Hard carbon material precursor, precarbonized product, hard carbon material and secondary battery, and preparation method and application thereof
Through Fuker alkylation reaction and pre-carbonization treatment, the problem of complex preparation methods and high energy consumption cost of hard carbon materials is solved, and hard carbon materials with excellent electrochemical properties are obtained. They are suitable for secondary battery electrodes and meet high capacity. Demand for low-cost negative electrode materials.
Patent Information
- Application Number
- CN202111627150.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-28
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-12-28
AI Technical Summary
The existing hard carbon material preparation methods are complex, have high energy consumption and insufficient electrochemical performance, making it difficult to meet the secondary battery industry's demand for high-capacity and low-cost negative electrode materials.
The raw polymer organic matter of the aryl hard carbon material containing raw materials is catalyzed by Lewis acid in halogenated hydrocarbons to prepare the hard carbon material precursor, and through pre-carbonization and carbonization treatment, hard carbon with excellent electrochemical properties is obtained. Material.
It realizes the preparation of hard carbon materials with simple and easy operation and low energy consumption. The resulting material has a stable structure and excellent electrochemical properties, making it suitable for use as a secondary battery electrode material.
Smart Images

Figure CN114361389B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a hard carbon material precursor, a hard carbon material pre-carbonized product, a hard carbon material and a secondary battery, as well as a preparation method and application of the hard carbon material. Background Art
[0002] In recent years, with the rise of the new energy industry, secondary batteries such as lithium-ion batteries and sodium-ion batteries have gradually entered the production and life of society. With the growing demand for high-quality, low-cost products, the secondary battery industry has also put forward higher requirements for the negative electrode materials of batteries. Research and development of high-capacity, low-cost negative electrode materials has become a hot topic in the secondary battery industry.
[0003] At present, the main commercial materials for secondary batteries are carbon materials with high structural stability and excellent electrochemical performance. Many researchers have carried out a series of research on carbon negative electrode materials. Graphite has become the main negative electrode material for lithium-ion batteries due to its small volume change, stable structure and stable cycle performance. However, commercial graphite negative electrodes have basically reached the theoretical capacity of lithium-ion batteries, 372mAh / g. The carbon layer spacing of graphite is small, which leads to its very low sodium storage capacity in sodium-ion batteries. In recent years, commercial graphite has been mainly artificial graphite. The graphitization process in the manufacturing process requires a lot of electricity, which greatly increases the manufacturing cost. The huge energy consumption is also obviously contrary to my country's policy of vigorously promoting carbon neutrality. Therefore, the development of new negative electrode materials has become an urgent need.
[0004] Hard carbon is a carbon material with a large interlayer spacing that facilitates the insertion and extraction of sodium ions. In addition, hard carbon has better lithium storage performance than graphite, so hard carbon materials can improve the performance of lithium-ion batteries and sodium-ion batteries compared to graphite materials. Most importantly, the preparation process of hard carbon does not require a high carbonization temperature like graphitization, so hard carbon consumes less energy and has lower cost than graphite, making it more suitable for industrialization.
[0005] At present, there have been reports on the application of hard carbon materials, but the existing hard carbon materials are still not ideal in terms of preparation process complexity, energy consumption cost, and electrochemical performance of products, and are in urgent need of improvement. Summary of the invention
[0006] In order to overcome the problems of the existing hard carbon material preparation method being complicated, high energy consumption cost, and insufficient electrochemical performance of the obtained battery product, the present invention provides a hard carbon material precursor, a hard carbon material pre-carbonized product, a hard carbon material and a secondary battery, and their preparation methods and applications of the hard carbon material. The preparation method of the present invention is simple and easy to operate, has low energy consumption cost, strong controllability, and the obtained hard carbon material has a stable structure and has excellent electrochemical performance as a secondary battery electrode material.
[0007] The present invention applies the Friedel-Crafts alkylation reaction to the preparation process of secondary battery electrode materials for the first time. It is unexpectedly found that not only is the method itself simple, low-cost, and highly controllable, but the prepared hard carbon material also exhibits excellent electrochemical properties as a secondary battery electrode material.
[0008] The present invention solves the above technical problems through the following technical solutions:
[0009] The invention provides a method for preparing a hard carbon material precursor, which comprises the following steps: in halogenated hydrocarbons, under the action of a Lewis acid catalyst, subjecting a raw material high molecular organic matter containing an aromatic hard carbon material to a Friedel-Crafts alkylation reaction to obtain the precursor.
[0010] The aromatic-containing hard carbon material raw material polymer organic matter is an aromatic-containing polymer organic matter suitable for preparing hard carbon materials, such as resin and / or asphalt, preferably selected from one or more of coumarone resin, epoxy resin, phenolic resin and mesophase asphalt.
[0011] The halogenated hydrocarbon participates in the Friedel-Crafts alkylation reaction and is also used as a solvent, preferably one or more of chloroform, carbon tetrachloride and dibromomethane. The amount of the halogenated hydrocarbon used can be based on the applicable amount of the solvent, specifically: the mass ratio of the raw material high molecular organic matter containing aromatic hard carbon material to the halogenated hydrocarbon can be 0.1-1, preferably 0.3-0.5.
[0012] The Lewis acid catalyst can be conventional in the art, preferably FeCl3 or AlCl3, more preferably AlCl3. The amount of the Lewis acid catalyst is a catalytically effective amount. Specifically, the mass ratio of the Lewis acid catalyst to the high molecular organic matter of the aromatic hard carbon material raw material can be 0.01-0.5, preferably 0.05-0.2.
[0013] The reaction temperature and time can be selected according to the conventional conditions of Friedel-Crafts alkylation reaction. The reaction temperature is preferably 30-80° C., more preferably 40-60° C. The reaction time can be 3-24 hours, more preferably 12-24 hours.
[0014] After the reaction is completed, post-treatment can be performed according to conventional methods, such as filtering, washing and drying in sequence.
[0015] The present invention also provides a hard carbon material precursor prepared by the preparation method of the hard carbon material precursor.
[0016] The present invention also provides a method for preparing a hard carbon pre-carbonized product, which comprises the following steps: subjecting the above hard carbon material precursor to a pre-carbonization treatment to obtain the hard carbon pre-carbonized product.
[0017] The method and conditions of the pre-carbonization can be selected according to the conventional methods in the art. The temperature of the pre-carbonization can be 300-700°C, preferably 400-600°C. The time of the pre-carbonization can be 1-8h, preferably 3-4h. The pre-carbonization can be carried out in a protective gas, such as nitrogen. The pre-carbonization equipment is preferably a pit furnace.
[0018] The present invention also provides a hard carbon pre-carbonized product prepared by the preparation method of the hard carbon pre-carbonized product.
[0019] The present invention also provides a method for preparing a hard carbon material, which comprises the following steps: carbonizing the hard carbon pre-carbonized product to obtain the hard carbon material.
[0020] The carbonization method and conditions can be selected according to the conventional methods in the art. The carbonization temperature can be 800-1200°C, preferably 1000-1200°C. The carbonization time can be 1-8h, preferably 3-4h. The carbonization can be carried out in a protective gas, such as nitrogen. The carbonization equipment is preferably a tubular furnace.
[0021] After the carbonization is completed, the hard carbon material may be crushed according to the conventional method in the art. The crushing method and conditions may be selected according to the conventional method in the art. The crushing may crush the particle size of the hard carbon material to 2-20 μm, preferably to 6-10 μm. The crushing equipment is preferably a jet mill.
[0022] The present invention also provides a hard carbon material prepared by the method for preparing the hard carbon material.
[0023] The present invention also provides the use of the hard carbon material in preparing secondary battery electrodes.
[0024] The present invention also provides a secondary battery, which comprises an electrode prepared from the hard carbon material.
[0025] Wherein, the secondary battery can be a lithium ion battery or a sodium ion battery. The electrode can be a positive electrode or a negative electrode.
[0026] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0027] The reagents and raw materials used in the present invention are commercially available.
[0028] The positive and progressive effects of the present invention are:
[0029] 1) The preparation method of the present invention has simple process and low energy consumption cost.
[0030] 2) The preparation method of the present invention can regulate the pore size and specific surface area of the product by changing the reaction conditions, and has good controllability.
[0031] 3) The hard carbon material of the present invention has a stable structure and has excellent electrochemical properties as a secondary battery electrical material. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is the XRD pattern of the hard carbon material prepared in Example 1. DETAILED DESCRIPTION
[0033] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0034] The asphalt and resin used in the examples were purchased from the following companies:
[0035] Coumarone resin: Puyang Xinde Petrochemical Co., Ltd.
[0036] Epoxy resin: Jinan Sunny Chemical
[0037] Mesophase asphalt: Suzhou Kaimei Chemical Co., Ltd.
[0038] Example 1
[0039] (1) Preparation of hard carbon material precursor
[0040] 50g of coumarone resin was dissolved in 100g of chloroform solution, and 5g of AlCl3 (the mass ratio of coumarone resin to chloroform was 0.5, and the mass ratio of AlCl3 to coumarone resin was 0.1) was added to the resulting solution, and stirred in a water bath at 60°C for 24h. After the reaction was completed, the generated precipitate was filtered, washed, and dried to obtain a hard carbon material precursor.
[0041] (2) Preparation of pre-carbonized hard carbon materials
[0042] The hard carbon material precursor obtained in step (1) is pre-carbonized in a pit furnace under nitrogen protection at a pre-carbonization temperature of 600° C. for 4 hours to obtain a pre-carbonized hard carbon material.
[0043] (3) Preparation of hard carbon materials
[0044] The pre-carbonized hard carbon material obtained in step (2) was carbonized in a tubular furnace under nitrogen protection at a carbonization temperature of 1000° C. for 4 hours. Thereafter, the carbonized hard carbon material was crushed in a jet mill to a particle size of 6 μm.
[0045] The XRD pattern of the obtained hard carbon material is shown in Figure 1 shown.
[0046] Example 2
[0047] The coumarone resin in Example 1 was replaced with epoxy resin, and other conditions and operations remained unchanged.
[0048] Example 3
[0049] The coumarone resin in Example 1 was replaced with mesophase asphalt, and other conditions and operations remained unchanged.
[0050] Example 4
[0051] The amount of coumarone resin in Example 1 is changed to 30 g (the mass ratio of coumarone resin to chloroform is 0.3, and the mass ratio of AlCl3 to coumarone resin is 0.17), and other conditions and operations remain unchanged.
[0052] Example 5
[0053] The amount of coumarone resin in Example 1 is changed to 100 g (the mass ratio of coumarone resin to chloroform is 1, and the mass ratio of AlCl3 to coumarone resin is 0.07), and other conditions and operations remain unchanged.
[0054] Example 6
[0055] The catalyst AlCl3 in Example 1 was replaced by FeCl3, and other conditions and operations remained unchanged.
[0056] Example 7
[0057] The amount of catalyst AlCl3 in Example 1 was changed to 10g (the mass ratio of AlCl3 to coumarone resin was 0.2), and other conditions and operations remained unchanged.
[0058] Example 8
[0059] The reaction temperature of (1) in Example 1 was changed to 40°C, while other conditions and operations remained unchanged.
[0060] Example 9
[0061] The reaction time of (1) in Example 1 was changed to 12 h, and other conditions and operations remained unchanged.
[0062] Example 10
[0063] The pre-carbonization temperature in (2) of Example 1 was changed to 400° C., and other conditions and operations remained unchanged.
[0064] Embodiment 11
[0065] The carbonization temperature in (3) of Example 1 was changed to 1200° C., while other conditions and operations remained unchanged.
[0066] Example 12
[0067] The pulverizing step (3) in Example 1 was controlled to pulverize the hard carbon material to a particle size of 10 μm, and other conditions and operations remained unchanged.
[0068] Example 13
[0069] The chloroform solution in Example 1 was replaced with dibromomethane, and other conditions and operations remained unchanged.
[0070] Embodiment 14
[0071] The amount of coumarone resin in Example 1 is changed to 10 g (the mass ratio of coumarone resin to chloroform is 0.1, and the mass ratio of AlCl3 to coumarone resin is 0.5), and other conditions and operations remain unchanged.
[0072] Embodiment 15
[0073] The reaction temperature in Example 1 was changed to 80° C., and other conditions and operations remained unchanged.
[0074] Example 16
[0075] The reaction time of (1) in Example 1 was changed to 3 h, and the other conditions and operations remained unchanged.
[0076] Embodiment 17
[0077] The pre-carbonization temperature in (2) of Example 1 was changed to 300° C., and other conditions and operations remained unchanged.
[0078] Embodiment 18
[0079] The carbonization temperature in (3) of Example 1 was changed to 800° C., while other conditions and operations remained unchanged.
[0080] Comparative Example 1
[0081] The coumarone resin is directly pre-carbonized and carbonized according to the operation and conditions of (2) and (3) in Example 1 to obtain a hard carbon material.
[0082] Effect Example
[0083] The electrochemical properties of the hard carbon materials prepared in Examples 1-12 and Comparative Example 1 were tested.
[0084] The test method is as follows:
[0085] 1. Specific surface area and pore size test
[0086] Test instrument: 3020 fully automatic specific surface area and pore size analysis tester from American Micromeritics.
[0087] Test conditions: CO2 purity is 99.9%, tested under liquid nitrogen (77.3K).
[0088] Pre-test treatment: The sample to be tested was vacuum degassed in a heating furnace at 100°C for 12 h.
[0089] 2. Lithium-ion battery testing
[0090] According to the mass ratio of hard carbon material: conductive agent: binder of 90:5:5, they were weighed and mixed, and then an appropriate amount of deionized water was added to make a slurry, which was coated on copper foil and dried in a vacuum drying oven for 12 hours to make a negative electrode sheet. The electrolyte was 1M LiPF6 / EC:DEC:DMC=1:1:1 (volume ratio), the polypropylene microporous membrane was used as the diaphragm, and the counter electrode was a lithium sheet, which was assembled into a battery. The constant current charge and discharge experiment was carried out in the LAND battery test system, with a charge and discharge voltage window of 0.01~2.0V and a charge and discharge rate of 0.1C.
[0091] 3. Sodium ion battery testing
[0092] The hard carbon material: conductive agent: binder were weighed and mixed at a mass ratio of 90:5:5, and then fully ground to obtain a viscous slurry. The slurry was then coated on a copper foil by a doctor blade method, dried at room temperature, and then the coated film was placed in a vacuum oven at 80°C and dried for 12 hours. The dried electrode film was taken out and punched into a circular electrode sheet with a diameter of about 1 cm. The batteries tested were all CR2016 button batteries, the electrolyte was 1M NaClO4 / EC+DEC, the prepared electrode material was used as the positive electrode, the metal sodium was used as the negative electrode, and the polypropylene microporous membrane (Celgard 2400) was used as the diaphragm. They were assembled into 2016 button batteries in a glove box filled with argon atmosphere. Then the LAND charge and discharge tester was used to perform the charge and discharge test.
[0093] The test results are shown in Table 1:
[0094] Table 1 Electrochemical properties of hard carbon materials of Examples 1 to 12 and Comparative Example 1
[0095]
[0096]
Claims
1. A method for preparing a hard carbon material, characterized in that: It includes the following steps: (1) Preparation of hard carbon material precursor Dissolve 50g of coumarone resin in 100g of chloroform solution, add 5g of AlCl3 to the resulting solution, the mass ratio of coumarone resin to chloroform is 0.5, and the mass ratio of AlCl3 to coumarone resin is 0.1; stir and react in a 60°C water bath for 24h; after the reaction is completed, filter, wash and dry the generated precipitate to obtain a hard carbon material precursor; (2) Preparation of pre-carbonized hard carbon materials The hard carbon material precursor obtained in step (1) is pre-carbonized in a pit furnace under nitrogen protection at a temperature of 600° C. for 4 hours to obtain a pre-carbonized hard carbon material; (3) Preparation of hard carbon materials The pre-carbonized hard carbon material obtained in step (2) is carbonized in a tubular furnace under nitrogen protection at a carbonization temperature of 1000° C. for 4 hours. Thereafter, the hard carbon material obtained by carbonization is crushed in a jet mill to a particle size of 6 μm.
2. A hard carbon material, characterized in that: The hard carbon material is prepared by the method for preparing the hard carbon material according to claim 1.
3. Use of the hard carbon material as claimed in claim 2 in the preparation of secondary battery electrodes.
4. A secondary battery, characterized in that: It comprises an electrode made from the hard carbon material according to claim 2.
5. The secondary battery according to claim 4, characterized in that: The secondary battery is a lithium ion battery or a sodium ion battery, and / or the electrode is a positive electrode or a negative electrode.
Citation Information
Cited By
Preparation system and method of battery hard carbon negative electrode material and sodium ion battery
CN119191276A
Preparation system, method of a hard carbon anode material for a battery and a sodium ion battery
CN119191276B