A polypropylene composition and preparation method thereof
By using polypropylene composition in the warm edge spacer of hollow glass, hyperbranched polymer and modified montmorillonite improve bonding performance and compatibility, the easy deformation, poor temperature resistance and difficulty in bonding of traditional materials is solved. Problem, direct bonding to metals, simplifying process and reducing costs are achieved.
Patent Information
- Application Number
- CN202111677705.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-31
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-12-31
AI Technical Summary
The traditional hollow glass warm edge spacer material is easy to deform, has poor temperature resistance, is expensive and cannot be directly bonded to metal aluminum strips, the process is complicated and costly.
A polypropylene composition is adopted, including 55-90 parts of polypropylene resin, 1-5 parts of hyperbranched polymer, 5-10 parts of toughening agent, 5-10 parts of compatible agent, 0-30 parts of modified molyde Soil and 0.5-1 part of antioxidant improve bonding properties and material compatibility through hyperbranched polymers, directly bond to metals, simplify the process and reduce costs.
It improves the toughness, bending modulus and bonding properties of the material, and can be directly bonded to metal without the need for additional tackifiers, simplifies the process and reduces costs, significantly improving the mechanical properties and bonding properties of the material.
Smart Images

Figure BDA0003452698160000061 
Figure BDA0003452698160000071 
Figure BDA0003452698160000072
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a polypropylene composition and a preparation method thereof. Background Art
[0002] With the development of industries such as construction, automobiles, decoration, furniture, and information industry technology, and the improvement of people's requirements for living space environment, functional processed products such as safety glass and energy-saving insulating glass have been widely used. Compared with single-layer glass, insulating glass has better insulation and heat preservation effects, and its application is increasing. The main materials of insulating glass include glass, spacers, desiccant, etc. Traditional spacers are mostly aluminum strips. Due to the low thermal conductivity of metal, it is easy to produce condensation, frost, and poor insulation effect. A new type of warm edge spacer has emerged. At present, most of these materials are PVC or PP. According to relevant literature and patents and feedback from various warm edge strip production companies, most of these materials are imported, easy to change, poor temperature resistance, expensive, and cannot be directly bonded to metal aluminum strips. It is necessary to add adhesives to bond with metals, but this process is relatively complicated and costly. Therefore, it is necessary to develop a material that can be bonded to metal aluminum strips, is easy to process, has excellent heat resistance, and is dimensionally stable. Summary of the invention
[0003] The purpose of the present invention is to provide a polypropylene composition and a preparation method thereof in view of the above-mentioned deficiencies in the prior art. The polypropylene composition of the present invention has good toughness, bending modulus and bonding performance.
[0004] To achieve the above purpose, the technical solution adopted by the present invention is as follows: a polypropylene composition comprises the following components in parts by weight: 55-90 parts of polypropylene resin, 1-5 parts of hyperbranched polymer, 5-10 parts of toughening agent, 5-10 parts of compatibilizer, 0-30 parts of modified montmorillonite, and 0.5-1 part of antioxidant.
[0005] Hyperbranched polymer is a star-shaped or dendrite-shaped polymer, which contains a large amount of active groups and has good bonding performance. The polypropylene composition of the present invention can improve the bonding performance of the material by adding hyperbranched polymer, and can be directly bonded to the metal during molding without adding an additional layer of tackifier material, which can simplify the process and save costs; on the other hand, it can improve the compatibility of montmorillonite and the matrix resin, and improve the toughness and rigidity of the material. In addition, as the content of the hyperbranched polymer increases, the toughness and peel strength of the material increase.
[0006] As a preferred embodiment of the present invention, the hyperbranched polymer is at least one of hyperbranched polyethyleneimine, hyperbranched polyester, hyperbranched unsaturated resin and hyperbranched epoxy resin.
[0007] The hyperbranched polymer molecular chain of the present invention contains more polar functional groups, such as amine, amide, ester, unsaturated group or epoxy group, has good compatibility with resin and filler, and improves the overall material properties, such as mechanical properties, processing properties, adhesion, etc.
[0008] As a preferred embodiment of the present invention, the branching degree of the hyperbranched polymer is 0.5-0.7.
[0009] The degree of branching of the hyperbranched polymer affects the mechanical properties and adhesive properties of the polypropylene composition. As the degree of branching of the hyperbranched polymer increases, the impact strength and adhesive properties of the polypropylene composition are enhanced, and the flexural modulus decreases slightly. However, if the degree of branching of the hyperbranched polymer is too high, the compatibility of the hyperbranched polymer with polypropylene deteriorates, which will reduce the mechanical properties and adhesive properties of the material.
[0010] As a preferred embodiment of the present invention, the modified montmorillonite is a montmorillonite whose surface is acid-modified and / or quaternary ammonium salt-modified; the D50 particle size of the modified montmorillonite is 2-5 μm; more preferably, the modified montmorillonite is a montmorillonite whose surface is acid-modified and quaternary ammonium salt-modified.
[0011] Montmorillonite is a highly polar lamellar silicate. After being treated with acid, its polar bonds are passivated, its specific surface area and pore size are increased. At the same time, after being treated with quaternary ammonium salt, it not only enhances its adsorption and bonding properties, but also improves its compatibility with resins. Compared with unmodified montmorillonite, the mechanical properties and bonding properties with metals of the polypropylene composition prepared by modified montmorillonite are significantly enhanced.
[0012] As a preferred embodiment of the present invention, the polypropylene resin has a melt flow rate of 1-5 g / 10 min under the test conditions of 230° C. and 2.16 kg according to the test standard ISO1133-1-2011.
[0013] The present invention selects polypropylene resin with low melt flow rate, which is beneficial to material extrusion molding and can avoid the unstable molding caused by low viscosity of polypropylene and high melt flow performance.
[0014] As a preferred embodiment of the present invention, the toughening agent is at least one of POE, EVA, acrylic elastomer, and EPDM; the toughening agent has a melt flow rate of 0.5-5 g / 10 min under the test conditions of 190° C. and 2.16 kg according to the test standard ISO 1133-1-2011.
[0015] As a preferred embodiment of the present invention, the compatibilizer is polypropylene grafted with maleic anhydride.
[0016] As a preferred embodiment of the present invention, the antioxidant is a mixture of antioxidant 1010 and antioxidant 168; the mass ratio of the antioxidant 1010 to the antioxidant 168 is 1:(1-2).
[0017] In addition, the present invention also claims a method for preparing the polypropylene composition, comprising the following steps:
[0018] (1) uniformly mixing a hyperbranched polymer, modified montmorillonite and a compatibilizer, and then melt-extruding and granulating the mixture to obtain a mixture;
[0019] (2) The mixture, the polypropylene resin, the toughening agent and the antioxidant are mixed, melt-extruded and granulated to obtain the polypropylene composition.
[0020] As a preferred embodiment of the present invention, in the step (2), the device for melt extrusion and granulation is a twin-screw extruder, the extrusion temperature of the twin-screw extruder is 180-210°C, the aspect ratio is (38-42):1, and the rotation speed is 300-500rpm.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) The present invention utilizes the good adhesive properties of the hyperbranched polymer. The hyperbranched polymer is added to the polypropylene composition. On the one hand, the adhesive properties of the material can be improved, and it can be directly bonded to the metal during molding without adding an additional layer of tackifier material, thereby simplifying the process and saving costs. On the other hand, the compatibility of the filler and the matrix resin can be improved, and the toughness and rigidity of the material can be increased.
[0023] (2) In addition, the present invention uses modified montmorillonite to improve the compatibility of montmorillonite with resin, thereby improving the mechanical properties of the polypropylene composition and at the same time improving the bonding performance with metal. DETAILED DESCRIPTION
[0024] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0025] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. Unless otherwise specified, the reagents and materials used in the present invention are commercially available.
[0026] The following raw materials are used in the examples and comparative examples of the present invention:
[0027] Polypropylene A: melt flow rate tested at 230°C and 2.16 kg is 3 g / 10 min, brand: PP K8003, purchased from Maoming Petrochemical;
[0028] Polypropylene B: melt flow rate tested at 230°C and 2.16 kg is 1 g / 10 min, brand: PP EPS30R, purchased from Maoming Petrochemical;
[0029] Polypropylene C: melt flow rate tested at 230°C and 2.16 kg is 5 g / 10 min, brand: PP K1005, purchased from Yanshan Petrochemical;
[0030] Toughener A: POE, melt flow rate tested at 190°C and 2.16 kg is 5 g / 10 min, brand: POE7447, purchased from DOW;
[0031] Toughener B: POE, with a melt flow rate of 0.5 g / 10 min at 190°C and 2.16 kg, brand: POE8150, purchased from DOW;
[0032] Toughening agent C: POE, the melt flow rate tested at 190°C and 2.16 kg is 6 g / 10 min, brand: POELC610, purchased from LG;
[0033] Hyperbranched polymer A: hyperbranched polyester, branching degree 0.5, brand: Hyper H102, purchased from Wuhan Hyperbranched;
[0034] Hyperbranched polymer B: hyperbranched polyester, branching degree 0.6, brand: Hyper H103, purchased from Wuhan Hyperbranched;
[0035] Hyperbranched polymer C: hyperbranched polyester, branching degree 0.7, brand: Hyper H104, purchased from Wuhan Hyperbranched;
[0036] Hyperbranched polymer D: hyperbranched polyester, branching degree 0.4, brand: Hyper H101, purchased from Wuhan Hyperbranching;
[0037] Hyperbranched polymer E: hyperbranched polyester, branching degree 0.75, brand: Hyper H105, purchased from Wuhan Hyperbranching;
[0038] Modified montmorillonite A: montmorillonite with surface acidification and quaternary ammonium salt modification, D50 is 3um, brand: DK4-D, purchased from Zhejiang Fenghong;
[0039] Modified montmorillonite B: montmorillonite with surface modified by acidification, D50 is 3um, brand: DK4-S, purchased from Zhejiang Fenghong;
[0040] Modified montmorillonite C: montmorillonite with surface modified by quaternary ammonium salt, D50 is 3um, brand: DK4-Y, purchased from Zhejiang Fenghong;
[0041] Montmorillonite D: unmodified, D50 is 3um, brand: DK4-1, purchased from Zhejiang Fenghong;
[0042] Compatibilizer: polypropylene grafted maleic anhydride, commercially available, the same compatibilizer is used in both the examples of the present invention and the comparative examples;
[0043] Antioxidant: a mixture of antioxidant 1010 and antioxidant 168, with a mass ratio of 1:1. The same antioxidant is used in both the examples of the present invention and the comparative examples.
[0044] Examples 1 to 14 and Comparative Examples 1 to 5
[0045] The components of the polypropylene compositions of Examples 1 to 14 of the present invention are shown in Table 1, and the components of the polypropylene compositions of Comparative Examples 1 to 5 are shown in Table 2.
[0046] The preparation method of the polypropylene composition described in Examples 1 to 9, 11 to 14 and Comparative Examples 2 to 4 of the present invention is:
[0047] (1) uniformly mixing a hyperbranched polymer, modified montmorillonite and a compatibilizer, and then melt-extruding and granulating the mixture to obtain a mixture;
[0048] (2) adding the mixture, polypropylene resin, toughening agent and antioxidant into a twin-screw extruder for mixing, melt extruding and granulating to obtain the polypropylene composition; the extrusion temperature of the twin-screw extruder is 180-210° C., the aspect ratio is 40:1, and the rotation speed is 300-500 rpm.
[0049] The preparation method of the polypropylene composition described in Example 10 of the present invention is:
[0050] (1) uniformly mixing the hyperbranched polymer and the compatibilizer, and then melt-extruding and granulating the mixture;
[0051] (2) adding the mixture, polypropylene resin, toughening agent and antioxidant into a twin-screw extruder for mixing, melt extruding and granulating to obtain the polypropylene composition; the extrusion temperature of the twin-screw extruder is 180-210°C.
[0052] The preparation method of the polypropylene composition described in Comparative Example 1 of the present invention is:
[0053] (1) uniformly mixing the modified montmorillonite and the compatibilizer, and then melt-extruding and granulating the mixture;
[0054] (2) adding the mixture, polypropylene resin, toughening agent and antioxidant into a twin-screw extruder for mixing, melt extruding and granulating to obtain the polypropylene composition; the extrusion temperature of the twin-screw extruder is 180-210°C.
[0055] The preparation method of the polypropylene composition described in Comparative Example 5 of the present invention is:
[0056] (1) uniformly mixing a hyperbranched polymer, unmodified montmorillonite and a compatibilizer, and then melt-extruding and granulating the mixture to obtain a mixture;
[0057] (2) adding the mixture, polypropylene resin, toughening agent and antioxidant into a twin-screw extruder for mixing, melt extruding and granulating to obtain the polypropylene composition; the extrusion temperature of the twin-screw extruder is 180-210°C.
[0058] Table 1
[0059]
[0060]
[0061] Table 2
[0062]
[0063] Effect example
[0064] The properties of the polypropylene compositions prepared in the examples and comparative examples were tested, and the specific test items and test methods are as follows:
[0065] (1) Izod impact strength: tested in accordance with GB / T 1843-2008;
[0066] (2) Flexural modulus: tested according to standard GB / T 9341-2008;
[0067] (3) Peel strength: Tested according to GB / T 2792-2014.
[0068] The performance test results of the polypropylene compositions described in Examples 1-14 and Comparative Examples 1-5 are shown in Table 3.
[0069] Table 3
[0070]
[0071] According to the data of Table 3, the Izod impact strength and peel strength of the polypropylene composition described in Examples 1-14 are much higher than those prepared by Comparative Examples 1-5. According to Examples 1-3, as the amount of hyperbranched polymer added increases, the Izod impact strength, flexural modulus and adhesive properties of the material increase; but according to the comparison between Comparative Examples 1-3 and Examples 1-3, it can be seen that the addition of hyperbranched polymers in the present invention can enhance the Izod impact strength, flexural modulus and adhesive properties of the material, but when the amount of hyperbranched polymer added is not within the scope of the present invention, the Izod impact strength, flexural modulus and adhesive properties of the material decrease. According to the data of Examples 2, 4-7, as the degree of branching of the hyperbranched polymer increases, the Izod impact strength, flexural modulus and adhesive properties of the material first increase and then decrease, and in the range of 0.5-0.7 of the degree of branching, the performance of the material is the best. According to the data of Examples 2, 8-9 and Comparative Example 5, compared with unmodified montmorillonite, modified montmorillonite can significantly enhance the mechanical properties and bonding properties of the material, and the montmorillonite with surface acidification modification and quaternary ammonium salt modification has the most obvious improvement on the performance of the material. According to the data of Examples 2, 10-12, as the amount of modified montmorillonite added increases, the cantilever beam impact strength, bending modulus and bonding properties of the material increase, but when the amount added exceeds the limited range of the present invention, the cantilever beam impact strength and bonding properties of the material are significantly reduced.
[0072] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A polypropylene composition, It is characterized in that The polypropylene composition comprises the following components in parts by weight: 55-90 parts of polypropylene resin, 1-5 parts of hyperbranched polymer, 5-10 parts of toughening agent, 5-10 parts of compatibilizer, 10-30 parts of modified montmorillonite, and 0.5-1 part of antioxidant; The hyperbranched polymer is a hyperbranched polyester, and the branching degree of the hyperbranched polymer is 0.5-0.7; The modified montmorillonite is a montmorillonite whose surface is modified by acidification, and the D50 particle size of the modified montmorillonite is 2-5 μm.
2. The polypropylene composition according to claim 1, It is characterized in that The polypropylene resin has a melt flow rate of 1-5 g / 10 min under the test conditions of 230° C. and 2.16 kg.
3. The polypropylene composition according to claim 1, It is characterized in that The toughening agent is at least one of POE, EVA, acrylic elastomer and EPDM; the toughening agent has a melt flow rate of 0.5-5 g / 10 min under the test conditions of 190° C. and 2.16 kg.
4. The polypropylene composition according to claim 1, It is characterized in that The compatibilizer is polypropylene grafted with maleic anhydride.
5. The polypropylene composition according to claim 1, It is characterized in that The antioxidant is a mixture of antioxidant 1010 and antioxidant 168.
6. A method for preparing a polypropylene composition according to any one of claims 1 to 5, It is characterized in that The steps include: (1) uniformly mixing a hyperbranched polymer, modified montmorillonite and a compatibilizer, and then melt-extruding and granulating the mixture to obtain a mixture; (2) The mixture, the polypropylene resin, the toughening agent and the antioxidant are mixed, melt-extruded and granulated to obtain the polypropylene composition.
7. The method for preparing the polypropylene composition according to claim 6, It is characterized in that In the step (2), the device for melt extrusion and granulation is a twin-screw extruder, and the extrusion temperature of the twin-screw extruder is 180-210°C.