A kind of biuret polyisocyanate composition and preparation method thereof

By adding binding hindered phenol antioxidants to biuret polyisocyanate, the color stability problem of long-term storage and high-temperature conditions is solved, and the efficient storage stability of polyurethane coatings is achieved.

CN114316210BActive Publication Date: 2024-11-12WANHUA CHEMICAL (NINGBO) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210004646.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-05
Publication Date
2024-11-12
Estimated Expiration
2042-01-05

AI Technical Summary

Technical Problem

Biuret polyisocyanate compositions are difficult to maintain the color size stability during long periods of storage, especially at environments above room temperature, which affects its performance in polyurethane coatings.

Method used

By adding 0.003-0.1% by weight of the binding hindered phenol antioxidant to the biuretic polyisocyanate, it ensures that the chromaticity of the platinum-cobalt color number evaluation increases by ≤5Hazen after 12 months of storage at room temperature, and 3 are stored at 50°C. The color level rises after the month ≤10Hazen.

Benefits of technology

The storage stability of the biuret polyisocyanate composition is achieved, ensuring its color stability under long-term storage and even high temperature conditions, and improving the performance of polyurethane coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0003456120360000041
    Figure BDA0003456120360000041
  • Figure BDA0003456120360000071
    Figure BDA0003456120360000071
Patent Text Reader

Abstract

The invention discloses a biuret polyisocyanate composition and a preparation method thereof. The composition contains 0.003-0.1wt% of a bound hindered phenol antioxidant, and the composition of the invention has excellent storage stability, and can achieve a chromaticity increase of ≤5 Hazen evaluated by a platinum-cobalt color number after storage at 25°C for 12 months, and a chromaticity increase of ≤10 Hazen evaluated by a platinum-cobalt color number after storage at 50°C for 3 months.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of isocyanates, and in particular relates to a biuret polyisocyanate composition and a preparation method thereof. Background Art

[0002] Polyurethane materials are known as the world's sixth largest synthetic material due to their flexible formula, diverse product forms and excellent product performance. They are increasingly widely used in various industries. Polyurethane coatings are one of the most important application areas of polyurethane materials. With their excellent mechanical wear resistance, good flexibility, strong adhesion and excellent chemical resistance, they are widely used in the fields of automotive original paint, automotive repair paint, plastic coatings, anti-corrosion coatings, wood paint, leather paint, etc.

[0003] The industrial products of diisocyanates used in polyurethane coatings mainly include MDI, TDI, HDI, IPDI, H 12 MDI and XDI, etc., are divided into aromatic isocyanates and aliphatic (cyclic) isocyanates. Among them, aliphatic (cyclic) isocyanate curing agents have good yellowing resistance, so they are more widely used in high-end fields such as original automotive paint and automotive repair paint, especially isocyanate curing agent products based on HDI. At present, the HDI-based isocyanate curing agents on the market are mainly HDI trimer and HDI biuret. Among them, the curing agent based on HDI biuret is famous for its excellent flexibility and strong adhesion of the coating film.

[0004] During long-term storage, the color number of HDI biuret-based curing agents will gradually increase, especially when stored above room temperature, the color number increase is more significant, seriously affecting downstream applications. When using curing agents containing HDI biuret, downstream coating customers are usually unable to use them in a timely manner. They often have to store them for a period of time before using them. Inevitably, they will be stored at higher temperatures. The industry has done a lot of research on the storage stability of isocyanates and the preparation of low-color isocyanates.

[0005] Chinese patent CN105601565B discloses a method for preparing biuret polyisocyanate, which utilizes polyisocyanate and water to react in the presence of substituted 8-aminomethylquinoline compounds and hydrazine derivatives to prepare biuret-containing polyisocyanate, the color number of the prepared product is lower than 20 Hazen, under the synergistic effect of substituted 8-aminomethylquinoline compounds and hydrazine hydrocarbon derivatives, the increase in monomer content of the product after 6 months of storage is less than 0.1wt%, and has excellent long-term storage stability. The method does not mention the color stability of the biuret polyisocyanate composition during storage.

[0006] Chinese patent CN106946741B discloses a method for preparing dicyclohexylmethane diisocyanate (H 12 MDI) method, by reacting the raw material dicyclohexylmethanediamine (H 12 MDA) was purified to obtain H containing less than 0.1 wt% of aromatic monoamine compounds. 12 MDA, then phosgenated to obtain H 12 MDI, the H 12 MDI has excellent storage resistance to yellowing. Under the same conditions and storage time, H 12 MDI color number is more stable, this method is suitable for polyisocyanate monomer H 12 The improvement of MDI's yellowing resistance during storage has no guiding role in improving the color stability of HDI-based biuret polyisocyanate compositions during storage.

[0007] Chinese patent CN110982045A discloses a low-viscosity and low-color isocyanate curing agent. The polarity of the polyisocyanate can be effectively reduced by using a long-chain fatty alcohol or alicyclic alcohol with a higher molecular weight for modification, thereby reducing the viscosity of the curing agent. At the same time, by controlling the peroxide and double bond content in the long-chain alcohol, a low-viscosity and low-color isocyanate curing agent can be prepared, which is beneficial to improving the storage stability of the curing agent. This patent improves the color stability of the isocyanate curing agent during storage by alcohol modification. The modification method changes the structure of the isocyanate itself, which will affect the application performance of the isocyanate curing agent.

[0008] CN111635502A discloses a method for preparing a polyisocyanate composition with stable color number, which relates to a polyisocyanate composition containing carbamate obtained by reacting isocyanate with a low molecular weight polyhydroxy compound, and the polyisocyanate composition can maintain stable color number when stored at room temperature for at least 12 months. The method is mainly characterized in that a debrominating agent is prepared, and a prepolymer obtained by reacting isocyanate with the polyhydroxy compound is debrominated by the debrominating agent, so as to achieve the polyisocyanate composition containing carbamate maintaining stable color number when stored at room temperature. The preparation process of the debrominating agent is complicated, which is not conducive to industrial implementation.

[0009] CN112225857A discloses a chromaticity-stable isocyanurate-containing polyisocyanate composition and a preparation method thereof, and relates to the improvement of the chromaticity stability of an HDI trimer curing agent during storage. The method is mainly characterized in that the HDI trimer product is heat-treated under high vacuum to reduce the content of cleavable amines in the product, and the chromaticity stability of the HDI trimer curing agent during storage is mainly solved from the perspective of controlling the content of catalyst residues in the preparation process of the HDI trimer. Since the catalytic mechanism of the HDI trimer is inconsistent with that of the HDI biuret, it has no guiding role in improving the chromaticity stability of the HDI biuret during storage.

[0010] The prior art mentions the preparation of light-colored polyisocyanate compositions, but there is no discussion on the chromaticity stability (i.e., maintaining a stable color number) of the biuret polyisocyanate composition. There is even no discussion on the color stability of the biuret polyisocyanate composition during use when the storage temperature is high.

[0011] When the biuret polyisocyanate composition is stored for a long period of time, especially when stored at a relatively high temperature (room temperature to 50° C.), it is difficult to maintain a stable color, which affects its performance in polyurethane coatings. Therefore, there is still an urgent need for a biuret polyisocyanate composition that can maintain a stable color. Summary of the invention

[0012] The object of the present invention is to provide a biuret polyisocyanate composition with excellent storage stability. The biuret polyisocyanate composition product has excellent storage stability and can achieve a product color increase of ≤5 Hazen evaluated by a platinum-cobalt color number after storage at room temperature for 12 months, and a product color increase of ≤10 Hazen evaluated by a platinum-cobalt color number after storage at 50°C for 3 months.

[0013] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:

[0014] A biuret polyisocyanate composition contains 0.003-0.1wt% of a bound hindered phenol antioxidant. Based on the total mass of the composition, the composition has a chromaticity increase of ≤5 Hazen as evaluated by a platinum-cobalt color number after being stored at 25°C for 12 months, and a chromaticity increase of ≤10 Hazen as evaluated by a platinum-cobalt color number after being stored at 50°C for 3 months.

[0015] In the present invention, the bound hindered phenol antioxidant has the following structure:

[0016]

[0017] Wherein, R is the residue in the polyisocyanate structure other than the NCO group bonded to the phenolic hydroxyl group,

[0018] Here, X is the residue of the hindered phenol antioxidant structure except the phenolic hydroxyl group bonded to the NCO group.

[0019] In the present invention, the composition is a polyisocyanate containing biuret groups prepared from diisocyanate monomers as raw materials.

[0020] In the present invention, the diisocyanate monomer is one or more diisocyanate monomers containing 4 to 20 carbon atoms in addition to the NCO group in the carbon skeleton, and at least contains hexamethylene diisocyanate monomers, preferably toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, naphthalene diisocyanate, p-phenylene diisocyanate, 1,4-cyclohexane diisocyanate, methylcyclohexyl diisocyanate, norbornane diisocyanate, trimethyl-1,6-hexamethylene diisocyanate. The monomer is one or more of pentamethylene diisocyanate, hexamethylene diisocyanate, 1,4-cyclohexane diisocyanate, and at least hexamethylene diisocyanate monomer. The monomer is more preferably one or more of pentamethylene diisocyanate, hexamethylene diisocyanate, and 1,4-cyclohexane diisocyanate, and at least hexamethylene diisocyanate monomer. The monomer is further preferably pentamethylene diisocyanate and / or hexamethylene diisocyanate, and at least hexamethylene diisocyanate monomer. The most preferred monomer is hexamethylene diisocyanate.

[0021] In the present invention, the hindered phenol antioxidant is a monohydric hindered phenol antioxidant and / or a polyhydric hindered phenol antioxidant; wherein the monohydric hindered phenol antioxidant is one or more of 2,6-di-tert-butyl-4-methylphenol (antioxidant BHT), β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl alcohol ester (antioxidant 1076), 3,5-di-tert-butyl-4-hydroxyphenylpropionic acid C7-C9 mixed ester (antioxidant 1135), 4,6-di(octylthiomethyl)-o-cresol (antioxidant 1520), 4,6-di(dodecylthiomethyl)-o-cresol (antioxidant 1726). The polyhedral hindered phenol antioxidants are pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] (antioxidant 1010), N,N'-bis(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl)propylenediamine (antioxidant 1019), 2,2'-thioethylene glycol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] (antioxidant 1035), N,N'-hexamethylene bis(3,5-di-tert-butyl-4-hydroxyphenyl propionamide) (antioxidant 1098), 1,3,5-tris(4-tert-butyl-3-hydroxy-2 ,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione (Antioxidant 1790), triethylene glycol bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl) propionate] (Antioxidant 245), 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (Antioxidant 3114), 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene (Antioxidant 330), diethylene glycol bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl) propionate] (Antioxidant 245), 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (Antioxidant 3114), 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene (Antioxidant 330), One or more of (3,5-di-tert-butyl-4-hydroxy-phenylpropionyl) hydrazine (antioxidant MD-1024), 2,2-oxalyl-bis[ethyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)] propionate (antioxidant MD-697); preferably one or more of BHT, 3,5-di-tert-butyl-4-hydroxyphenylpropionic acid C7-C9 mixed ester (antioxidant 1135), 4,6-bis(octylthiomethyl)-o-cresol (antioxidant 1520), more preferably 3,5-di-tert-butyl-4-hydroxyphenylpropionic acid C7-C9 mixed ester (antioxidant 1135).

[0022] Another object of the present invention is to provide a method for preparing the biuret polyisocyanate composition.

[0023] A preparation method for the above-mentioned biuret polyisocyanate composition, the preparation method comprising: a diisocyanate monomer and water are subjected to a polymerization reaction under the action of a catalyst to obtain a biuret polyisocyanate reaction liquid, the reaction liquid is separated to obtain an intermediate of the biuret polyisocyanate composition, the intermediate is mixed with a solvent according to specific uses to obtain a biuret polyisocyanate composition solution product with different solid contents, or is directly packaged into a biuret polyisocyanate composition product, wherein a hindered phenol antioxidant is added in the above-mentioned preparation process.

[0024] In one embodiment, the reaction process of the preparation method of the biuret polyisocyanate composition adopts the following process: in the presence of a catalyst, the polyisocyanate monomer reacts with water at 150° C. for 3 hours; the amount of water used is 20% of the molar amount of the NCO group of the polyisocyanate monomer. The catalyst is diisooctyl phosphate, and the amount of the catalyst used is 0.15% based on the total amount of the polyisocyanate monomer used.

[0025] In one embodiment, the separation process of the preparation method of the biuret polyisocyanate composition adopts the following process, wherein the reaction liquid of the biuret polyisocyanate composition is separated by a thin film evaporator and / or a short path evaporator. According to the well-known art, two, three or more stages of thin film evaporators and / or short path evaporators can be used in series to separate the reaction liquid of the biuret polyisocyanate composition. In the present invention, two stages of short path evaporators are preferably used in series to separate to obtain a biuret polyisocyanate intermediate. In the present invention, the hindered phenol antioxidant is added in any stage of the reaction or separation process in the method. Preferably, the hindered phenol antioxidant is added together with the raw materials during the reaction process of preparing biuret polyisocyanate, or the hindered phenol antioxidant is added to the reaction solution after the reaction solution of biuret polyisocyanate is prepared and enters the separation system together with the reaction solution, or the hindered phenol antioxidant is added to the biuret polyisocyanate intermediate by premixing after the reaction solution containing the biuret polyisocyanate composition is separated, and more preferably, the hindered phenol antioxidant is added to the biuret polyisocyanate intermediate by premixing after the reaction solution containing the biuret polyisocyanate composition is separated.

[0026] In the present invention, the hindered phenol antioxidant is added in the following manner: a portion of the biuret polyisocyanate reaction liquid is separated to obtain a biuret polyisocyanate intermediate, and the hindered phenol antioxidant is added to an antioxidant premixing kettle for premixing, and then mixed with the remaining portion of the biuret polyisocyanate intermediate to obtain a biuret polyisocyanate composition product. During the premixing process, the amount of the hindered phenol antioxidant added is 0.5-10wt%, and the molar ratio of the NCO group to the phenolic hydroxyl group is far in excess. The reaction of the phenolic hydroxyl group with the NCO group usually only generates a bound hindered phenol antioxidant of the following structure as described in the present invention:

[0027]

[0028] Wherein, R is the residue in the polyisocyanate structure other than the NCO group bonded to the phenolic hydroxyl group,

[0029] Here, X is the residue of the hindered phenol antioxidant structure except the phenolic hydroxyl group bonded to the NCO group.

[0030] Theoretically, since the bonding reaction between the phenolic hydroxyl group of the hindered phenol antioxidant and the NCO group of the biuret polyisocyanate intermediate is a slow reaction and the molar ratio of the NCO group is far in excess, the reaction of a single biuret polyisocyanate intermediate molecule with multiple hindered phenol antioxidant molecules will not occur. In fact, the structure of a single biuret polyisocyanate intermediate molecule reacting with multiple hindered phenol antioxidant molecules was not detected during the analysis and detection.

[0031] The total amount of hindered phenol antioxidant added in the biuret polyisocyanate composition product is 0.005-0.2% of the total mass of the biuret polyisocyanate composition, wherein the hindered phenol antioxidant exists in two forms in the biuret polyisocyanate composition product, namely, a bound state and a free state, and the bound state content is 0.003-0.1% of the total mass of the biuret polyisocyanate composition.

[0032] In the present invention, the antioxidant premixing kettle is a kettle reactor containing a stirrer, and the reactor is equipped with a circulation pump and a circulation pipeline; preferably, the hindered phenol antioxidant is added to the reactor through a Venturi mixer arranged in the circulation pipeline.

[0033] In the present invention, the temperature of the antioxidant premixing kettle is 60-90°C, preferably 70-80°C, and the residence time of the hindered phenol antioxidant and the biuret polyisocyanate intermediate in the kettle is 10-40min, preferably 20-30min.

[0034] In the present invention, in the antioxidant premixing kettle, the material at the point where the hindered phenol antioxidant is added is in a turbulent state, and the Reynolds number is ≥5000, preferably ≥6000.

[0035] In the present invention, in the antioxidant premixing kettle, the stirring power received by the material per unit volume is 3-10KW / m 3 , preferably 5-8KW / m 3 .

[0036] In a preferred embodiment, the hindered phenol antioxidant is antioxidant 1135, and the biuret polyisocyanate composition product is HDI biuret polyisocyanate. The structure of the hindered phenol antioxidant in the combined state of the present invention is exemplified as follows. It should be noted that these are all exemplary descriptions, and do not mean that the present invention requires that the structure of the hindered phenol antioxidant in the combined state be selected from one of the following structures:

[0037]

[0038] The inventors of the present application have conducted extensive research on the preparation and storage stability of biuret polyisocyanate compositions, especially the factors affecting the color stability during long-term storage or even storage at higher temperatures (room temperature to 50°C), and found that the presence of a certain amount of the bound hindered phenol antioxidant described in the present invention significantly improves the color stability of the biuret polyisocyanate during storage.

[0039] The yellowing of isocyanate products during long-term storage is a well-known technical problem in the industry, especially in aromatic isocyanate products. The yellowing mechanism is mainly free radical reaction caused by light and oxidation. The usual solution in the industry is to add antioxidants to the products. In the field of isocyanates, hindered phenol antioxidants or compound antioxidants with hindered phenol antioxidants as the main antioxidants are usually used. However, there are some unavoidable disadvantages in adding antioxidants. A small amount of addition will lead to a poor antioxidant effect and cannot meet the requirements of long-term storage of the product. A large amount of addition will inevitably lead to an increase in the free phenol content in the product. Due to the increasingly stringent environmental protection requirements, excessive free phenol seriously affects the application and promotion of isocyanate products in the downstream market. To solve this problem, some antioxidant manufacturers are also developing hindered phenol antioxidants with more complex structures and better performance. However, due to technical and cost reasons, it is still difficult to achieve industrial application. The present invention controls the production process by adding conventional hindered phenol antioxidants into biuret polyisocyanate, so that the product can maintain color stability during long-term storage or even storage at higher temperatures (room temperature to 50° C.), which is unknown in the prior art.

[0040] The usual method of adding antioxidants in the biuret polyisocyanate composition industry is to add them to the product at room temperature before packaging. However, due to the excessive steric hindrance of the phenolic hydroxyl group in the hindered phenol molecular chain, the phenolic hydroxyl group added to the biuret polyisocyanate at room temperature is chemically inert and will not react with the NCO group in the biuret polyisocyanate, that is, the hindered phenol antioxidant is in a free state.

[0041] The inventors have found that by special process control, such as adding the hindered phenol antioxidant at any stage of the reaction or separation process of the preparation of the biuret polyisocyanate, it is ensured that the hindered phenol antioxidant is mixed and stirred with the free NCO group at a temperature of at least 60°C for at least 10 minutes after addition. The present invention preferably adds the hindered phenol antioxidant by premixing treatment, so that the NCO group in the biuret polyisocyanate can be bonded with the phenolic hydroxyl group in part of the hindered phenol antioxidant. At the same time, the bound hindered phenol antioxidant after bonding can exert a more lasting antioxidant effect when the biuret polyisocyanate is stored for a long period of time or even at a higher temperature (room temperature to 50°C), thereby achieving color stability of the biuret polyisocyanate.

[0042] The reaction in the premixing kettle of the present invention is as follows (taking HDI and antioxidant 1135 as an example):

[0043]

[0044] The inventors have found through long-term research that when the biuret polyisocyanate composition product is stored for a long period of time or even at a relatively high temperature (room temperature to 50° C.), the added free hindered phenol antioxidant is more likely to undergo thermal oxidative aging and lose its antioxidant effect, while the bound hindered phenol antioxidant will gradually undergo a slow reaction as described in the following formula (taking HDI and antioxidant 1135 as an example), gradually releasing new free hindered phenol antioxidants:

[0045]

[0046] The released free hindered phenol antioxidant can continuously play an antioxidant effect and maintain the color stability of the biuret isocyanate composition. Compared with the biuret polyisocyanate composition product to which only the free hindered phenol antioxidant is added, the biuret polyisocyanate prepared by the scheme of the present invention has better color stability during storage.

[0047] The technical solution provided by the present invention has the following beneficial effects:

[0048] According to the preparation method of the present invention, the prepared biuret polyisocyanate composition product has excellent storage stability, and the color of the product evaluated by the platinum-cobalt color number can be increased by ≤5 Hazen after storage at room temperature for 12 months, and the color of the product evaluated by the platinum-cobalt color number can be increased by ≤10 Hazen after storage at 50°C for 3 months. DETAILED DESCRIPTION

[0049] In order to better understand the technical solution of the present invention, the content of the present invention is further described below in conjunction with specific embodiments, but it should be noted that the content of the present invention is not limited to the following embodiments.

[0050] The bound hindered phenol antioxidants were qualitatively and quantitatively analyzed by high performance liquid chromatography;

[0051] Instrument: Agilent 1260; chromatographic column: Agilent Extend C18 RRHD 2.1×100mm 1.8μm; column temperature: 40°C; flow rate: 0.2ml / min; mobile phase: A: pure water, B: pure acetonitrile (Sigma-Aldrich (Shanghai) Trading Co., Ltd., HPLC, purity 99.9%); injection volume: 20μL; detection wavelength: 210nm.

[0052] The color number of the biuret polyisocyanate composition product is determined by GB / T 3143-1982 to determine its platinum-cobalt color number value, and is specifically measured using the German BYK LCS IV liquid colorimeter.

[0053] Example 1

[0054] The hindered phenol antioxidant is added after the separation stage.

[0055] Step 1: Preparation of HDI biuret polyisocyanate intermediates:

[0056] 3000 g of hexamethylene diisocyanate (HDI, Wanhua Chemical Group Co., Ltd., brand No. HDI, purity 99.95%), 64.3g of water vapor was introduced, 8.6g of diisooctyl phosphate (Luoyang Aoda Chemical Co., Ltd., CAS No.: 298-07-7, purity 95%) was added as a catalyst, and the mixture was reacted at 150°C for 3 hours to obtain an HDI biuret reaction liquid. The obtained HDI biuret reaction liquid was separated in series by a two-stage short-path evaporator to obtain an HDI biuret polyisocyanate intermediate.

[0057] Step 2: Antioxidant premixing: Take 95g of the HDI biuret polyisocyanate intermediate obtained in the first step and add it to the antioxidant premixing kettle, add 5g of 3,5-di-tert-butyl-4-hydroxyphenylpropionic acid C7-C9 mixed ester (Antioxidant 1135, Tianjin Lianlong New Materials Co., Ltd., brand antioxidant 1135, purity 98%) is added to the antioxidant premixing kettle through a Venturi mixer set in the circulation line. The liquid in the circulation pipe is in a turbulent state, the Reynolds number is 7500, the temperature in the premixing kettle is controlled at 75°C, and the stirring power in the kettle is 6KW / m 3 , stirring and reacting for 25 minutes, to obtain an HDI biuret polyisocyanate intermediate containing bound antioxidant 1135. The detection showed that the content of bound antioxidant 1135 accounted for 60% of the total amount of added antioxidant 1135.

[0058] Step 3: Product preparation: Take 1g of the HDI biuret polyisocyanate intermediate containing bound antioxidant 1135 obtained in the second step, and mix it with 999g of the HDI biuret polyisocyanate intermediate obtained in the first step. After mixing evenly, the total content of antioxidant 1135 in the HDI biuret polyisocyanate product is 0.005wt%, and the content of bound antioxidant 1135 is 0.003wt%.

[0059] The HDI biuret polyisocyanate product obtained in the third step was stored at room temperature for 12 months and at 50° C. for 3 months, and the color numbers before and after storage were tested respectively.

[0060] Example 2

[0061] Hindered phenol antioxidant was added before the reaction stage. 3000 g of hexamethylene diisocyanate (HDI, Wanhua Chemical Group Co., Ltd., brand HDI, purity 99.95%), 64.3g of water vapor was introduced, 8.6g of diisooctyl phosphate (Luoyang Aoda Chemical Co., Ltd., CAS No.: 298-07-7, purity 95%) was added as a catalyst, 0.08g of antioxidant 1135 was added, and the mixture was reacted at 150°C for 3 hours to obtain HDI biuret reaction liquid. The obtained HDI biuret reaction liquid was separated in series by a two-stage short-path evaporator to obtain an HDI biuret polyisocyanate intermediate. The total content of antioxidant 1135 was 0.05wt%, and the content of bound antioxidant 1135 was 0.04wt%.

[0062] Example 3

[0063] The hindered phenol antioxidant is added before the separation stage.

[0064] 3000 g of hexamethylene diisocyanate (HDI, Wanhua Chemical Group Co., Ltd., brand No. HDI, purity 99.95%), 64.3g of water vapor was introduced, 8.6g of diisooctyl phosphate (Luoyang Aoda Chemical Co., Ltd., CAS No.: 298-07-7, purity 95%) was added as a catalyst, and the mixture was reacted at 150°C for 3 hours to obtain an HDI biuret reaction liquid. 0.08g of antioxidant 1135 was first added to the obtained HDI biuret reaction liquid, and then separated by a two-stage short-path evaporator in series to obtain an HDI biuret polyisocyanate intermediate. The total content of antioxidant 1135 was 0.05wt%, and the content of bound antioxidant 1135 was 0.03wt%.

[0065] Embodiment 4-8

[0066] Examples 4-8 were prepared with reference to Example 1, except that the mixing ratio of the antioxidant and the HDI biuret polyisocyanate intermediate in the second step "antioxidant premixing" was different and the mixing ratio in the third step "product preparation" was different. The HDI biuret polyisocyanate product was prepared by controlling the mixing ratio of the antioxidant 1135 in the antioxidant premixing kettle in the second step and the preparation ratio in the third step.

[0067] Example 9

[0068] The hindered phenol antioxidant is added after the separation stage.

[0069] Step 1: Preparation of HDI / PDI mixed biuret polyisocyanate intermediates:

[0070] 1500 g of hexamethylene diisocyanate (HDI, Wanhua Chemical Group Co., Ltd., brand No. HDI, purity 99.95%) and 1500g of pentamethylene diisocyanate (PDI, CAS: 4538-42-5 purchased from Mitsui Chemicals, Inc., purity 99.5%), 67.2g of water vapor is introduced, 8.6g of diisooctyl phosphate (Luoyang Aoda Chemical Co., Ltd., CAS No.: 298-07-7, purity 95%) is added as a catalyst, and the mixture is reacted at 150°C for 3 hours to obtain an HDI / PDI mixed biuret reaction liquid. The obtained HDI / PDI mixed biuret reaction liquid is separated in series by a two-stage short-path evaporator to obtain an HDI / PDI mixed biuret polyisocyanate intermediate.

[0071] Step 2: Antioxidant premixing: Take 99.5g of the HDI / PDI mixed biuret polyisocyanate intermediate obtained in the first step and add it to the antioxidant premixing kettle, add 0.5g of antioxidant BHT (Tianjin Lianlong New Materials Co., Ltd., brand antioxidant BHT, purity 98%) was added to the antioxidant premixing kettle through a Venturi mixer set in the circulation line. The liquid in the circulation pipe was in a turbulent state, the Reynolds number was 8000, the temperature in the premixing kettle was controlled at 60°C, and the stirring power in the kettle was 10KW / m 3 , stirring and reacting for 40 minutes, to obtain an HDI / PDI mixed biuret polyisocyanate intermediate containing a bound antioxidant BHT. The detection showed that the content of the bound antioxidant BHT accounted for 80% of the total amount of the added antioxidant BHT.

[0072] Step 3: Product preparation: Take 10g of the HDI / PDI mixed biuret polyisocyanate intermediate containing bound antioxidant BHT obtained in the second step, and mix it with 990g of the HDI / PDI mixed biuret polyisocyanate intermediate obtained in the first step. After mixing evenly, the total content of antioxidant BHT in the HDI / PDI mixed biuret polyisocyanate product is 0.005wt%, and the content of bound antioxidant BHT is 0.004wt%.

[0073] The HDI / PDI mixed biuret polyisocyanate product obtained in the third step was stored at room temperature for 12 months and at 50° C. for 3 months, and the color numbers before and after storage were tested respectively.

[0074] Example 10

[0075] The hindered phenol antioxidant is added after the separation stage.

[0076] Step 1: Preparation of HDI / PDI / CHDI mixed biuret polyisocyanate intermediates:

[0077] 1000 g of hexamethylene diisocyanate (HDI, Wanhua Chemical Group Co., Ltd., brand No. HDI, purity 99.95%) and 1000g of pentamethylene diisocyanate (PDI, CAS: 4538-42-5, purchased from Mitsui Chemicals, Inc., purity 99.5%) and 1000g of 1,4-cyclohexane diisocyanate (CHDI, CAS: 7517-76-2, purchased from DuPont, USA, purity 99%), 66.5g of water vapor is introduced, 8.6g of diisooctyl phosphate (Luoyang Aoda Chemical Co., Ltd., CAS No.: 298-07-7, purity 95%) is added as a catalyst, and the mixture is reacted at 150°C for 3 hours to obtain an HDI / PDI / CHDI mixed biuret reaction liquid. The obtained HDI / PDI / CHDI mixed biuret reaction liquid is separated in series by a two-stage short-path evaporator to obtain an HDI / PDI / CHDI mixed biuret polyisocyanate intermediate.

[0078] Step 2: Antioxidant premixing: Take 90g of the HDI / PDI / CHDI mixed biuret polyisocyanate intermediate obtained in the first step and add it to the antioxidant premixing kettle, add 10g of 4,6-bis(octylthiomethyl)-o-cresol (Antioxidant 1520, Tianjin Lianlong New Materials Co., Ltd., brand antioxidant 1520, purity 98%) is added to the antioxidant premixing kettle through a Venturi mixer set in the circulation line. The liquid in the circulation pipe is in a turbulent state, the Reynolds number is 7000, the temperature in the premixing kettle is controlled at 70°C, and the stirring power in the kettle is 8KW / m 3 , stirring and reacting for 30 minutes, to obtain an HDI / PDI / CHDI mixed biuret polyisocyanate intermediate containing bound antioxidant 1520. The detection showed that the content of bound antioxidant 1520 accounted for 35% of the total amount of added antioxidant 1520.

[0079] Step 3: Product preparation: Take 1g of the HDI / PDI / CHDI mixed biuret polyisocyanate intermediate containing bound antioxidant 1520 obtained in the second step, and mix it with 999g of the HDI / PDI / CHDI mixed biuret polyisocyanate intermediate obtained in the first step. After mixing evenly, the total content of antioxidant 1520 in the HDI / PDI / CHDI mixed biuret polyisocyanate product is 0.01wt%, and the content of bound antioxidant 1520 is 0.0035wt%.

[0080] The HDI / PDI / CHDI mixed biuret polyisocyanate product obtained in the third step was stored at room temperature for 12 months and at 50°C for 3 months, and the color numbers before and after storage were tested respectively.

[0081] Embodiment 11

[0082] The hindered phenol antioxidant is added after the separation stage.

[0083] Step 1: Preparation of HDI / TDI mixed biuret polyisocyanate intermediates:

[0084] 1500 g of hexamethylene diisocyanate (HDI, Wanhua Chemical Group Co., Ltd., brand No. HDI, purity 99.95%) and 1500 g toluene diisocyanate (TDI, Wanhua Chemical Group Co., Ltd., brand TDI-80, purity 99.5%), 63.2g of water vapor was introduced, 8.6g of diisooctyl phosphate (Luoyang Aoda Chemical Co., Ltd., CAS No.: 298-07-7, purity 95%) was added as a catalyst, and the mixture was reacted at 150°C for 3 hours to obtain an HDI / TDI mixed biuret reaction liquid. The obtained HDI / TDI mixed biuret reaction liquid was separated in series by a two-stage short-path evaporator to obtain an HDI / TDI mixed biuret polyisocyanate intermediate.

[0085] Step 2: Antioxidant premixing: Take 95g of the HDI / TDI mixed biuret polyisocyanate intermediate obtained in the first step and add it to the antioxidant premixing kettle, add 5g of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (Antioxidant 1010, Tianjin Lianlong New Materials Co., Ltd., brand antioxidant 1010, purity 98%) is added to the antioxidant premixing kettle through a Venturi mixer set in the circulation line. The liquid in the circulation pipe is in a turbulent state, the Reynolds number is 6000, the temperature in the premixing kettle is controlled at 80°C, and the stirring power in the kettle is 5KW / m 3 , stirring and reacting for 20 minutes, to obtain an HDI / TDI mixed biuret polyisocyanate intermediate containing bound antioxidant 1010. The detection showed that the content of bound antioxidant 1010 accounted for 50% of the total amount of added antioxidant 1010.

[0086] Step 3: Product preparation: Take 10g of the HDI / TDI mixed biuret polyisocyanate intermediate containing bound antioxidant 1010 obtained in the second step, and mix it with 240g of the HDI / TDI mixed biuret polyisocyanate intermediate obtained in the first step. After mixing evenly, the total content of antioxidant 1010 in the HDI / TDI mixed biuret polyisocyanate product is 0.2wt%, and the content of bound antioxidant 1010 is 0.1wt%.

[0087] The HDI / TDI mixed biuret polyisocyanate product obtained in the third step was stored at room temperature for 12 months and at 50° C. for 3 months, and the color numbers before and after storage were tested respectively.

[0088] Example 12

[0089] The hindered phenol antioxidant is added after the separation stage.

[0090] Step 1: Preparation of HDI / IPDI mixed biuret polyisocyanate intermediates:

[0091] 1500 g of hexamethylene diisocyanate (HDI, Wanhua Chemical Group Co., Ltd., brand No. HDI, purity 99.95%) and 1500 g isophorone diisocyanate (IPDI, Wanhua Chemical Group Co., Ltd., brand IPDI, purity 99.5%), 56.5g of water vapor was introduced, 8.6g of diisooctyl phosphate (Luoyang Aoda Chemical Co., Ltd., CAS No.: 298-07-7, purity 95%) was added as a catalyst, and the mixture was reacted at 150°C for 3 hours to obtain an HDI / IPDI mixed biuret reaction liquid. The obtained HDI / IPDI mixed biuret reaction liquid was separated in series by a two-stage short-path evaporator to obtain an HDI / IPDI mixed biuret polyisocyanate intermediate.

[0092] Step 2: Antioxidant premixing: 97 g of the HDI / IPDI mixed biuret polyisocyanate intermediate obtained in the first step was added to the antioxidant premixing kettle, and 3 g of triethylene glycol bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl) propionate] (Antioxidant 245, Tianjin Lianlong New Materials Co., Ltd., brand antioxidant 245, purity 98%) is added to the antioxidant premixing kettle through a Venturi mixer set in the circulation line. The liquid in the circulation pipe is in a turbulent state, the Reynolds number is 5000, the temperature in the premixing kettle is controlled at 90°C, and the stirring power in the kettle is 3KW / m 3, stirring and reacting for 10 minutes, to obtain an HDI / IPDI mixed biuret polyisocyanate intermediate containing bound antioxidant 245. The detection showed that the content of bound antioxidant 245 accounted for 10% of the total amount of added antioxidant 245.

[0093] Step 3: Product preparation: Take 10g of the HDI / IPDI mixed biuret polyisocyanate intermediate containing bound antioxidant 245 obtained in the second step, and mix it with 900g of the HDI / IPDI mixed biuret polyisocyanate intermediate obtained in the first step. After mixing evenly, the total content of antioxidant 245 in the HDI / IPDI mixed biuret polyisocyanate product is 0.03wt%, and the content of bound antioxidant 245 is 0.003wt%.

[0094] The HDI / IPDI mixed biuret polyisocyanate product obtained in the third step was stored at room temperature for 12 months and at 50°C for 3 months, and the color numbers before and after storage were tested respectively.

[0095] Comparative Examples 1-4

[0096] Comparative Examples 1-4 were prepared with reference to Example 1.

[0097] The difference between Comparative Example 1 and Example 1 is that the second step of "antioxidant premixing" and the third step of "product preparation" are omitted, and no antioxidant is added, and the HDI biuret polyisocyanate product without antioxidant is prepared.

[0098] The difference between Comparative Example 2-4 and Example 1 is that there is no second step of "antioxidant premixing" and the third step of "product preparation", and the free antioxidant 1135 is directly added to the HDI biuret polyisocyanate intermediate in the first step at room temperature, and mixed evenly to produce the HDI biuret polyisocyanate product.

[0099] The content of antioxidant 1135 in HDI biuret polyisocyanate and the color change data during storage in the examples and comparative examples are shown in Table 1:

[0100] Table 1 Conditions and results of Examples 1-12 and Comparative Examples 1-4

[0101]

[0102] According to the results of Examples 1-8 and Comparative Examples 1-3, when HDI biuret polyisocyanate products with the same initial color number are stored at room temperature for 12 months, the color number of the product without adding an antioxidant increases by 25 Hazen, the color number of the product containing 0.003-0.1wt% of the bound antioxidant 1135 increases by ≤5 Hazen, and the color number of the product with the same amount of free antioxidant 1135 increases by 10-15 Hazen; during storage at 50°C for 3 months, the color number of the product without adding an antioxidant increases by 30 Hazen, the color number of the product containing 0.003-0.1wt% of the bound antioxidant 1135 increases by ≤10 Hazen, and the color number of the product with the same amount of free antioxidant 1135 increases by 15-25 Hazen.

[0103] Comparison of the results of Example 1 with those of Example 2 and Example 3 shows that there is no essential difference in achieving the effect of the present invention between the preferred method of premixing and adding the antioxidant 1135 and the method of adding the antioxidant 1135 during the reaction or separation process of preparing HDI biuret polyisocyanate. As long as the content of bound antioxidant 1135 in the final product is ensured to be 0.003-0.1wt%, the product color evaluated by the platinum-cobalt color number after storage at room temperature for 12 months can increase by ≤5Hazen, and the product color evaluated by the platinum-cobalt color number can increase by ≤10Hazen after storage at 50°C for 3 months.

[0104] By comparing the data of Examples 9-12 with that of Example 1, it can be seen that not only HDI biuret polyisocyanate, but also biuret polyisocyanates prepared from other polyisocyanate monomers described in this patent, by adding hindered phenol antioxidants using the method of the present invention, not only the preferred antioxidant 1135 of the present invention, but also other hindered phenol antioxidants that meet the description of the present invention can be used, as long as the content of bound hindered phenol antioxidant in the final biuret polyisocyanate product is ensured to be 0.003-0.1wt%, the chromaticity of the biuret polyisocyanate product evaluated by platinum-cobalt color number after storage at room temperature for 12 months can be increased by ≤5Hazen, and the chromaticity evaluated by platinum-cobalt color number after storage at 50°C for 3 months can be increased by ≤10Hazen.

[0105] Those skilled in the art will appreciate that, based on the teachings of this specification, some modifications or adjustments may be made to the present invention, and these modifications or adjustments should also be within the scope defined by the claims of the present invention.

Claims

1. A biuret polyisocyanate composition, characterized in that: The composition contains 0.003-0.1 wt% of a bound hindered phenol antioxidant, based on the total mass of the composition, and the color of the composition evaluated by a platinum-cobalt color number increases by ≤5 Hazen after being stored at 25° C. for 12 months, and the color of the composition evaluated by a platinum-cobalt color number increases by ≤10 Hazen after being stored at 50° C. for 3 months; The bound hindered phenol antioxidant has the following structure: wherein R is a residue in the polyisocyanate structure other than the NCO group bonded to the phenolic hydroxyl group, wherein X is a residue in the hindered phenol antioxidant structure other than the phenolic hydroxyl group bonded to the NCO group; The biuret polyisocyanate composition is prepared by polymerization of diisocyanate monomers and water under the action of a catalyst to obtain a biuret polyisocyanate reaction liquid, and the reaction liquid is separated to obtain an intermediate of the biuret polyisocyanate composition. The intermediate is mixed with a solvent to obtain a biuret polyisocyanate composition solution product with different solid contents according to specific uses, or is directly packaged into a biuret polyisocyanate composition product, wherein a hindered phenol antioxidant is added in the above preparation process.

2. The composition according to claim 1, characterized in that The composition is a polyisocyanate containing biuret groups which is prepared by taking diisocyanate monomer as raw material.

3. The composition according to claim 1, characterized in that The diisocyanate monomers are one or more diisocyanate monomers containing 4 to 20 carbon atoms in addition to the NCO group in the carbon skeleton, and at least contain hexamethylene diisocyanate monomers.

4. The composition according to claim 3, characterized in that The diisocyanate monomer is one or more of toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, naphthalene diisocyanate, p-phenylene diisocyanate, 1,4-cyclohexane diisocyanate, methylcyclohexyl diisocyanate, norbornane diisocyanate, trimethyl-1,6-hexamethylene diisocyanate, tetramethyl meta-xylylene diisocyanate, lysine diisocyanate, cyclohexane dimethylene diisocyanate, and xylylene diisocyanate, and at least contains hexamethylene diisocyanate monomer.

5. The composition according to claim 4, characterized in that The diisocyanate monomer is one or more of pentamethylene diisocyanate, hexamethylene diisocyanate, and 1,4-cyclohexane diisocyanate, and at least contains hexamethylene diisocyanate monomer.

6. The composition according to claim 5, characterized in that The diisocyanate monomer is pentamethylene diisocyanate and / or hexamethylene diisocyanate, and at least contains hexamethylene diisocyanate monomer.

7. The composition according to claim 6, characterized in that The diisocyanate monomer is hexamethylene diisocyanate.

8. The composition according to claim 1, characterized in that The hindered phenol antioxidant is a monohydric hindered phenol antioxidant and / or a polyhydric hindered phenol antioxidant; wherein the monohydric hindered phenol antioxidant is 2,6-di-tert-butyl-4-methylphenol (antioxidant BHT), β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl alcohol ester (antioxidant 1076), 3,5-di-tert-butyl-4-hydroxyphenylpropionic acid C7-C9 mixed ester (antioxidant 1135), 4,6-di(octylthiomethyl) o-cresol (antioxidant 1520), 4,6-di(dodecane) The polyhedral hindered phenol antioxidant is one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol ester (antioxidant 1010), N,N'-bis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)propylenediamine (antioxidant 1019), 2,2'-thioethylene glycol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (antioxidant 1035), N,N'-hexamethoxyethane Methyl bis(3,5-di-tert-butyl-4-hydroxyphenylpropionamide) (Antioxidant 1098), 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione (Antioxidant 1790), triethylene glycol bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl) propionate] (Antioxidant 245), 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1, One or more of 3,5-triazine-2,4,6(1H,3H,5H)-trione (antioxidant 3114), 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene (antioxidant 330), bis(3,5-di-tert-butyl-4-hydroxy-phenylpropionyl)hydrazine (antioxidant MD-1024), and 2,2-oxalylamino-bis[ethyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)]propionate (antioxidant MD-697).

9. The composition according to claim 8, characterized in that The hindered phenol antioxidant is one or more of BHT, 3,5-di-tert-butyl-4-hydroxybenzenepropionic acid C7-C9 mixed ester (antioxidant 1135), and 4,6-di(octylthiomethyl)-o-cresol (antioxidant 1520).

10. The composition according to claim 9, characterized in that The hindered phenol antioxidant is 3,5-di-tert-butyl-4-hydroxybenzenepropionic acid C7-C9 mixed ester (antioxidant 1135).

11. A method for preparing the biuret polyisocyanate composition according to any one of claims 1 to 10, characterized in that: The preparation method comprises the following steps: a diisocyanate monomer and water are polymerized under the action of a catalyst to obtain a biuret polyisocyanate reaction liquid; the reaction liquid is separated to obtain an intermediate of a biuret polyisocyanate composition; the intermediate is mixed with a solvent to obtain a biuret polyisocyanate composition solution product with different solid contents according to specific uses, or the intermediate is directly packaged into a biuret polyisocyanate composition product; wherein a hindered phenol antioxidant is added in the above preparation process.

12. The preparation method according to claim 11, characterized in that: In the method, the hindered phenol antioxidant is added at any stage of the reaction or separation process.

13. The preparation method according to claim 12, characterized in that: In the method, the hindered phenol antioxidant is added together with the raw materials during the reaction process of preparing the biuret polyisocyanate, or the hindered phenol antioxidant is added to the reaction solution after the biuret polyisocyanate is prepared, and enters the separation system together with the reaction solution, or the hindered phenol antioxidant is added to the biuret polyisocyanate intermediate by premixing after the reaction solution containing the biuret polyisocyanate composition is separated; Add the hindered phenol antioxidant and stir to mix.

14. The preparation method according to claim 13, characterized in that: In the method, after the hindered phenol antioxidant is separated from the reaction liquid containing the biuret polyisocyanate composition, the hindered phenol antioxidant is added to the biuret polyisocyanate intermediate by premixing; The stirring temperature of the stirring mixture is ≥60°C and the stirring time is ≥10min.

15. The preparation method according to claim 12, characterized in that: The hindered phenol antioxidant is added in the following manner: a biuret polyisocyanate intermediate obtained by separating a portion of the biuret polyisocyanate reaction liquid is added into an antioxidant premixing kettle together with the hindered phenol antioxidant for premixing, and then the premixed product is mixed with the remaining biuret polyisocyanate intermediate to obtain a biuret polyisocyanate composition product.

16. The preparation method according to claim 15, characterized in that: The materials added to the antioxidant premixing kettle include 99.5-90 wt % of the biuret polyisocyanate intermediate and 0.5-10 wt % of the hindered phenol antioxidant, based on the total mass of the materials.

17. The preparation method according to claim 15, characterized in that: The antioxidant premixing kettle is a kettle-type reactor containing a stirrer, and the reactor is equipped with a circulation pump and a circulation pipeline.

18. The preparation method according to claim 17, characterized in that: The hindered phenol antioxidant is added into the reactor through a venturi mixer arranged in the circulation line.

19. The preparation method according to claim 15, characterized in that: The temperature of the antioxidant premixing kettle is 60-90°C, and the residence time of the hindered phenol antioxidant and the biuret polyisocyanate intermediate in the kettle is 10-40 minutes; and / or, in the antioxidant premixing kettle, the material at the point where the hindered phenol antioxidant is added is in a turbulent state, and the Reynolds number is ≥5000; And / or, in the antioxidant premixing kettle, the stirring power received by the unit volume of the material is 3-10 KW / m3.

20. The preparation method according to claim 19, characterized in that: The temperature of the antioxidant premixing kettle is 70-80°C, and the residence time of the hindered phenol antioxidant and the biuret polyisocyanate intermediate in the kettle is 20-30 minutes; and / or, in the antioxidant premixing kettle, the material at the point where the hindered phenol antioxidant is added is in a turbulent state, and the Reynolds number is ≥6000; And / or, in the antioxidant premixing kettle, the stirring power received by the unit volume of the material is 5-8 KW / m3.