver nanoparticles according to the technical solution of the present invention are uniform in size, non-agglomerated, easily dispersed, and have good dispersibility in organic solvents. At the same time, the method for preparing silver nanoparticles according to the technical solution of the present invention introduces a reducing gas as a reducing agent, and the reaction does not need to be carried out at a high temperature of more than 150° C., which reduces the crosslinking degree of the organic coating on the surface of the silver nanoparticles, thereby achieving the decomposition of the organic coating on the surface at a relatively low temperature.

[0009] In a feasible implementation, the ratio of the silver nitrate, the dodecanoic acid, the polyvinyl pyrrolidone and the organic solvent is (0.005 mol to 0.008 mol): (0.016 mol to 0.032 mol): (0.15 g to 0.4 g): (0.8 mol to 1.2 mol).

[0010] In a feasible implementation, the organic solvent is ethanol.

[0011] In a feasible implementation, the reducing gas is carbon monoxide or hydrogen.

[0012] In a feasible implementation, the reaction pressure is maintained at 1.0 MPa to 2.0 MPa.

[0013] In a feasible implementation, the molecular weight of the polyvinyl pyrrolidone is 8,000-40,000.

[0014] In a feasible implementation, the molecular weight of the polyvinyl pyrrolidone is 12,000.

[0015] In a feasible implementation, the operation of performing solid-liquid separation and retaining the solid after sufficient reaction is as follows: after sufficient reaction, a reaction product is obtained, the reaction product is uniformly mixed with acetone, and then solid-liquid separation is performed and the solid is retained.

[0016] In a feasible implementation, the time for sufficient reaction is 2 h to 3 h.

[0017] The present invention also provides a silver nanoparticle, which is prepared by any of the above-mentioned methods for preparing the silver nanoparticle.

[0018] Experimental verification shows that the silver nanoparticles of the technical solution of the present invention are uniform in size, non-agglomerated, easy to disperse, have good dispersibility in organic solvents, and the organic coating layer on the surface can be decomposed at a relatively low temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is a flow chart of a method for preparing silver nanoparticles according to one embodiment of the present invention;

[0020] Figure 2 Transmission electron microscopy (TEM) image of silver nanoparticles prepared in Example 1;

[0021] Figure 3 Thermogravimetric analysis diagrams of silver nanoparticles prepared in Example 2 and Comparative Example 4. DETAILED DESCRIPTION

[0022] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0024] See also Figure 1 The method for preparing silver nanoparticles according to one embodiment of the present invention comprises the following steps:

[0025] S10, mixing silver nitrate, dodecanoic acid, polyvinyl pyrrolidone and an organic solvent uniformly to obtain a mixed solution.

[0026] In step S10, silver nitrate is used as a precursor to provide a silver source; dodecanoic acid is used as a reducing agent; and polyvinyl pyrrolidone (PVP) is used as a stabilizer to prevent the finally generated silver nanoparticles from agglomerating in an organic solvent.

[0027] In a feasible implementation, the ratio of silver nitrate, dodecanoic acid, polyvinyl pyrrolidone and organic solvent is (0.005 mol to 0.008 mol): (0.016 mol to 0.032 mol): (0.15 g to 0.4 g): (0.8 mol to 1.2 mol).

[0028] In a feasible implementation, the organic solvent is ethanol. Silver nitrate, dodecanoic acid and polyvinyl pyrrolidone have good solubility in ethanol, and ethanol is easily available and has low cost.

[0029] In a feasible implementation, the molecular weight of polyvinyl pyrrolidone is 8000 to 40000. Polyvinyl pyrrolidone with a molecular weight of 8000 to 40000 can better stabilize the silver nanoparticles and is more conducive to the dispersion of the silver nanoparticles in the organic solvent.

[0030] In a feasible implementation, the molecular weight of polyvinyl pyrrolidone is 12000. Polyvinyl pyrrolidone with a molecular weight of 12000 has the best stabilizing effect.

[0031] S20, heating the mixed solution obtained in step S10 to 80°C to 100°C in a reducing gas atmosphere, maintaining the reaction pressure at 0.5MPa to 3.0MPa, performing solid-liquid separation after sufficient reaction and retaining the solid to obtain silver nanoparticles.

[0032] In step S20, the reducing gas acts as a reducing agent together with dodecanoic acid during the reaction process. Under the reaction conditions of a reaction temperature of 80°C to 100°C and a reaction pressure of 0.5MPa to 3.0MPa, silver nitrate undergoes an oxidation-reduction reaction with the reducing gas and dodecanoic acid, and polyvinyl pyrrolidone acts as a stabilizer. After sufficient reaction, product silver nanoparticles are obtained.

[0033] In a feasible implementation, the reducing gas is carbon monoxide or hydrogen. Among them, the reducing gas is preferably carbon monoxide. Of course, the reducing gas in the present invention is not limited thereto, and can also be other gases that can play a reducing role.

[0034] In a feasible implementation, the reaction pressure is maintained at 1.0 MPa to 2.0 MPa. When the reaction pressure is maintained at 1.0 MPa to 2.0 MPa, the reducing gas can fully react with the silver nitrate to ensure that the reaction proceeds fully.

[0035] In a feasible implementation, the operation of performing solid-liquid separation and retaining solid after sufficient reaction is: obtaining a reaction product after sufficient reaction, mixing the reaction product with acetone, and then performing solid-liquid separation and retaining solid. In the above operation, acetone can remove residual ethanol, dodecanoic acid and polyvinyl pyrrolidone. In addition, the step of drying the solid can be further included.

[0036] In a feasible implementation, the time for sufficient reaction is 2 h to 3 h.

[0037] Experimental verification shows that compared with the traditional method for preparing silver nanoparticles, the silver nanoparticles prepared by the method for preparing silver nanoparticles according to the technical solution of the present invention are uniform in size, non-agglomerated, easily dispersed, and have good dispersibility in organic solvents. At the same time, the method for preparing silver nanoparticles according to the technical solution of the present invention introduces a reducing gas as a reducing agent, and the reaction does not need to be carried out at a high temperature of more than 150° C., which reduces the crosslinking degree of the organic coating on the surface of the silver nanoparticles, thereby achieving the decomposition of the organic coating on the surface at a relatively low temperature.

[0038] The silver nanoparticles according to one embodiment of the present invention are prepared by any of the above-mentioned methods for preparing silver nanoparticles.

[0039] Experimental verification shows that the silver nanoparticles of the technical solution of the present invention are uniform in size, non-agglomerated, easy to disperse, have good dispersibility in organic solvents, and the organic coating layer on the surface can be decomposed at a relatively low temperature.

[0040] With reference to the above implementation contents, in order to make the technical solution of the present application more specific, clear and easy to understand, the technical solution of the present application is now exemplified. However, it should be noted that the contents to be protected by the present application are not limited to the following Examples 1 to 4.

[0041] Example 1

[0042] 0.8 mol of ethanol, 0.02 mol of dodecanoic acid, 0.0066 mol of silver nitrate and 0.21 g of PVP were added into a reaction container and mixed in the reaction container to obtain a mixed solution;

[0043] The reaction container containing the mixed solution is placed in a pressure-resistant reactor, and the air in the reactor is exhausted with carbon monoxide; then a certain amount of carbon monoxide is charged into the reactor so that the pressure in the reactor reaches 1.0 MPa; the temperature is slowly raised to 90° C. while stirring, and the reaction is carried out at this temperature for 2 hours; then the pressure in the reactor is released, and the reaction is carried out by filtering with acetone and drying to obtain the silver nanoparticles of Example 1.

[0044] The silver nanoparticles prepared in Example 1 were characterized by transmission electron microscopy, and the Figure 1 .Depend on Figure 1 It can be seen that the silver nanoparticles prepared in Example 1 are uniform in size, with an average size of 4.41 nm, and are evenly distributed without obvious agglomeration.

[0045] Example 2

[0046] 0.8 mol of ethanol, 0.02 mol of dodecanoic acid, 0.0066 mol of silver nitrate and 0.21 g of PVP were added into a reaction container and mixed in the reaction container to obtain a mixed solution;

[0047] The reaction container containing the mixed solution is placed in a pressure-resistant reactor, and the air in the reactor is exhausted with carbon monoxide; then a certain amount of carbon monoxide is filled into the reactor so that the pressure in the reactor reaches 0.5 MPa; the temperature is slowly raised to 90° C. while stirring, and the reaction is carried out at this temperature for 2 hours; then the pressure in the reactor is released, and the reaction is carried out by filtering with acetone and drying to obtain the silver nanoparticles of Example 2.

[0048] Example 3

[0049] 0.8 mol of ethanol, 0.02 mol of dodecanoic acid, 0.0066 mol of silver nitrate and 0.21 g of PVP were added into a reaction container and mixed in the reaction container to obtain a mixed solution;

[0050] The reaction container containing the mixed solution is placed in a pressure-resistant reactor, and the air in the reactor is exhausted with carbon monoxide; then a certain amount of carbon monoxide is filled into the reactor so that the pressure in the reactor reaches 1.5 MPa; the temperature is slowly raised to 90° C. while stirring, and the reaction is carried out at this temperature for 2 hours; then the pressure in the reactor is released, and the reaction is carried out by filtering with acetone and drying to obtain the silver nanoparticles of Example 3.

[0051] Example 4

[0052] 0.8 mol of ethanol, 0.02 mol of dodecanoic acid, 0.0066 mol of silver nitrate and 0.21 g of PVP were added into a reaction container and mixed in the reaction container to obtain a mixed solution;

[0053] The reaction container containing the mixed solution is placed in a pressure-resistant reactor, and the air in the reactor is exhausted with carbon monoxide; then a certain amount of carbon monoxide is filled into the reactor so that the pressure in the reactor reaches 2.0 MPa; the temperature is slowly raised to 90° C. while stirring, and the reaction is carried out at this temperature for 2 hours; then the pressure in the reactor is released, and the reaction is carried out by filtering with acetone and drying to obtain the silver nanoparticles of Example 4.

[0054] Comparative Example 1

[0055] This comparative example is a comparative example of Example 1, and provides a silver nanoparticle and a preparation method thereof, which is different from the preparation method of Example 1 only in that the pressure in the kettle reaches 0.1 MPa.

[0056] Comparative Example 2

[0057] 0.8 mol of ethanol, 0.02 mol of dodecanoic acid, 0.0066 mol of silver nitrate and 0.21 g of PVP were added to a reaction container, slowly heated to 160° C. while stirring, and reacted at this temperature for 2 hours; finally, acetone was used for filtration, and the silver nanoparticles of Comparative Example 2 were obtained after drying.

[0058] Performance Test:

[0059] (1) The silver nanoparticles prepared in Examples 1 to 4, Comparative Examples 1 and 2 were added to cyclohexane at a ratio of 15 wt %, and 10 ml was placed in a test tube, stirred for 30 minutes, and then allowed to stand for 5 minutes. Then, 1 ml of the upper clear liquid was taken to determine the concentration of the silver nanoparticles therein by the dry weight method. The results are shown in Table 1.

[0060] Table 1 Dispersibility data of silver nanoparticles obtained in Examples 1 to 4, Comparative Examples 1 and 2

[0061]

[0062] The following conclusions can be drawn from Table 1: Compared with the preparation methods of the silver nanoparticles of Comparative Examples 1 and 2, in the preparation methods of the silver nanoparticles of Examples 1 to 4 of the present invention, when the reducing gas pressure in the reactor is above 0.5 MPa, the concentration of the silver nanoparticles in the supernatant of cyclohexane is above 10 wt %; by comparing the data of the silver nanoparticles of Examples 1 to 4, it can be seen that as the reducing gas pressure increases, the concentration of the silver nanoparticles in the supernatant also increases. The above shows that the introduction of reducing gas and the addition of PVP as a stabilizer can effectively improve the dispersibility of the silver nanoparticles in cyclohexane.

[0063] (2) The thermal decomposition behavior of the organic coating layer on the surface of the silver nanoparticles of Example 1 and Comparative Example 2 was analyzed by thermogravimetry. The results are as follows Figure 3 As shown. Figure 3 It can be seen that the thermal decomposition temperature of the surface organic coating layer of the silver nanoparticles obtained by Example 1 is reduced by 20° C. compared with that of Comparative Example 2, indicating that the introduction of reducing gas in the preparation method of the silver nanoparticles in Example 1 can reduce the decomposition temperature of the surface coating layer.

[0064] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0065] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing silver nanoparticles, characterized in that: The steps include: Mixing silver nitrate, dodecanoic acid, polyvinyl pyrrolidone and an organic solvent uniformly to obtain a mixed solution; and The mixed solution is heated to 80° C. to 100° C. in a reducing gas atmosphere, and the reaction pressure is maintained at 0.5 MPa to 3.0 MPa. After sufficient reaction, solid-liquid separation is performed and solid is retained to remove residual organic solvent, dodecanoic acid and polyvinyl pyrrolidone, thereby obtaining silver nanoparticles; The reducing gas is carbon monoxide.

2. The method for preparing silver nanoparticles according to claim 1, characterized in that: The ratio of the silver nitrate, the dodecanoic acid, the polyvinyl pyrrolidone and the organic solvent is (0.005 mol to 0.008 mol): (0.016 mol to 0.032 mol): (0.15 g to 0.4 g): (0.8 mol to 1.2 mol).

3. The method for preparing silver nanoparticles according to claim 1 or 2, characterized in that: The organic solvent is ethanol.

4. The method for preparing silver nanoparticles according to claim 1, characterized in that: The reaction pressure was maintained at 1.0 MPa to 2.0 MPa.

5. The method for preparing silver nanoparticles according to claim 1, characterized in that: The molecular weight of the polyvinyl pyrrolidone is 8000-40000.

6. The method for preparing silver nanoparticles according to claim 5, characterized in that: The molecular weight of the polyvinyl pyrrolidone is 12,000.

7. The method for preparing silver nanoparticles according to claim 1, characterized in that: The operation of performing solid-liquid separation and retaining the solid after sufficient reaction is as follows: after sufficient reaction, a reaction product is obtained, the reaction product is uniformly mixed with acetone, and then solid-liquid separation is performed and the solid is retained.

8. The method for preparing silver nanoparticles according to claim 1, characterized in that: The time for full reaction is 2h to 3h.

9. A silver nanoparticle, characterized in that: The silver nanoparticles are prepared by the method for preparing the silver nanoparticles according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Preparing method of triangular flaky nanometer silver particles

    CN103769601A

  • Method for preparing metal nano material by utilizing hydrogen

    CN104043841A

  • Nano-silver particle, and preparation method and purpose thereof

    CN111097922A

  • Preparation method of silver nanoparticles

    CN111992736A

  • Method for preparing nano silver powder through hydrogen reduction

    CN113427014A