A sintering process for nano-silver conductive adhesive with low void ratio and high thermal conductivity
Through the sintering process of low cavities and high thermal conductivity nano-silver conductive glue, the problem of high cavities after sintering of nano-silver materials is solved, and the welding effect with high thermal conductivity is achieved, which simplifies operation and reduces costs. It is suitable for high reliability scenarios .
Patent Information
- Application Number
- CN202111439932.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-11-30
AI Technical Summary
When using nanosilver materials as thermal interface materials in the prior art, hollows are prone to occur after sintering, resulting in the failure to significantly improve thermal conductivity, and the welding process is complex and costly, making it difficult to apply in military products and high reliability scenarios.
Using the sintering process of low-altitude and high-thermal conduction nano-silver conductive glue, the nano-silver conductive glue is transferred to the carrier, the silicon wafer is mounted and the circle friction operation is performed, and then heated to 200°C in an electric blower drying box for 90 minutes. to achieve sintering.
The low cavity rate and high thermal conductivity of nano-silver conductive adhesives are achieved, the operation process is simplified, the cost is reduced, and the special temperature control equipment is eliminated or pressurized tooling is required, which protects the chip and significantly improves the welding quality.
Smart Images

Figure CN114361052B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrical equipment, and in particular to a sintering process of a low-voiding-rate and high-thermal-conductivity nano-silver conductive adhesive. Background Art
[0002] There are two main types of high-reliability welding for power chips: eutectic welding technology and nano-silver paste welding technology. Eutectic welding has the characteristics of low connection resistance and high welding strength, but this method has a high welding temperature and requires pressure to be applied during welding. In actual engineering production, it requires extremely high operating technology levels and is difficult. In addition, special tooling or instruments and equipment must be customized for chips of different types and sizes. The process is difficult and the cost is high. In addition, the thermal conductivity of traditional AuGe and AuSn eutectic solders is generally 40 to 50 W / mK, while the thermal conductivity of nano-silver can theoretically be as high as 200 W / mK or more, which can achieve low-temperature sintering. Therefore, nano-silver conductive adhesives that can be sintered at low temperatures and serve at high temperatures have become ideal thermal interface materials for chip welding, and have high application value in the field of high-power device assembly.
[0003] Nanosilver materials are currently used in certain consumer electronic products, but are rarely used in military products and other scenarios with high reliability requirements. On the one hand, when nanosilver materials are used as thermal interface materials, due to the residual voids inside after sintering, the actual thermal conductivity obtained does not show a significant advantage over the thermal conductivity of gold-tin solder after sintering. Summary of the invention
[0004] The present invention aims to provide a sintering process for a nano-silver conductive adhesive with low void ratio and high thermal conductivity, which can realize a chip assembled with the nano-silver conductive adhesive with low void ratio and high thermal conductivity.
[0005] To achieve the above object, the present invention is implemented by adopting the following technical solutions:
[0006] The present invention discloses a sintering process of a low-voiding-rate and high-thermal-conductivity nano-silver conductive adhesive, comprising the following steps:
[0007] a. Transfer printing, transferring the nano silver conductive glue to the carrier to form a covering area;
[0008] b. Mounting, mounting the silicon wafer on the cover area to prepare a sample, and performing a circular rubbing operation on the silicon wafer relative to the cover area during the mounting process;
[0009] c. Sintering: Place the sample in a heating device, heat it to 200±5°C, and maintain the temperature for 90±10 minutes.
[0010] Preferably, the coverage area is a continuous coverage area, and the area of the coverage area is 90% to 100% of the bottom area of the silicon wafer to be mounted.
[0011] Preferably, in step a, the nanosilver conductive glue is transferred to the carrier by a needle transfer method.
[0012] Furthermore, in step b, after the silicon wafer is rubbed in a circular motion relative to the covering area until the nanosilver conductive adhesive overflows from around the chip, a pressing force is applied to the silicon wafer relative to the carrier until the silicon wafer is flat.
[0013] Preferably, in step a, the nanosilver conductive paste is transferred to the carrier by a manual needle transfer method, the needle is a tungsten needle, and the circular rubbing operation and the application of pressing force are both performed manually.
[0014] Preferably, in step c, the heating device is an electric blast drying oven, and the sample is placed in the electric blast drying oven at room temperature, and taken out and cooled naturally after solidification.
[0015] Further preferably, in step c, the sample is cured at 200° C. for 90 min.
[0016] As a preferred embodiment, the carrier is a molybdenum-copper carrier plate.
[0017] Further preferably, the size of the silicon wafer is not greater than 3mm×3mm, and the carrier is a gold-plated / silver-plated molybdenum copper carrier, a gold-plated / silver-plated tungsten copper carrier, a gold-plated / silver-plated oxygen-free copper carrier, a gold-plated / silver-plated copper shell, or a gold-plated / silver-plated aluminum alloy cavity.
[0018] Furthermore, before step a, the nano silver conductive glue is taken out from the freezing environment and thawed for more than 1 hour.
[0019] The beneficial effects of the present invention are as follows:
[0020] 1. The present invention can achieve low void rate and high thermal conductivity of nano silver conductive adhesive assembled chips.
[0021] 2. The present invention does not require special temperature control equipment or setting of temperature gradient, and is simple to operate and easy to implement with low cost.
[0022] 3. The present invention adopts a circular friction method when placing the chip, and no special tooling is required for pressurization during subsequent sintering, which is beneficial to chip protection and cost saving. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a photo of the sample after glue was dispensed on 90% of the chip area in Example 1.
[0024] Figure 2 This is a photo of the sample after dispensing glue on 100% chip area in Example 2.
[0025] Figure 3 This is a photo of the sample after glue was dispensed on 95% of the chip area in Example 3.
[0026] Figure 4 This is an X-ray photograph of the sample after sintering in Example 1.
[0027] Figure 5 This is a photo of the sample in Comparative Example 1 after the sample was placed without rubbing in circles.
[0028] Figure 6 This is an X-ray photograph of the sample after sintering in Comparative Example 1.
[0029] Figure 7 This is an X-ray photograph of the sample after sintering in Comparative Example 2.
[0030] Figure 8 The (K) coefficient tests the fitted curve.
[0031] Fig. 9 It is a schematic diagram of the structure function curve of the thermal resistance test of the nanosilver mounted circuit and the thermal resistance treatment results.
[0032] Fig.10 Schematic diagram of the structure function of the dry contact between the gold-tin mounted circuit and the heat sink and the comparison.
[0033] Fig.11 Schematic diagram of the thermal resistance test structure of two circuits in dry contact. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings.
[0035] Example 1
[0036] Take out Kyocera CT2700R7 brand nano silver conductive adhesive from the freezer and thaw it for 1 hour for later use; of course, other nano silver conductive adhesives can also be used.
[0037] Fix the molybdenum-copper carrier in a sticky chip box, use a tungsten needle to dip the nanosilver conductive glue and transfer it to the molybdenum-copper carrier 2, use tweezers to pick up the silicon wafer and place it on the covered area of the molybdenum-copper carrier that has been dotted with nanosilver conductive glue, and rub it in circles. When the nanosilver conductive glue overflows around the silicon wafer, press it gently to make the silicon wafer flat and complete the placement. Among them, rubbing in circles refers to moving the silicon wafer circumferentially when the silicon wafer is in contact with the covered area.
[0038] The sample was placed in an electric blast drying oven at room temperature, and then the temperature of the electric blast drying oven was set to 200°C. After the temperature of the electric blast drying oven stabilized, the sample was kept warm and cured for 90 minutes. After the curing was completed, the sample was taken out and cooled naturally to complete the sintering of the nano-silver conductive adhesive.
[0039] Among them, the transfer of nano silver conductive glue is based on 90% of the silicon wafer area. Figure 1 As shown, it can be seen from the appearance that the nano silver conductive adhesive 3 can be seen overflowing around the chip 1 after it is placed, which meets the visual inspection acceptance standard in GJB548B-2005.
[0040] like Figure 4 As shown, there are scattered small voids within the chip, but no large voids that penetrate the chip. The failure mode of the shear test is silicon chip fragmentation, the interface is intact, and the test is qualified. The sintered sample can achieve a void rate of less than 10%, and the shear force is greater than the strength of the chip material.
[0041] After the temperature rises to 200℃, the sintering process of keeping warm for 90 minutes is suitable for assembling chips of 3mm*3mm and below to gold-plated / silver-plated molybdenum copper carriers, gold-plated / silver-plated tungsten copper carriers, gold-plated / silver-plated oxygen-free copper carriers, gold-plated / silver-plated copper shells, gold-plated / silver-plated aluminum alloy cavities, etc.
[0042] Example 2
[0043] The difference between this embodiment and embodiment 1 is that the nano silver conductive glue is transferred by dispensing according to 100% of the silicon wafer area; other operations are the same and will not be described in detail.
[0044] like Figure 2 As shown, in the appearance of this embodiment, nano silver conductive adhesive can be seen overflowing around the silicon wafer after placement, which meets the visual inspection acceptance standard in GJB548B-2005.
[0045] After sintering, the sample has scattered small voids within the chip range, but no large voids that penetrate through it. The failure mode of the shear test is silicon chip fragmentation, the interface is intact, and the test is qualified. The sintered sample can achieve a void rate of less than 10%, and the shear force is greater than the strength of the chip material.
[0046] Example 3
[0047] The difference between this embodiment and embodiments 1 and 2 is that the transfer of the nano silver conductive glue is performed by dispensing 95% of the silicon wafer area; other operations are the same and will not be described in detail.
[0048] like Figure 3 As shown, in the appearance of this embodiment, nano silver conductive adhesive can be seen overflowing around the silicon wafer after placement, which meets the visual inspection acceptance standard in GJB548B-2005.
[0049] After sintering, the sample has scattered small voids within the chip range, but no large voids that penetrate through it. The failure mode of the shear test is silicon chip fragmentation, the interface is intact, and the test is qualified. The sintered sample can achieve a void rate of less than 10%, and the shear force is greater than the strength of the chip material.
[0050] Comparative Example 1
[0051] Take out Kyocera CT2700R7 brand nanosilver conductive glue from the freezer and thaw for 1 hour. Fix the molybdenum copper carrier 2 in a sticky chip box, use a tungsten needle to dip the nanosilver conductive glue and transfer it to the molybdenum copper carrier, use tweezers to pick up the silicon wafer 1 and stick it to the area where the nanosilver conductive glue has been applied, and gently press the center position to make the silicon wafer flat and complete the placement. Place the sample in an electric blast drying oven at room temperature, then set the temperature of the electric blast drying oven to 200℃, and keep it warm and cure for 90 minutes after the temperature of the electric blast drying oven stabilizes. After the curing is completed, take out the sample and cool it naturally to complete the sintering of the nanosilver conductive glue.
[0052] Figure 5 This is a photo of the appearance of the patch after it was completed. It can be seen that the effect of nano silver conductive glue 3 overflowing all around can be achieved without friction, and the appearance inspection is qualified.
[0053] Figure 6 This is the X-ray morphology of the unfriction sample after sintering. It can be seen that there are a large number of voids in the picture, and their area is large. An obvious interface can be seen in the lower right corner, which is suspected to be not in contact with the nanosilver conductive glue.
[0054] Compared with Examples 1, 2, and 3, it can be seen that the circular friction placement technique can make the silicon wafer evenly stressed and fully contact the nano-silver conductive adhesive, which is beneficial to reducing voids and improving sintering quality.
[0055] Comparative Example 2
[0056] Take out the Kyocera CT2700R7 brand nanosilver conductive glue from the freezer and thaw it for 1 hour. Fix the molybdenum copper sheet in a sticky chip box, use a tungsten needle to dip the nanosilver conductive glue and transfer it to the molybdenum copper carrier, use tweezers to pick up the silicon wafer and stick it to the area where the nanosilver conductive glue has been applied, and rub it in circles. When the nanosilver conductive glue overflows around the silicon wafer, press it gently to make the silicon wafer flat and complete the placement. Set the electric hot air drying oven to 200℃ to heat it up. After the temperature stabilizes, place the sample in the electric hot air drying oven for 90 minutes of heat preservation and curing. After the curing is completed, take out the sample and cool it naturally to complete the sintering of the nanosilver conductive glue.
[0057] Figure 7 This is an X-ray photo of a sample that was directly cured and sintered at 200°C. It can be seen that there are large areas of voids in the middle of the silicon wafer and they are very concentrated. Figure 4 Compared with the sintering quality, the sintering quality is seriously reduced. Since the sample is placed in a 200℃ electric heating blast drying oven from room temperature, the sample heating rate is very fast, so the gas generated by the organic matter in the nano-silver conductive glue is not enough time to be discharged, thus forming a cavity in the middle.
[0058] Compared with Examples 1, 2, and 3, it can be seen that the sintering method of placing the sample in an electric blast drying oven at room temperature and allowing the sample to heat up with the furnace can reduce the heating rate of the sample and leave enough exhaust time, thereby reducing the void rate after sintering and improving the sintering quality.
[0059] Example 4
[0060] This example is a thermal resistance test report, which is as follows:
[0061] 1. Test requirements
[0062] Thermal resistance tests were conducted on nanosilver mounted circuits and gold-tin mounted circuits, and the thermal resistance of the mounting materials was stripped using the structure function.
[0063] 2. Test principle and test equipment
[0064] 2.1 Test Principle
[0065] Conducted according to JEDEC JESD51-1 and JESD51-14 thermal test standards.
[0066] 2.2 Test Equipment
[0067] T3ster2000 Thermal Resistance Tester.
[0068] 3. Circuit information
[0069] According to the input information table, the device power supply is reversely connected to the ground, and the parasitic diode formed is used as a temperature-sensitive diode. The device is powered forward to make it work and generate heat, and the parasitic diode is used in the reverse direction to measure the temperature. The forward voltage drop of the diode is used as a temperature-sensitive parameter (K coefficient).
[0070] 4. Temperature sensitivity coefficient (K coefficient) test
[0071] The power supply and ground of the device are reversed to act as a temperature-sensitive diode, and the forward voltage drop of the diode is used as the temperature-sensitive parameter (K coefficient).
[0072] 4.1 Test Environment
[0073] Use T3Ster dry-type temperature controller to provide a constant temperature environment. As shown in Figure 3 below, place the sample in a digital dry-type constant temperature bath. The temperature controller can control the temperature range of -25℃~125℃.
[0074] 4.2 Test parameters
[0075] Ambient temperature: 30℃~70℃, the diode forward voltage drop is collected every 10℃.
[0076] 4.3 Test Results
[0077] Figure 8 is the fitting curve of the test circuit K coefficient test. The temperature sensitivity coefficient (K) of the gold-tin mounted circuit is measured to be -1.4379mV / ℃, and the temperature sensitivity coefficient of the nano-silver mounted circuit is -1.4427mV / ℃.
[0078] 5. Thermal resistance test
[0079] 5.1 Test Method
[0080] According to JEDEC JESD51-14 structure function thermal resistance test method. First, the nanosilver chip circuit is tested twice, the first time in dry contact with the heat sink, and the second time in contact with the heat sink through thermal conductive silicone grease. The thermal resistance from the shell to the environment is obtained by comparing the structure function separation point. Then the gold-tin chip circuit is tested in dry contact with the heat sink, and the structure function of the nanosilver chip circuit in dry contact is compared to strip off the thermal resistance of the two chip materials.
[0081] 5.2 Test Results
[0082] The nanosilver chip circuit was tested for dry contact and silicone grease contact, with a test current of 0.6A. Fig. 9 As shown in the figure, the structure function obtained by dry contact test is blue, the structure function obtained by silicone contact is red, and the separation point is between the shell and the heat sink. Therefore, the thermal resistance after the separation point is the shell-to-ambient thermal resistance, and the thermal resistance before the separation point is the junction-to-shell thermal resistance. It can be seen from the figure that the thermal resistance from shell to environment is 0.7204℃ / W.
[0083] The AuSn chip mounted circuit and the heat sink dry contact were tested, and the structure function of the nanosilver chip mounted circuit dry contact was compared, as shown in Figure 10. Fig.11 shown.
[0084] Since the two circuit cases have the same size and the test heat sink size, it is assumed here that the thermal resistance from the two circuit cases to the environment is the same, both 0.7204℃ / W.
[0085] A1 and B1 are the contact interfaces between the chip and the mounting material (gold, tin or nanosilver); the thermal resistance before this point is the thermal resistance inside the chip, and the position of this point is determined by the obvious difference in slope after points A1 and B1.
[0086] A2 and B2 are the contact interfaces between the shell and the heat sink; this point is obtained by subtracting the shell-to-ambient thermal resistance 0.7204℃ / W from the final point of the structure function.
[0087] A3 and B3 are the contact interfaces between the mounting material and the housing. Since there is a certain difference in thermal conductivity between the mounting material and the heat sink, they present different slopes on the structure function. The position of this point is between A1 / B1 and A2 / B2.
[0088] The position of slope mutation is determined.
[0089] Therefore, after calculation, the thermal resistance of the gold-tin material between A1 and A3 is: 0.603+0.496+0.7204+0.555=2.3744℃ / W
[0090] The thermal resistance of nanosilver material is 0.603℃ / W between B1 and B3.
[0091] The above tests demonstrate the high thermal conductivity of nanosilver mounted circuits.
[0092] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims attached to the present invention.
Claims
1. A sintering process for low void ratio and high thermal conductivity nano silver conductive adhesive, characterized in that: The following steps are involved: a. Transfer printing, transferring the nano silver conductive glue to the carrier to form a covering area; b. Mounting, mounting the silicon wafer on the cover area to prepare a sample, and performing a circular rubbing operation on the silicon wafer relative to the cover area during the mounting process; c. Sintering: place the sample in a heating device, heat it to 200±5°C, and then maintain the temperature to cure for 90±10 minutes; The coverage area is a continuous coverage area, and the area of the coverage area is 90% to 100% of the bottom area of the silicon wafer to be mounted; In step a, the nano silver conductive paste is transferred to the carrier by a needle transfer method, the needle is a tungsten needle, and the circular rubbing operation and the application of pressing force are both performed manually; In step b, after the silicon wafer is rubbed in a circular motion relative to the covering area until the nanosilver conductive adhesive overflows from around the chip, a pressing force is applied to the silicon wafer relative to the carrier until the silicon wafer is flat; In step c, the heating device is an electric blast drying oven. The sample is placed in the electric blast drying oven at room temperature, taken out after curing and cooled naturally. The sample is cured at 200° C. for 90 minutes.
2. The sintering process of the low void ratio and high thermal conductivity nano silver conductive adhesive according to claim 1, characterized in that: The carrier is a molybdenum-copper carrier plate.
3. The sintering process of low void ratio and high thermal conductivity nano silver conductive adhesive according to claim 1, characterized in that: The size of the silicon wafer is no more than 3mm×3mm, and the carrier is a gold-plated / silver-plated molybdenum copper carrier, a gold-plated / silver-plated tungsten copper carrier, a gold-plated / silver-plated oxygen-free copper carrier, a gold-plated / silver-plated copper shell, or a gold-plated / silver-plated aluminum alloy cavity.
4. The sintering process of low void ratio and high thermal conductivity nano silver conductive adhesive according to any one of claims 1 to 3, characterized in that: Before step a, the nano silver conductive glue is taken out from the freezing environment and thawed for more than 1 hour.