Positive electrode active material for lithium ion secondary battery and lithium ion secondary battery
By using specially prepared lithium-containing transition metal composite oxide particles in lithium-ion secondary batteries, the problem of insufficient output characteristics and mechanical strength of the positive electrode active material is solved, higher battery capacity and cycle characteristics are achieved, and it is suitable for high energy density and high-output electric vehicle power supplies.
Patent Information
- Application Number
- CN202080066186.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-09-18
AI Technical Summary
The output characteristics and mechanical strength of the cathode active material of existing lithium-ion secondary batteries are insufficient, resulting in poor battery capacity and cycle characteristics, especially high internal resistance in electric vehicle applications.
The cathode active material composed of lithium-containing transition metal composite oxide particles is used. By controlling the particle size, particle size distribution and multi-layer structure, the mechanical strength is improved and the reaction area with the electrolyte is increased, specifically including the use of Li1+uNixMnyCozMtO2. Secondary particles are formed by agglomeration of primary particles into, having a 50% cumulative diameter between 3.0μm and 7.0μm, a BET specific surface area between 2.0m2/g and 5.0m2/g, a tap density between 1.0g/cm3 and 2.0g/cm3, and passing STEM-EDX analysis ensures concentration uniformity of added elements.
It significantly improves the output characteristics and mechanical strength of lithium-ion secondary batteries, enhances the capacity and cycle characteristics of the battery, and is suitable for high energy density and high output electric vehicle power supplies.
Smart Images

Figure CN114424367B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a positive electrode active material for a lithium ion secondary battery composed of a composite oxide containing a lithium transition metal, and a lithium ion secondary battery using the positive electrode active material for a lithium ion secondary battery as a positive electrode material. Background Art
[0002] In recent years, with the popularity of portable electronic devices such as smart phones, tablet terminals, digital cameras, and notebook computers, there is a strong desire to develop small and lightweight secondary batteries with high energy density. In addition, there is a strong desire to develop high-capacity and high-output secondary batteries as power sources for electric vehicles such as hybrid electric vehicles, plug-in hybrid electric vehicles, and battery-type electric vehicles.
[0003] As a secondary battery that meets the above requirements, there is a lithium ion secondary battery. The lithium ion secondary battery is composed of a negative electrode, a positive electrode, a non-aqueous electrolyte or a solid electrolyte, etc., and a material that can remove and insert lithium is used in the active material used as the material of its negative electrode and positive electrode. It should be noted that as a non-aqueous electrolyte, there is a non-aqueous electrolyte prepared by dissolving a lithium salt as a supporting salt in an organic solvent, and as a solid electrolyte, there is an inorganic or organic solid electrolyte that is non-flammable and has lithium ion conductivity.
[0004] Among lithium-ion secondary batteries, lithium-ion secondary batteries that use lithium-containing transition metal composite oxides with a layered rock salt type or spinel type crystal structure as the positive electrode material can obtain a voltage of 4V, so as to be a battery with high energy density, research and development and practical application are currently underway.
[0005] As positive electrode materials for lithium-ion secondary batteries, lithium cobalt composite oxide (LiCoO2), which is relatively easy to synthesize, lithium nickel composite oxide (LiNiO2), which uses nickel that is cheaper than cobalt, and lithium nickel manganese cobalt composite oxide (LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2), lithium manganese composite oxide (LiMn2O4), lithium nickel manganese composite oxide (LiNi 0.5 Mn 0.5 The positive electrode active material is composed of a composite oxide containing lithium transition metals such as O2).
[0006] In recent years, among these lithium-containing transition metal composite oxides, lithium nickel manganese cobalt composite oxide (LiNi 1 / 3 Mn 1 / 3 Co 1 / 3The ternary positive electrode active material composed of a composite oxide (NMC) containing lithium nickel manganese cobalt, including lithium cobalt oxide (NMC) and containing at least nickel, manganese and cobalt as transition metals, has attracted attention as a material with excellent thermal stability, high capacity, good cycle characteristics of battery capacity, low resistance and high output. The composite oxide containing lithium nickel manganese cobalt is a compound having a layered rock salt type crystal structure, similar to lithium cobalt composite oxide and lithium nickel composite oxide.
[0007] The development of lithium-containing transition metal composite oxides focuses on achieving high output by reducing internal resistance. In particular, in the application of power sources for electric vehicles, there is a high level of demand for high output by further reducing internal resistance.
[0008] In order to improve the output characteristics and cycle characteristics of the positive electrode active material composed of composite oxides containing lithium transition metals such as composite oxides containing lithium nickel and composite oxides containing lithium nickel manganese cobalt, it is important to use particles with a small particle size and a narrow particle size distribution. The specific surface area of particles with a small particle size is large. When used as a positive electrode active material, the reaction area with the electrolyte can be fully ensured. Furthermore, the positive electrode can be formed thinner and the movement distance of lithium ions between the positive electrode and the negative electrode can be shortened. Therefore, by setting the particles to have a small particle size, the positive electrode resistance can be reduced. In addition, by using particles with a narrow particle size distribution, the voltage applied to the particles in the electrode can be uniformized, so the reduction in battery capacity caused by the selective degradation of the particles can be suppressed.
[0009] In order to further improve the output characteristics, the improvement of the particle structure of the composite oxide containing lithium transition metals is also studied and developed. For example, in order to improve the output characteristics, it is considered effective to form a space portion inside the positive electrode active material into which the electrolyte can invade. By adopting such a structure, the reaction area with the electrolyte can be increased compared to the positive electrode active material of a solid structure with the same particle size, so the positive electrode resistance can be significantly reduced. In addition, it is known that the positive electrode active material will continue the particle properties of the composite hydroxide containing transition metals as its precursor. That is, in order to obtain a positive electrode active material with a space portion, it is necessary to appropriately control the particle size, particle size distribution and particle structure of the secondary particles of the composite hydroxide containing transition metals as its precursor.
[0010] For example, Japanese Patent Publication No. 2012-246199 and WO2012 / 131881 disclose a method for manufacturing composite hydroxide particles containing transition metals as a precursor of a positive electrode active material by a crystallization reaction clearly divided into a nucleation process for mainly performing nucleation and a particle growth process for mainly performing particle growth. In these methods, by appropriately adjusting the pH value and reaction environment in the nucleation process and the particle growth process, composite hydroxide particles containing transition metals having a small particle size and a narrow particle size distribution, a low-density center portion and a high-density shell portion are obtained, the center portion is composed of fine primary particles, and the shell portion is composed of plate-like or needle-like primary particles. The positive electrode active material obtained from such composite hydroxide particles has a hollow structure, and the contact area with the electrolyte is increased, which can improve the output characteristics.
[0011] In the WO2014 / 181891 Gazette and the Japanese Patent Publication No. 2018-104276, a method for producing composite hydroxide particles containing transition metals is disclosed, which is characterized in that it includes: a nucleation process, in which the pH value of the nucleation aqueous solution containing a metal compound and an ammonium ion donor is controlled to be greater than 12.0 and less than 14.0 to perform nucleation, and the metal compound contains at least a transition metal; and a particle growth process, in which the pH value of the particle growth aqueous solution containing the generated nuclei is controlled to be lower than the pH value of the nucleation process and greater than 10.5 and less than 12.0 to allow it to grow, the initial stages of the nucleation process and the particle growth process are set to a non-oxidizing environment, and at least one environmental control is performed, and the environmental control is switched to an oxidizing environment at a specified time in the particle growth process and then switched to a non-oxidizing environment again. According to this method, it is possible to obtain transition metal-containing composite hydroxide particles having a small particle size and a narrow particle size distribution, and having a central portion formed by agglomeration of plate-like or needle-like primary particles. The transition metal-containing composite hydroxide particles have two stacked structures on the outside of the central portion, and the stacked structure is a stacked structure in which a low-density layer formed by agglomeration of fine primary particles and a high-density layer formed by agglomeration of plate-like primary particles are alternately stacked.
[0012] The positive electrode active material using these transition metal-containing composite hydroxide particles as precursors has a small particle size, a narrow particle size distribution, and a multilayer structure having a hollow structure or a space portion. Therefore, the secondary battery using these positive electrode active materials can simultaneously improve the battery capacity, output characteristics, and cycle characteristics.
[0013] Prior art literature
[0014] Patent Literature
[0015] Patent Document 1: Japanese Patent Application Publication No. 2012-246199
[0016] Patent Document 2: WO2012 / 131881
[0017] Patent Document 3: WO2014 / 181891
[0018] Patent Document 4: Japanese Patent Application Publication No. 2018-104276 Summary of the invention
[0019] Problem that the invention aims to solve
[0020] However, since the output characteristics of the positive electrode active materials described in these documents have room for improvement, further improvement of the output characteristics is required.
[0021] In addition, compared with the secondary particles with dense structure, the mechanical strength of the secondary particles with multilayer structure having hollow structure or space portion is small. When the positive electrode active material is compressed, rolled or other forces are applied in the battery manufacturing process, the secondary particles collapse and sometimes their internal structure is damaged. If the internal structure of the secondary particles is damaged, it is possible that the battery capacity, output characteristics and cycle characteristics expected for the positive electrode active material cannot be obtained.
[0022] Therefore, the present invention relates to a positive electrode active material which can contribute to improving output characteristics and is composed of secondary particles having a hollow structure or a multilayer structure with space portions, and its object is to further improve its output characteristics and enhance its mechanical strength.
[0023] Means used to solve problems
[0024] A positive electrode active material for a lithium ion secondary battery according to one embodiment of the present invention is composed of composite oxide particles containing lithium transition metals.
[0025] The lithium transition metal-containing composite oxide particles have a general formula (A): Li 1+u Ni x Mn y Co z M t O2 (wherein, -0.05≤u≤0.5, x+y+z+t=1, 0.3≤x≤0.9, 0≤y≤0.5, 0≤z≤0.5, 0<t≤0.05, M is one or more additive elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta and W) and a layered rock salt type crystal structure,
[0026] The lithium-transition metal-containing composite oxide particles are composed of secondary particles, which are formed by agglomeration of primary particles.
[0027] The secondary particles have: a 50% cumulative diameter d50 of 3.0 μm or more and 7.0 μm or less, as determined from a particle size distribution measurement value; 2.0 μm or less 2 / g or more and 5.0m 2 / g or less BET specific surface area; 1.0g / cm 3 Above and 2.0g / cm 3 A tap density of 30 mL / 100 g or more and 60 mL / 100 g or less; and an oil absorption of 30 mL / 100 g or more and 60 mL / 100 g or less,
[0028] Among the primary particles, for a plurality of primary particles having a primary particle size within the range of greater than 0.1 μm and less than 1.0 μm, when the concentration of the added element M is measured at a plurality of locations and the coefficient of variation of the concentration of the added element M is calculated by cross-sectional STEM or TEM-EDX analysis, the coefficient of variation is less than 1.5, and the coefficient of variation is a value obtained by dividing the standard deviation of the concentration of the added element M by the average concentration of the added element M.
[0029] The total volume of the connecting parts between the primary particles in the binary image and the number of the primary particles in the binary image are determined using a watershed algorithm based on a binary image obtained by binarizing the three-dimensional observation image of the secondary particles. The volume of the connecting part of each primary particle obtained based on the total volume of the connecting parts between the primary particles in the binary image and the number of the primary particles in the binary image is preferably 5×10 5 nm 3 Above and 9×10 7 nm 3 The volume of the connecting portion per primary particle is more preferably 8×10 5 nm 3 Above and 9×10 6 nm 3 the following.
[0030] The volume of the connecting part of each of the primary particles can be calculated by the following evaluation method, which includes: (a) a process of obtaining a binary image based on the three-dimensional observation image of the secondary particles; (b) a process of determining the connecting parts between the primary particles and the number of the primary particles by a watershed algorithm based on the obtained binary image; and (c) a process of calculating the volume of the connecting part of each of the primary particles.
[0031] The 50% cumulative diameter d50 of the secondary particles is preferably 4.0 μm or more and 6.0 μm or less.
[0032] [(d90-d10) / d50] (where d10 is the 10% cumulative diameter obtained from the particle size distribution measurement value, and d90 is the 90% cumulative diameter obtained from the particle size distribution measurement value) which is an indicator of the width of the particle size distribution of the secondary particles is preferably less than 1.0.
[0033] The value of d90 / d10 of the secondary particles is preferably 1.0 or more and 2.0 or less.
[0034] Preferably, the secondary particle has: an agglomeration portion; one or more communicating holes connecting the periphery of the agglomeration portion; and two or more space portions existing inside the agglomeration portion and connecting to the communicating holes. The number of the communicating holes is preferably two or more. Preferably, the two or more space portions are connected to the connecting holes or other space portions.
[0035] The additional element M is preferably one or more selected from Mg, Al, Si, Ti, Zr, Nb, Mo, and W. The additional element M is preferably W.
[0036] A lithium-ion secondary battery according to one embodiment of the present invention is characterized in that it has a positive electrode, a negative electrode, a separator and a non-aqueous electrolyte (non-aqueous electrolyte secondary battery), or has a positive electrode, a negative electrode and a solid electrolyte (solid electrolyte secondary battery), and as the positive electrode active material for the positive electrode, the positive electrode active material for the lithium-ion secondary battery according to the embodiment of the present invention is used.
[0037] Effects of the Invention
[0038] For the positive electrode active material for lithium ion secondary batteries of one embodiment of the present invention, since a sufficiently large mechanical strength can be obtained and the contact area with the non-aqueous electrolyte or solid electrolyte is sufficiently large, the insertion and extraction of lithium ions at the particle interface are promoted, and its output characteristics can be improved. Therefore, the lithium ion secondary battery using the positive electrode active material for lithium ion secondary batteries of one embodiment of the present invention can provide high output characteristics, and thus its industrial significance is very large. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a SEM photograph of a cross section of secondary particles constituting the positive electrode active material for a lithium ion secondary battery of Example 1.
[0040] Figure 2 The cross-sectional data show the measurement results of the W concentration of the primary particles constituting the positive electrode active material for lithium ion secondary batteries of Example 1 by TEM-EDX analysis.
[0041] Figure 3 (a)~ Figure 3(c) is a conceptual diagram for explaining a means for obtaining the volume of the connecting portion of each primary particle. Figure 3 (a) is the binary image before primary particle separation. Figure 3 (b) is the binary image after primary particle separation. Figure 3 (c) is a binary image of the connection between primary particles.
[0042] Figure 4 This is a SEM photograph of a cross section of secondary particles constituting the positive electrode active material for a lithium ion secondary battery of Comparative Example 1.
[0043] Figure 5 This is a schematic cross-sectional view of a 2032-type coin-shaped battery used in battery evaluation.
[0044] Figure 6 It is a figure which shows the measurement example of impedance evaluation.
[0045] Figure 7 This is a schematic diagram of the equivalent circuit used for analysis. DETAILED DESCRIPTION
[0046] 1. Positive electrode active material for lithium-ion secondary batteries
[0047] A positive electrode active material for a lithium ion secondary battery (hereinafter referred to as “positive electrode active material”) according to one embodiment of the present invention is characterized in that it is composed of composite oxide particles containing lithium transition metals (hereinafter referred to as “composite oxide particles”) and has the following requirements (1) to (7).
[0048] (1) Composition
[0049] The composite oxide particles have the general formula (A): Li 1+u Ni x Mn y Co z M t O2 (wherein, -0.05≤u≤0.5, x+y+z+t=1, 0.3≤x≤0.9, 0≤y≤0.5, 0≤z≤0.5, 0<t≤0.05, and M is one or more additional elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta and W).
[0050] In the positive electrode active material of the present embodiment, the value of u representing the excess amount of lithium (Li) is greater than -0.05 and less than 0.5. Preferably, it is greater than 0 and less than 0.50, and more preferably greater than 0 and less than 0.35. By limiting the value of u to the above range, the output characteristics and battery capacity of a lithium ion secondary battery using the positive electrode active material as a positive electrode material can be improved. In contrast, when the value of u is less than -0.05, the positive electrode resistance of the secondary battery increases, and therefore, it is possible that the output characteristics cannot be improved. When the value of u is greater than 0.5, not only the initial discharge capacity is reduced, but also the positive electrode resistance is likely to increase.
[0051] Nickel (Ni) is an element that contributes to the high potential and high capacity of secondary batteries, and the value of x representing its content is 0.3 or more and 0.9 or less. Preferably, it is 0.4 or more and 0.7 or less, more preferably 0.4 or more and 0.6 or less. When the value of x is less than 0.3, it is possible that the energy density of the secondary battery using the positive electrode active material cannot be fully improved. When the value of x is greater than 0.9, the content of other elements that improve the output characteristics and the durability characteristics is reduced, and it is possible that the characteristics as the positive electrode active material cannot be fully obtained.
[0052] Manganese (Mn) is an element that helps improve thermal stability, and the value of y representing its content is greater than 0 and less than 0.5. Preferably, it is greater than 0.1 and less than 0.4. When the value of y is greater than 0.5, Mn dissolves from the positive electrode active material during high temperature operation, and sometimes the charge and discharge cycle characteristics deteriorate.
[0053] Cobalt (Co) is an element that helps improve charge-discharge cycle characteristics and output characteristics, and the value of z representing its content is greater than 0 and less than 0.5. Preferably, it is greater than 0.1 and less than 0.4. When the value of z is greater than 0.5, the initial discharge capacity of a secondary battery using the positive electrode active material is sometimes reduced.
[0054] The positive electrode active material of the present embodiment may contain the following additional element M. As the additional element M, one or more selected from magnesium (Mg), aluminum (Al), silicon (Si), calcium (Ca), titanium (Ti), vanadium (V), chromium (Cr), zirconium (Zr), niobium (Nb), molybdenum (Mo), hafnium (Hf), tantalum (Ta) and tungsten (W) may be used.
[0055] The additional element M is preferably at least one selected from the group consisting of Mg, Al, Si, Ti, Zr, Nb, Mo, and W, and more preferably W.
[0056] The value of t, which indicates the content of the added element M, is greater than 0 and less than 0.05. It is preferably greater than 0.001 and less than 0.03. When the value of t is greater than 0.05, the metal element contributing to the Redox reaction decreases, and thus the battery capacity of the secondary battery decreases.
[0057] The additional element M may be dispersed inside the composite oxide particles or may cover the surface of the composite oxide particles. In either case, the content of the additional element M is preferably controlled within the above range.
[0058] The composite oxide particles of the present embodiment are preferably composed of a lithium-containing nickel-manganese-cobalt composite oxide (NMC) containing Ni, Mn, and Co as main transition metals. In this case, the composite oxide particles preferably have the general formula (B): Li 1+ u Ni x Mn y Co z M t The composition of O2 (-0.05≤u≤0.5, x+y+z+t=1, 0.3≤x≤0.7, 0.15≤y≤0.4, 0.15≤z≤0.4, 0<t≤0.05, M is one or more additional elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta and W).
[0059] The composition of the positive electrode active material can be confirmed by performing Tewold analysis or the like on parameters obtained using inductively coupled plasma emission analysis or powder X-ray diffraction.
[0060] When the positive electrode active material of the present embodiment has the composition of the above-mentioned general formula (A) or general formula (B), it is a layered rock salt type and has a hexagonal crystal structure.
[0061] (2) Particle structure
[0062] In the positive electrode active material of the present embodiment, the composite oxide particles are composed of secondary particles formed by aggregation of a plurality of primary particles.
[0063] Preferably, the secondary particle has: an aggregated portion; one or more communicating holes communicating with the outer periphery of the aggregated portion; and two or more space portions existing inside the aggregated portion and communicating with the communicating holes.
[0064] It is preferred that the two or more space portions communicate with the communicating hole or other space portions. It is also preferred that the number of the communicating holes is two or more.
[0065] Since the composite oxide particles have such a secondary particle structure, the particle properties of the positive electrode active material according to one embodiment of the present invention described later can be easily achieved.
[0066] When the connecting hole of the peripheral part is not connected to the internal space part, the space part inside the particle is isolated, the electrolyte cannot fully invade the interior of the composite oxide particle (secondary particle), and sufficient reaction place cannot be ensured. Therefore, in the secondary battery using the positive electrode active material, the desired battery performance is sometimes not fully demonstrated. The two or more internal space parts can be directly connected to the connecting holes of the peripheral part respectively. Alternatively, it can also be connected to the connecting holes of the peripheral part through other connecting holes.
[0067] According to this structure, the electrolyte fully penetrates into the space inside the particle through the connecting holes in the periphery. Therefore, lithium can be extracted and inserted not only on the surface of the secondary particle but also inside the secondary particle, ensuring sufficient reaction sites and significantly reducing the internal resistance of the battery.
[0068] Therefore, when a lithium ion secondary battery is constructed using a positive electrode active material having such a structure as a positive electrode material, the output characteristics can be further improved.
[0069] (3) Particle size
[0070] In the positive electrode active material of this embodiment, the secondary particles have a 50% cumulative diameter d50 of 3.0 μm to 7.0 μm, which is obtained from the particle size distribution measurement value. The 50% cumulative diameter d50 of the secondary particles is preferably 4.0 μm to 6.5 μm, and more preferably 4.0 μm to 6.0 μm.
[0071] More specifically, the 50% cumulative diameter d50 is the particle size at which the cumulative volume is 50% of the total volume of all particles (the particle size at the point where the cumulative curve is 50% when the cumulative curve of the particle size distribution is obtained with the total volume set as 100%), as calculated based on the volume integral value measured by a laser diffraction scattering particle size analyzer.
[0072] When the 50% cumulative diameter d50 of the secondary particles constituting the positive electrode active material is within the above range, not only can the battery capacity per unit volume of a secondary battery using the positive electrode active material be increased, but also the safety and output characteristics can be improved.
[0073] In contrast, when the 50% cumulative diameter d50 is less than 3.0 μm, the filling property of the positive electrode active material is reduced, and the battery capacity per unit volume may not be increased. When the 50% cumulative diameter d50 is greater than 7.0 μm, the reaction area of the positive electrode active material is reduced, and the interface with the electrolyte is reduced, so it may be difficult to improve the output characteristics.
[0074] (4) BET specific surface area
[0075] In the positive electrode active material of this embodiment, the secondary particles have a diameter of 2.0 m 2 / g or more and 5.0m 2 / g or less. The BET specific surface area is preferably 2.5 m 2 / g or more and 4.5m 2 / g or less.
[0076] The BET specific surface area of the secondary particles is an indicator of the particle properties (contact area with the electrolyte) of the positive electrode active material. When the secondary particles have an agglomeration portion, one or more connected holes connected to the periphery of the agglomeration portion, and two or more space portions present inside the agglomeration portion and connected to the connected holes, the BET specific surface area represents the surface area of the connected holes (openings) present in the periphery of the secondary particles and the microscopic cavities (space portions) inside the secondary particles.
[0077] The BET specific surface area is measured by the BET method based on nitrogen adsorption.
[0078] The BET specific surface area of secondary particles is less than 2.0 m 2 When the positive electrode active material is used to form a secondary battery, the reaction area with the electrolyte cannot be sufficiently ensured, and the output characteristics may not be sufficiently improved. 2 When the reaction area between the positive electrode active material and the electrolyte is too large, the durability of the secondary battery may be reduced.
[0079] (5) Tap density
[0080] In the positive electrode active material of this embodiment, the secondary particles have a particle size of 1.0 g / cm 3 Above and 2.0g / cm 3 The tap density is preferably 1.0 g / cm 3 More preferably 1.2 g / cm 3 above.
[0081] The tap density is an index reflecting the density of the amount of solid region inside a spherical particle, for example.
[0082] Tap density less than 1.0g / cm 3 Even if the BET specific surface area is increased, the amount of solid area in the secondary particles is small, and the durability of the secondary battery is sometimes reduced. There is no particular restriction on the upper limit of the tap density. In the positive electrode active material of this embodiment, when the secondary particles have an agglomeration portion, one or more connecting holes connecting the outer periphery of the agglomeration portion, and two or more space portions existing inside the agglomeration portion and connecting to the connecting holes, the upper limit under normal manufacturing conditions is 2.0 g / cm 3 about.
[0083] The tap density is the bulk density after a sample powder collected in a container is tapped 100 times based on JIS Z-2504, and can be measured using a vibration specific gravity meter.
[0084] (6) Oil absorption
[0085] In the positive electrode active material of the present embodiment, the secondary particles have an oil absorption of 30 mL / 100 g or more and 60 mL / 100 g or less. The oil absorption is preferably 35 mL / 100 g or more and 55 mL / 100 g or less.
[0086] The oil absorption is an indicator that represents the total volume (total cavities) of the space inside the secondary particles. The oil absorption is determined by following the steps described in "JIS K6217-4:2008 (Carbon black for rubber - Basic properties - Part 4, Method for determining oil absorption (including compression specimens))". However, since the operation process is complicated, the oil absorption is usually determined using an oil absorption measuring device that is marketed in accordance with the above JIS. It should be noted that di-n-butyl phthalate (DBP) is used as the measuring oil (oil), and the measurement result is calculated from the oil absorption per 100g of sample, so the unit is expressed in "mL / 100g".
[0087] When the oil absorption is less than 30 mL / 100 g, sufficient space cannot be formed inside the secondary particles, and sufficient BET specific surface area may not be obtained. On the other hand, when the absorption is greater than 60 mL / 100 g, there are more space inside the secondary particles in structure, the packing density is reduced and the filling property is reduced, and when a secondary battery is formed, the battery capacity per unit volume may not be fully obtained.
[0088] (7) Coefficient of variation of the concentration of added element M
[0089] In the positive electrode active material of the present embodiment, the coefficient of variation (CV) indicating the variation in the concentration of the additional element M in the primary particles constituting the secondary particles is 1.5 or less, preferably 1.3 or less, and more preferably 1.2 or less.
[0090] The coefficient of variation of the concentration of the added element M is an index showing the dispersion of the concentration of the added element M in the entire primary particle including the interior of the primary particle and the grain boundary.
[0091] The coefficient of variation of the concentration of the added element M is obtained as described below. First, the positive electrode active material is thinly sliced by a focused ion beam device (FIB), an ion milling device, etc., so that the cross section of the secondary particle is exposed. Using a scanning transmission electron microscope (STEM) or a transmission electron microscope (TEM), for two connected primary particles with a primary particle size in the range of 0.1 μm or more and 1.0 μm or less in the cross section of the secondary particle, multiple parts of the two primary particles are irradiated with electron beams, and the energy of the characteristic X-rays of the generated added element M is analyzed by an energy dispersive X-ray analyzer (EDX), so as to obtain the concentration of the added element M in each part.
[0092] From the obtained data of the concentration of the added element M, the average concentration (μ) of the added element M and the standard deviation (σ) of the concentration of the added element M are determined.
[0093] The coefficient of variation (CV) of the concentration of the added element M is calculated according to the formula: CV = σ / μ.
[0094] When the coefficient of variation (CV) of the concentration of the added element M is greater than 1.5, the distribution of the added element M in the primary particles and / or secondary particles is shifted, and battery performance such as battery capacity and output characteristics may be impaired in a secondary battery using the positive electrode active material.
[0095] (8) Volume of the connecting part of each primary particle
[0096] In the positive electrode active material of this embodiment, based on the binarized image obtained by binarizing the three-dimensional observation image of the secondary particles, the total volume of the connecting portion between the primary particles in the binarized image and the number of the primary particles in the binarized image are determined using a watershed algorithm. The volume of the connecting portion of each primary particle obtained based on the total volume of the connecting portion between the primary particles in the binarized image and the number of the primary particles in the binarized image is preferably 5×10 5 nm 3 Above and 9×10 7 nm 3 the following.
[0097] The value of the volume of the connecting portion of each primary particle is a parameter for controlling the strength of the secondary particles constituting the positive electrode active material. By limiting the volume of the connecting portion of each primary particle to the above range, in the positive electrode active material of the present embodiment having the above characteristics, in particular, in the positive electrode active material having a structure in which the secondary particle has an agglomeration portion, one or more connecting holes connecting the outer periphery of the agglomeration portion, and two or more space portions existing on the inner side of the agglomeration portion and connected to the connecting holes, a sufficiently large mechanical strength can be obtained, and the output characteristics can be further improved without reducing the battery capacity, output characteristics, and cycle characteristics.
[0098] The volume of the connecting part of each primary particle is less than 5×10 5 nm 3 When the positive electrode active material is crushed in the crushing process, fine powder is generated, and the battery characteristics are reduced. On the other hand, when the positive electrode active material is greater than 9×10 7 nm 3 That is, as the primary particles increase in size, the porosity of the secondary particles decreases, and the reaction area between the electrolyte and the positive electrode active material decreases, thereby reducing the battery characteristics.
[0099] Considering the balance between the strength and porosity of the secondary particles, the volume of the connecting part of each primary particle is preferably 8×10 5 nm 3 Above and 9×10 6 nm 3 Below, more preferably 1×10 6 nm 3 Above and 8×10 6 m 3 the following.
[0100] The following is a method for determining the value of the volume of the connecting portion of each primary particle. Specifically, the value can be basically determined by the following evaluation method, which includes: (a) a process of obtaining a binary image based on a three-dimensional observation image of a secondary particle; (b) a process of determining the connecting portion between primary particles and the number of primary particles by a watershed algorithm based on the obtained binary image; and (c) a process of determining the volume of the connecting portion of each primary particle.
[0101] (a) Step of obtaining a binary image from a three-dimensional observation image of secondary particles
[0102] In this process, a three-dimensional observation image of the secondary particles is initially obtained. In view of the size of the secondary particles and the expected contact area with the probe, an evaluation device with appropriate spatial resolution and observation conditions are selected to implement the observation of the secondary particles. For example, for secondary particles with a particle size of more than tens of nm and less than hundreds of μm, a scanning electron microscope (hereinafter referred to as "SEM") is preferably used. For particles with a particle size of more than a few nm and less than a few hundred nm, a transmission electron microscope (hereinafter referred to as "TEM") can be used for image observation. For secondary particles of any particle size, a scanning transmission electron microscope (hereinafter referred to as "STEM") can be used.
[0103] In addition, in this embodiment, as the initially obtained observation image, an observation image including a plurality of secondary particles can be used. That is, for the observation image including a plurality of secondary particles, the process of obtaining the volume of the connecting portion of each primary particle described later can be implemented. That is, it is not limited to the observation image of a single secondary particle. Among them, the observation image of a single secondary particle can also be used.
[0104] In the case of SEM observation, a SEM device with a focused ion beam processing observation device (FIB) can be used to obtain a set of two-dimensional observation images (i.e., obtained in each depth direction) by repeatedly performing cross-sectional processing with a specified processing width and SEM observation. Based on the set of two-dimensional observation images, image analysis software can be used to obtain a three-dimensional observation image of the secondary particles.
[0105] In the case of TEM, a three-dimensional observation image of secondary particles can be obtained by three-dimensionally constructing a two-dimensional observation image captured by changing the tilt angle using tomography.
[0106] The image acquisition conditions can be changed appropriately according to the size of the particle to be observed, etc. For example, in SEM observation, generally, the following ideas can be used to change each measurement parameter.
[0107] <Accelerating voltage>
[0108] The higher the acceleration voltage, the more information about the deeper part of the sample surface will be mixed in the observed image. That is, regardless of whether the observed image is a two-dimensional image, information about the depth direction (such as information about particles buried in the cross section) is mixed in the observed image. Therefore, it is preferred to use the lowest possible acceleration voltage within the range that can ensure the required spatial resolution.
[0109] <Current>
[0110] Generally, the lower the current value (smaller aperture size), the higher the spatial resolution, but the lower the brightness, the lower the signal, the more noise, and the worse the image quality. Therefore, it is preferred to select a condition that can achieve a balance between spatial resolution and image quality.
[0111] <Working distance>
[0112] If the working distance is shortened during SEM observation, the aberration of the lens is reduced and the resolution is improved. In particular, when observing under low accelerating voltage conditions, the shorter the working distance, the higher the spatial resolution.
[0113] <Magnification and number of pixels of observation images>
[0114] The higher the magnification, the higher the spatial resolution. On the other hand, the observable range and the number of primary particles decrease. Therefore, a balanced condition is selected in consideration of the number of primary particles required for observation and the spatial resolution.
[0115] The greater the number of pixels, the higher the resolution of the image. However, this also has disadvantages such as increased image acquisition time. Therefore, it is preferable to select an appropriate value according to the required image resolution.
[0116] The size of a pixel (hereinafter, sometimes referred to as "Pixel" in the case of two-dimensional images, and sometimes referred to as "Voxel" in the case of three-dimensional images) is the minimum unit for various processing during image analysis. In image analysis, the magnification and number of pixels are determined by considering the degree of resolution under which processing is required, and the degree of size of a pixel in actual space.
[0117] <Beam dwell time per scan (Dwell Time)>
[0118] The longer the dwell time, the more signal there is and the less noise there is, so the image quality improves. However, this has the disadvantage of extending the observation time. Select appropriate conditions within the required range.
[0119] <Detector>
[0120] The electrons generated by the electron beam incident on the sample generally contain secondary electrons (inelastically scattered electrons) and reflected electrons (elastically scattered electrons). For SEM, usually, the signal ratio of secondary electrons and reflected electrons in the observed image is adjusted by adjusting various detectors and detection conditions, so as to obtain the target observed image. In the case of implementing image analysis, in most cases, the material is cut according to the contrast based on the composition. In addition, in image analysis, the contrast of the sample concave and convex generated during sample cross-section processing, etc. will become an obstacle. Therefore, it is not preferred to strongly produce a secondary electron image of the contrast from the concave and convex due to the edge effect. From this point of view, the observed image when implementing image analysis is preferably a reflected electron image composed of reflected electrons.
[0121] In the case of TEM, the higher the acceleration voltage, the higher the spatial resolution. However, depending on the sample, the sample may be damaged by electron beam irradiation. Therefore, when processing such a sample, changes such as reducing the acceleration voltage and current value can be applied.
[0122] Generally, the axes of a three-dimensionally constructed image are defined as the horizontal direction of a two-dimensional observation image as the X-axis, the vertical direction as the Y-axis, and in the case of SEM, the cross-sectional processing direction by FIB as the Z-axis.
[0123] Two-dimensional observation images are often slightly offset in X and Y positions due to the influence of stage drift during observation. Therefore, when overlapping, the X and Y positions can be aligned by performing least squares fitting between adjacent images.
[0124] In the case of TEM, a three-dimensional image can be constructed by tomography. Specifically, a two-dimensional observation image taken by changing the tilt angle is obtained in advance. At this time, Au nanopowder is added to the sample in advance. Then, the position information of the mark is added to the sample. Based on the position information in the sample, the least squares fitting is performed to implement alignment in the same way as SEM so that a three-dimensional image can be constructed.
[0125] <Pixel size equalization process>
[0126] Before the binarization process, a pixel size equivalence process can also be performed, that is, in the observation image of the sample, the incident angle of the electron beam of the electron microscope used to obtain the observation image relative to the secondary particles is added to make the pixel sizes of the X-axis and Y-axis, or the pixel sizes of the X-axis, Y-axis and Z-axis equivalent.
[0127] <Noise Removal Process>
[0128] The noise contained in the observed image after the pixel size is equalized may become an obstacle in the binarization process. Therefore, a noise removal process can also be performed as needed. As a specific method of the noise removal process, a known noise removal technology used in general image processing technology can be used.
[0129] <Binarization process>
[0130] The binarization process obtains a binarized image obtained by binarizing the observed image of the sample after the size equivalization process. Specifically, the substance to be analyzed and other substances are divided by binarization. Binarization processing is, for example, a process of dividing substances by setting a range of values of white and black intensity (Glay Scale) for each pixel of a monochrome image.
[0131] <Binarized image smoothing process>
[0132] The binary image can also be subjected to morphological processing. The "morphological processing" herein refers to a process of combining expansion and contraction of pixels of the island (or sea) portion in the island structure when the particle image is set as an island and the image of the other portion is set as a sea, which is intended to smooth the binary image and / or remove (fill in) isolated points.
[0133] However, in this embodiment, whether to implement the binarization image smoothing process is arbitrary according to the conditions for obtaining the observed image. The image is smoothed by the binarization image smoothing process, but by omitting the binarization image smoothing process, it is completed without causing information loss associated with image smoothing. Since the connecting portion of the primary particle is represented by a multi-pixel unit, it is possible to appropriately select whether to perform the binarization image smoothing process according to the conditions for obtaining the observed image.
[0134] (b) A step of determining the connection between primary particles and the number of primary particles using a watershed algorithm based on the obtained binary image.
[0135] A step of obtaining a binary image by separating and identifying primary particles using a watershed segmentation algorithm and performing labeling processing on the binary image.
[0136] The labeling process refers to the process of identifying the continuous area of pixels identified as the same substance as one area and numbering it for the binary image of the secondary particles. By performing this process to separately identify the primary particles separated by the watershed algorithm, the number (total number) of primary particles that constitute the secondary particles can be grasped.
[0137] There is no specific method for evaluating the number at this time, and the portion surrounded by the non-contacting portions between pixels can be clustered as one cluster, that is, one primary particle. In addition, each primary particle can be distinguished by numbering in the future, and the total number of each primary particle can be easily obtained.
[0138] As a method for judging whether pixels are continuous, there is the following method: if the pixels that are in contact with the pixel of interest by more than one point (point, line, surface) (in the case of two dimensions, the surrounding 8 pixels, in the case of three dimensions, the surrounding 26 pixels), or the pixels that are in contact with the pixel of interest by more than one line (line, surface) (in the case of two dimensions, the surrounding 4 pixels, in the case of three dimensions, the surrounding 18 pixels), or the pixels that are in contact with the pixel of interest by a surface (only in the case of three dimensions, the surrounding 6 pixels) are the same material, then they are judged to be continuous, and the method can be selected arbitrarily.
[0139] The watershed algorithm is a well-known technique in image processing and is a method for segmenting image regions with blurred boundaries. Specifically, in a binary image of an island structure, when a portion with a large distance from the sea to the island (i.e., the center of the island or its vicinity) is set to high brightness, it is a method for setting boundaries at appropriate positions between high brightness portions according to each brightness. In this way, the boundaries of touching objects in the image can be separated and identified.
[0140] When the watershed algorithm is applied, if there is one pixel (one pixel or one voxel) in a portion having brightness, the portion can be identified as a high brightness portion. However, this is not limited to this, and depending on the type of sample used as the object, the acquisition conditions of the observed image, or other reasons, the portion having brightness can be identified as a high brightness portion only when there are multiple pixels in the portion.
[0141] (c) Step of determining the volume of the connecting portion of each primary particle
[0142] For this process, in the previous process, based on the binarized image obtained by binarizing the three-dimensional observation image of a single or multiple secondary particles, the watershed algorithm is used to determine the data related to the primary particles, the connecting parts between the primary particles, and the number of primary particles. Based on the data, the value of the total volume of the connecting parts between the primary particles is obtained, and the volume of the connecting parts of each primary particle is calculated using the total volume of the connecting parts between the primary particles and the number of primary particles.
[0143] The degree of connection of the primary particles in the secondary particles having a porous structure is evaluated based on the volume of the connection portion per primary particle.
[0144] In this process, the value of the total volume of the connecting portion between the primary particles constituting the secondary particles is first obtained. The following is an example of a method for obtaining the total volume of the connecting portion between the primary particles. However, this method is not limited to the following example.
[0145] According to the number of pixels of the binary image before the separation of the primary particles based on the watershed algorithm, the total volume of the primary particles in the state before separation is obtained. Then, according to the number of pixels of the binary image after the separation of the primary particles based on the watershed algorithm, the total volume of the primary particles in the state after separation is obtained. Then, by subtracting the total volume of the primary particles after separation from the total volume of the primary particles before separation, the total volume of the connecting portion between the primary particles can be obtained.
[0146] More specifically, according to Figure 3 The area of the primary particle before separation in the binary image corresponding to the depth in the Z-axis direction before separation of the primary particles based on the watershed algorithm shown in (a) is subtracted from the area of the primary particle obtained based on the depth in the Z-axis direction. Figure 3 The area of the primary particles obtained from the image of the separated primary particles as shown in (b) can be used to obtain the area of the connecting portion between the primary particles (number of pixels: pixels), and the areas between the primary particles corresponding to the depth in the Z-axis direction can be summed up to obtain the total volume of the connecting portion (number of pixels: voxels).
[0147] Alternatively, a binary image of the connecting portion between the primary particles can be obtained based on the data of the binary image before and after separation of the primary particles based on the watershed algorithm, and the total volume of the connecting portion between the primary particles can be obtained based on the number of pixels in the binary image of the connecting portion between the primary particles.
[0148] More specifically, according to Figure 3 (a) shows a primary particle image before separation in a binary image corresponding to the depth in the Z-axis direction before separation of primary particles based on the watershed algorithm, and Figure 3 The image of the primary particles after separation as shown in (b) is obtained. Figure 3 A binary image of the connecting portion between the primary particles as shown in (c) is obtained, and then the area of the connecting portion between the primary particles (number of pixels: pixels) is obtained based on the binary image of the connecting portion between the primary particles. The areas between the primary particles corresponding to the depth in the Z-axis direction are summed up, thereby obtaining the total volume of the connecting portion (number of pixels: voxels).
[0149] In this embodiment, as described above, the volume of the connecting portion of each primary particle is obtained from the total volume of the connecting portion between primary particles and the number of primary particles determined from the binarized image obtained by binarizing the three-dimensional observation image using the watershed algorithm.
[0150] Even if it is not divided by the number of primary particles, the volume of the connecting portion can be obtained based on the total value of the number of pixels of the connecting portion and the information on the size of one pixel in the binary image in the actual space. However, the volume of the connecting portion is greatly affected by the number of primary particles. Therefore, in this embodiment, in order to evaluate the degree of compressive strength of the secondary particles of the porous structure in more detail, the influence of the number of primary particles is eliminated by dividing the volume of the connecting portion by the number of primary particles.
[0151] The image processing in each of the above-mentioned steps can be realized by using known software. As an example of such software, the image analysis software "AVIZO" (manufactured by FEI Co., Ltd., Japan) can be cited. Such image analysis software can be used to perform image processing in all steps and extract required numerical data. However, the present embodiment is not limited to the use of such image analysis software, and multiple known image analysis software can also be used to perform image analysis and extraction of numerical data in each step.
[0152] In addition, when obtaining an observation image of a single secondary particle based on an observation image including a plurality of secondary particles, especially an observation image including a tertiary particle formed by the aggregation of a plurality of secondary particles, a single secondary particle is extracted by determining the connection between the secondary particles using a watershed algorithm based on a binary image obtained from the observation image including the plurality of secondary particles. On this basis, a process of determining the volume of the connection of each primary particle can be implemented.
[0153] (9) Particle size distribution
[0154] Although it is arbitrary, in the positive electrode active material of the present embodiment, [(d90-d10) / d50], which is an index representing the width of the particle size distribution of the secondary particles, is preferably less than 1.0, more preferably less than 0.7, and further preferably less than 0.6. The proportion of fine particles and coarse particles in the positive electrode active material composed of secondary particles with such a narrow particle size distribution is small, and therefore, the safety, cycle characteristics and output characteristics of the secondary battery using the positive electrode active material are excellent.
[0155] When (d90-d10) / d50 is greater than 1.0, the proportion of fine particles and coarse particles in the positive electrode active material increases. For example, when the proportion of fine particles is high, the secondary battery is prone to heat due to the local reaction of the fine particles, which not only reduces safety, but also sometimes leads to poor cycle characteristics due to the selective degradation of the fine particles. In addition, when the proportion of coarse particles is high, the reaction area between the electrolyte and the positive electrode active material cannot be fully ensured, and sometimes the output characteristics are poor.
[0156] In the case of industrial-scale production, it is not realistic to use a material with too small [(d90-d10) / d50] as a positive electrode active material. Therefore, considering cost and productivity, the lower limit of [(d90-d10) / d50] is preferably about 0.3.
[0157] It should be noted that the meaning and calculation method of d10 and d90 in the index [(d90-d10) / d50] representing the width of the particle size distribution are the same as those of the above-mentioned d50, d90 refers to the particle size at which the volume of each particle accumulated from the side with a smaller particle size is 90% of the total volume of all particles, and d10 refers to the particle size at which the volume of each particle accumulated from the side with a smaller particle size is 10% of the total volume of all particles.
[0158] (10)d90 / d10
[0159] Although optional, in the positive electrode active material of this embodiment, the ratio of the d90 value to the d10 value (d90 / d10) obtained from the particle size distribution measurement value of the secondary particles is preferably 1.0 to 2.0, and more preferably 1.2 to 1.8.
[0160] If the value of d90 / d10 of the secondary particles constituting the positive electrode active material is within this range, not only can the battery capacity per unit volume of the secondary battery using the positive electrode active material be increased, but also the safety and output characteristics can be improved. When the value of d90 / d10 of the secondary particles is greater than 2.0, the reaction area of the positive electrode active material is reduced, and the interface with the electrolyte is reduced, so it may be difficult to improve the output characteristics.
[0161] (11) Grain size obtained from the X-ray diffraction pattern of the (003) plane
[0162] Although arbitrary, the composite oxide particles constituting the positive electrode active material of the present embodiment preferably have a primary particle crystallite diameter of 0.0407 W / m2 when the crystallite diameter is calculated using the Scherrer equation from the half-value width of the peak on the (003) plane based on X-ray diffraction. Above and The following are more preferably Above and The following is further preferably above The positive electrode active material having a crystal grain size within the above range has extremely high crystallinity, and can reduce the positive electrode resistance of the secondary battery and improve its output characteristics.
[0163] The grain size of (003) plane is smaller than When the primary particles are fine, the pores between the primary particles in the positive electrode active material are too fine, and the electrolyte is difficult to penetrate into the positive electrode active material. Therefore, the reaction area with the electrolyte is reduced, and the output characteristics of the secondary battery are reduced. The grain size of the (003) plane is larger than When the primary particles are too coarse, the proportion of pores occupied by the secondary particles is extremely reduced, and the intrusion paths of the electrolyte are reduced. Therefore, the reaction area with the electrolyte is reduced, and the output characteristics of the secondary battery are reduced.
[0164] 2. Method for producing positive electrode active material for lithium ion secondary battery
[0165] The positive electrode active material of the above-described embodiment is not limited by its production method as long as it has the above-described composition, crystal structure, particle structure, and particle properties.
[0166] However, by producing the positive electrode active material of the above-described embodiment by the production method described below, it is possible to easily produce the positive electrode active material having the above-described composition, crystal structure, particle structure, and particle properties.
[0167] Specifically, the positive electrode active material of the embodiment is obtained by switching the oxidizing environment and the non-oxidizing environment in the crystallization process, preparing a composite hydroxide containing transition metals such as a composite hydroxide containing nickel, manganese and cobalt, mixing the composite hydroxide or the heat-treated particles obtained by heat-treating the composite hydroxide with a lithium compound, and calcining the obtained lithium mixture.
[0168] Hereinafter, each step will be described in detail by taking the case where the composite oxide particles are composite oxide particles containing lithium, nickel, manganese and cobalt as an example.
[0169] (1) Crystallization process
[0170] Water, sodium hydroxide aqueous solution, sodium carbonate aqueous solution and ammonia water are supplied in appropriate amounts to the reaction tank, and a pre-reaction aqueous solution adjusted to a pH value of 11 or more and 13 or less at a liquid temperature of 25°C and an ammonium ion concentration of 9 g / L or more and 15 g / L or less is prepared. On the other hand, it is preferred to dissolve nickel sulfate, manganese sulfate, cobalt sulfate and a compound (sulfate, sodium salt, etc.) of the additive element M in water so that the molar ratio of each metal element (Ni, Co, Mn, M) satisfies the above formula (A), and prepare a raw material aqueous solution of 1.0 mol / L or more and 3.0 mol / L or less. Alternatively, nickel sulfate, manganese sulfate and cobalt sulfate are dissolved in water so that the molar ratio of each metal element (Ni, Co, Mn) satisfies the above formula (A), and a raw material aqueous solution of 1.0 mol / L or more and 3.0 mol / L or less is prepared, and an aqueous solution containing a compound of the additive element M is prepared, which can also be added to the raw material aqueous solution so that the amount of the additive element M satisfies the above formula (A).
[0171] Then, by blowing in a gas having an oxygen concentration of less than 2% by volume such as argon or nitrogen in a non-oxidizing environment, the raw aqueous solution is supplied to the aqueous solution before the reaction to generate nuclei. At this time, preferably, sodium hydroxide aqueous solution, sodium carbonate aqueous solution and ammonia water are appropriately supplied to maintain the pH value and ammonium ion concentration of the aqueous solution for nucleation within the above range.
[0172] After the nucleation is completed, an acid such as sulfuric acid is added to adjust the pH value to be greater than 10 and less than 12 at a liquid temperature of 25°C and less than the pH value in the nucleation process, thereby forming an aqueous solution for particle growth. After confirming that the pH value has reached a specified value, the above-mentioned raw material aqueous solution is supplied and the nuclei (particles) generated in the nucleation process are grown. In addition, when an aqueous solution containing a compound of an additional element M is prepared separately, the aqueous solution containing the compound of the additional element M can also be added only in the particle growth process or only in a specific stage (for example, the third stage and the fourth stage) of the particle growth process.
[0173] As the first stage of the particle growth, crystallization is continuously performed in a non-oxidizing atmosphere with an oxygen concentration of 2% by volume or less while stirring for a predetermined time using a stirrer from the start of the particle growth step.
[0174] As the second stage, while the raw material aqueous solution is continuously supplied, air or oxygen is circulated in the reaction tank using a diffuser tube having a pore size of 100 μm or more and 1 cm or less, and the reaction environment is adjusted to an oxidizing environment with an oxygen concentration of 21 volume % or more. After the start of the switching operation 1, crystallization is performed while stirring for a predetermined time using a stirrer while maintaining the oxidizing environment.
[0175] As the third stage, while the raw material aqueous solution is continuously supplied, a gas in a non-oxidizing environment is circulated in the reaction tank using a diffuser to adjust the reaction environment to a non-oxidizing environment with an oxygen concentration of 2% by volume or less. After the start of the switching operation 2, crystallization is performed while stirring for a predetermined time using a stirrer while maintaining the non-oxidizing environment.
[0176] As the fourth stage, while the raw material aqueous solution is continuously supplied, the gas in the oxidizing environment is circulated in the reaction tank using a diffuser to adjust the reaction environment to an oxidizing environment with an oxygen concentration of 21 volume % or more. After the start of the switching operation 3, crystallization is performed while stirring for a predetermined time using a stirrer while maintaining the oxidizing environment.
[0177] As the fifth stage, while the raw material aqueous solution is continuously supplied, a gas in a non-oxidizing environment is circulated in the reaction tank using a diffuser to adjust the reaction environment to a non-oxidizing environment with an oxygen concentration of 2% by volume or less, and a switching operation 4 is performed. After the switching operation 4 is started, crystallization is performed while stirring for a predetermined time using a stirrer while maintaining the non-oxidizing environment.
[0178] The time of each stage in the particle growth step is second stage ≤ fourth stage < first stage ≤ third stage ≤ fifth stage. It is preferred that the crystallization time of the entire particle growth step be within 8 hours.
[0179] The particle growth process can also perform switching operations 5 and 6 in the same manner, setting the sixth stage in an oxidizing environment and the seventh stage in a non-oxidizing environment. Further, it is also possible to perform switching operations 7 and 8, setting the eighth stage in an oxidizing environment and the ninth stage in a non-oxidizing environment. It is also possible to further perform switching operations 9 and 10, setting the tenth stage in an oxidizing environment and the eleventh stage in a non-oxidizing environment.
[0180] In these cases, the time of each stage in the particle growth process is also the second stage ≤ the fourth stage ≤ the sixth stage ≤ the eighth stage ≤ the tenth stage < the first stage ≤ the third stage ≤ the fifth stage ≤ the seventh stage ≤ the ninth stage ≤ the eleventh stage.
[0181] After the crystallization is completed, the obtained product is washed with water, filtered and dried, thereby obtaining predetermined nickel-cobalt-manganese-containing composite hydroxide particles.
[0182] In the particle growth step, it is preferred that the pH value and ammonium ion concentration of the aqueous solution for particle growth be maintained within the above ranges by appropriately supplying sodium hydroxide aqueous solution, sodium carbonate aqueous solution and ammonia water throughout the step.
[0183] The composite hydroxide particles obtained by the crystallization step have a particle structure in which a low-density layer and a high-density layer are stacked around a high-density center. By using the composite hydroxide particles having the particle structure as a precursor, it is easy to obtain composite oxide particles having a particle structure having an agglomeration portion, one or more connected holes connected to the peripheral portion of the agglomeration portion, and two or more space portions existing inside the agglomeration portion and connected to the connected holes.
[0184] (2) Mixing process
[0185] The mixing step is a step of mixing a lithium compound with the composite hydroxide particles or heat-treated particles obtained by heat-treating the composite hydroxide particles to obtain a lithium mixture.
[0186] In the mixing process, the composite hydroxide particles and the lithium compound are mixed so that the metal atoms other than Li in the lithium mixture, specifically the sum of the atomic numbers of Ni, Mn, Co and the added element M (Me) and the atomic number of Li (Li) (Li / Me) is 0.95 or more and 1.5 or less, preferably 1.0 or more and 1.5 or less, more preferably 1.0 or more and 1.35 or less, and further preferably 1.0 or more and 1.2 or less. That is, before and after the calcination process, since Li / Me does not change, it is necessary to mix the composite hydroxide and the lithium compound so that the Li / Me in the mixing process becomes the Li / Me of the target positive electrode active material.
[0187] The lithium compound used in the mixing step is not particularly limited, but lithium hydroxide, lithium nitrate, lithium carbonate or a mixture thereof is preferably used from the perspective of availability. In particular, lithium hydroxide or lithium carbonate is preferably used in consideration of the ease of handling and quality stability.
[0188] For mixing, a common mixer can be used, for example, a vibration mixer, a Lodyga mixer, a Julia mixer, a V-blender, etc. can be used.
[0189] (3) Pre-burning process
[0190] When lithium hydroxide or lithium carbonate is used as the lithium compound, a calcination step of calcining the lithium mixture at a temperature lower than the calcination temperature described later and at a temperature of 350° C. to 800° C., preferably 450° C. to 750° C., can be performed after the mixing step and before the calcination step. This allows Li to be sufficiently diffused in the composite hydroxide particles, and more uniform composite oxide particles can be obtained.
[0191] In addition, the holding time under the above temperature conditions is preferably 1 hour or more and 10 hours or less, more preferably 3 hours or more and 6 hours or less. In addition, the environment in the calcining step is preferably an oxidizing environment as in the calcining step described later, more preferably an environment with an oxygen concentration of 18 volume % or more and 100 volume % or less.
[0192] (4) Firing process
[0193] The calcining step is a step of calcining the lithium mixture obtained in the mixing step under predetermined conditions to diffuse and react Li in the composite hydroxide to obtain composite oxide particles.
[0194] The furnace used in the sintering process is not particularly limited, as long as the lithium mixture can be heated in the atmosphere or oxygen flow. However, from the viewpoint of uniformly maintaining the environment in the furnace, an electric furnace that does not generate gas is preferably used, and any of an intermittent or continuous electric furnace can be suitably used. In this regard, the furnace used in the heat treatment process and the pre-sintering process is also the same.
[0195] a) Firing temperature
[0196] The calcination temperature of the lithium mixture is set to be above 720°C and below 980°C. When the calcination temperature is less than 720°C, the composite hydroxide particles and Li cannot fully react, and the remaining Li and unreacted composite hydroxide remain, or the crystallinity of the obtained positive electrode active material is insufficient. On the other hand, when the calcination temperature is greater than 980°C, the interconnecting pores and space portions in the composite oxide particles are destroyed, which may lead to a decrease in the BET specific surface area, a decrease in oil absorption, and an increase in the tap density of the final positive electrode active material. In addition, the particles of the positive electrode active material are violently sintered, causing abnormal particle growth, and the proportion of amorphous coarse particles increases.
[0197] By controlling the calcination temperature, the BET specific surface area, oil absorption, tap density, volume of the connecting portion of each primary particle, and 50% cumulative diameter d50 obtained from the particle size distribution measurement value of the positive electrode active material (secondary particles) can be controlled. From the viewpoint of controlling the BET specific surface area, oil absorption, tap density, volume of the connecting portion of each primary particle, and 50% cumulative diameter d50 obtained from the particle size distribution measurement value of the positive electrode active material (secondary particles), the calcination temperature of the lithium mixture is preferably set to 730°C or more and 970°C or less, and more preferably set to 750°C or more and 970°C or less.
[0198] The heating rate in the calcining process is preferably set to 1°C / min or more and 10°C / min or less, and more preferably set to 3°C / min or more and 8°C / min or less. Further, in the calcining process, it is more preferred that the heating rate is reduced to 0.3°C / min or more and 6°C / min or less at a temperature near the melting point of the lithium compound. Thus, the composite hydroxide particles and the lithium compound can react more uniformly.
[0199] b) Firing time
[0200] In the calcination time, the holding time under the above calcination temperature conditions is preferably set to at least 2 hours, and more preferably set to 3 hours or more and 20 hours or less. When the holding time under the calcination temperature conditions is less than 2 hours, Li cannot be fully diffused in the composite oxide particles, and the remaining Li and unreacted composite oxide particles may remain, or the crystallinity of the obtained positive electrode active material may be insufficient.
[0201] c) Firing environment
[0202] The environment during firing is preferably set to an oxidizing environment, more preferably set to an environment with an oxygen concentration of 18% by volume or more and 100% by volume or less, and further preferably set to an environment with an oxygen concentration of 50% by volume or more and 100% by volume or less. It is particularly preferred to set it to a mixed environment of oxygen and an inert gas at the above oxygen concentration. That is, firing is preferably carried out in the atmosphere or an oxygen flow. When the oxygen concentration is less than 18% by volume, the crystallinity of the positive electrode active material may be insufficient.
[0203] (5) Crushing process
[0204] The secondary particles constituting the positive electrode active material obtained by the firing process sometimes produce agglomeration or light sintering. In this case, it is preferred to crush the agglomerate or sintered body. Thus, the average particle size and particle size distribution of the obtained positive electrode active material can be adjusted to a suitable range. It should be noted that crushing refers to the operation of applying mechanical energy to an agglomerate composed of a plurality of secondary particles generated by sintering necks between particles during firing, so as to separate them without substantially destroying the secondary particles themselves, thereby loosening the agglomerate.
[0205] As a crushing method, a known method can be used, for example, a pin mill, a hammer mill, etc. It should be noted that at this time, it is preferable to control the crushing force within an appropriate range so as not to destroy the secondary particles themselves.
[0206] As described above, by adjusting the sintering conditions, the BET specific surface area, oil absorption, tap density, volume of the connecting portion of each primary particle, and 50% cumulative diameter d50 calculated based on the particle size distribution measurement value of the positive electrode active material (secondary particles) can be controlled, and ultimately the positive electrode active material of the embodiment having specified particle properties can be easily obtained.
[0207] 3. Lithium-ion secondary battery
[0208] The lithium ion secondary battery of one embodiment of the present invention can adopt the same structure as a general non-aqueous electrolyte secondary battery having components such as a positive electrode, a negative electrode, a separator and a non-aqueous electrolyte. Alternatively, the lithium ion secondary battery of this embodiment can adopt the same structure as a general solid electrolyte secondary battery having components such as a positive electrode, a negative electrode and a solid electrolyte. That is, as long as it is a secondary battery that is charged and discharged by the extraction and insertion of lithium ions, the present invention can be widely applied to non-aqueous electrolyte secondary batteries to all-solid lithium ion secondary batteries. It should be noted that the embodiments described below are merely examples, and the present invention can be applied to lithium ion secondary batteries that have been variously changed and improved according to the embodiments described in this specification.
[0209] (1) Components
[0210] a) Positive electrode
[0211] Using the positive electrode active material of the above-described embodiment, a positive electrode of a lithium ion secondary battery is produced, for example, as follows.
[0212] First, a conductive material and a binder are mixed in the positive active material of the embodiment, and activated carbon, viscosity adjustment and other solvents are further added as needed, and these are mixed to manufacture a positive composite material paste. At this time, each mixing ratio in the positive composite material paste is also an important factor in determining the performance of the lithium ion secondary battery. For example, when the solid content of the positive composite material from which the solvent is removed is set to 100 parts by mass, similarly to the positive electrode of a general lithium ion secondary battery, the content of the positive active material can be set to more than 60 parts by mass and less than 95 parts by mass, the content of the conductive material is set to more than 1 part by mass and less than 20 parts by mass, and the content of the binder is set to more than 1 part by mass and less than 20 parts by mass.
[0213] The obtained positive electrode composite material paste is applied to the surface of a collector made of aluminum foil, for example, and dried to disperse the solvent. As needed, it is sometimes pressed by a roller press or the like to increase the electrode density. In this way, a sheet positive electrode can be prepared. The sheet positive electrode can be cut into appropriate sizes according to the target battery and used in the preparation of the battery. It should be noted that the manufacturing method of the positive electrode is not limited to the method exemplified above, and other methods can also be used.
[0214] As the conductive material, for example, carbon black materials such as graphite (natural graphite, artificial graphite, expanded graphite, etc.), acetylene black, and Ketjen black can be used.
[0215] The binder plays a role in linking the active material particles to prevent them from falling off, and for example, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluororubber, ethylene-propylene-diene rubber, styrene-butadiene, cellulose-based resin or polyacrylic acid can be used.
[0216] In addition, a solvent that disperses the positive active material, the conductive material and the activated carbon and dissolves the binder can be added to the positive composite material as required. As a solvent, specifically, organic solvents such as N-methyl-2-pyrrolidone can be used. In addition, in the positive composite material, activated carbon can also be added in order to increase the double electric layer capacity.
[0217] b) Negative electrode
[0218] In the negative electrode, metallic lithium, lithium alloy, etc. can be used. In addition, the negative electrode formed by mixing a binder in a negative electrode active material capable of absorbing and desorbing lithium ions, adding a suitable solvent, and preparing a paste-like negative electrode composite material, applying the negative electrode composite material to the surface of a metal foil collector such as copper, and drying it, and compressing it as needed to increase the electrode density to form a negative electrode.
[0219] As the negative electrode active material, for example, lithium-containing materials such as metallic lithium and lithium alloys, natural graphite, artificial graphite, sintered organic compounds such as phenolic resins, and carbon material powders such as coke that can absorb and release lithium ions can be used. In this case, as the negative electrode binder, fluorine-containing resins such as PVDF can be used in the same manner as the positive electrode, and as the solvent for dispersing these negative electrode active materials and binders, organic solvents such as N-methyl-2-pyrrolidone can be used.
[0220] c) Spacer
[0221] The separator is sandwiched between the positive electrode and the negative electrode in the lithium ion secondary battery, and has the function of separating the positive electrode from the negative electrode and retaining the electrolyte. As such a separator, for example, a film having many micropores in a film such as polyethylene or polypropylene can be used, but there is no particular limitation as long as it has the above-mentioned function. In addition, a solid electrolyte can also be used.
[0222] d) Electrolytes
[0223] As the nonaqueous electrolyte used in the nonaqueous electrolyte secondary battery, a nonaqueous electrolytic solution prepared by dissolving a lithium salt as a supporting salt in an organic solvent or the like is used.
[0224] As the organic solvent for the non-aqueous electrolyte, one selected from cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, and propylene trifluorocarbonate; chain carbonates such as diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, and dipropyl carbonate; ether compounds such as tetrahydrofuran, 2-methyltetrahydrofuran, and dimethoxyethane; sulfur compounds such as methyl ethyl sulfone and butane sultone; phosphorus compounds such as triethyl phosphate and trioctyl phosphate, etc. can be used alone, or two or more thereof can be mixed and used.
[0225] As supporting salts, LiPF6, LiBF4, LiClO4, LiAsF6, LiN(CF3SO2)2, and complex salts thereof can be used.
[0226] Furthermore, the non-aqueous electrolyte may contain a radical scavenger, a surfactant, a flame retardant, and the like.
[0227] Solid electrolytes used in solid electrolyte secondary batteries such as all-solid lithium ion secondary batteries have the property of withstanding high voltages. Solid electrolytes include inorganic solid electrolytes and organic solid electrolytes.
[0228] As the oxide solid electrolyte, an oxide containing oxygen (O) and having lithium ion conductivity and electronic insulation can be used, for example, Li 1.3 Al 0.3 Ti 1.7 (PO4)3, Li3PO4, Li3PO4NX 、LiBO2N X , LiNbO3, LiTaO3, Li2SiO3, Li4SiO4-Li3PO4, Li4SiO4-Li3VO4, Li2O-B2O3-P2O5, Li2O-SiO2, Li2O-B2O3-ZnO, Li 1+X Al X Ti 2-X (PO4)3(0≤X≤1), Li 1+X Al X Ge 2-X (PO4)3(0≤X≤1), LiTi2(PO4)3, Li 3X La 2 / 3-X TiO3(0≤X≤2 / 3), Li5La3Ta2O 12 、Li7La3Zr2O 12 、Li6BaLa2Ta2O 12 , Li 3.6 Si 0.6 P 0.4 O4, etc.
[0229] As a sulfide solid electrolyte, a sulfide containing sulfur (S) and having lithium ion conductivity and electronic insulation can be used, for example, Li2S-SiS2, Li2S-P2S5, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-B2S3, Li3PO4-Li2S-Si2S, Li3PO4-Li2S-SiS2, LiPO4-Li2S-SiS, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, etc.
[0230] As an inorganic solid electrolyte other than an oxide solid electrolyte and a sulfide solid electrolyte, for example, Li 3 N, LiI, Li 3 N—LiI—LiOH, etc. can be used.
[0231] As the organic solid electrolyte, a polymer compound exhibiting ion conductivity can be used, for example, polyethylene oxide, polypropylene oxide, copolymers thereof, etc. can be used. In addition, the organic solid electrolyte can include a supporting salt (lithium salt).
[0232] In addition, when a solid electrolyte is used, the solid electrolyte may be mixed with the positive electrode material in order to ensure contact between the electrolyte and the positive electrode active material.
[0233] (2) Structure of lithium-ion secondary battery
[0234] There is no particular limitation on the composition of the lithium ion secondary battery, and a structure consisting of a positive electrode, a negative electrode, a separator, a non-aqueous electrolyte, etc. in a non-aqueous electrolyte secondary battery, or a structure consisting of a positive electrode, a negative electrode, a solid electrolyte, etc. in a solid electrolyte secondary battery can be adopted. In addition, there is no particular limitation on the shape of the secondary battery, and various shapes such as a cylindrical shape and a stacked shape can be adopted.
[0235] In the case of a non-aqueous electrolyte secondary battery, for example, a positive electrode and a negative electrode are stacked with a separator to form an electrode body, a non-aqueous electrolyte is impregnated into the obtained electrode body, a collector lead or the like is used to connect the positive electrode collector and the positive terminal connected to the outside, and the negative electrode collector and the negative terminal connected to the outside, and the connection is sealed in a battery case to complete a lithium-ion secondary battery.
[0236] (3) Characteristics of lithium-ion secondary batteries
[0237] The lithium-ion secondary battery of this embodiment uses the positive electrode active material of the embodiment as the positive electrode material as described above, and therefore has excellent output characteristics and durability characteristics. The positive electrode active material is composed of secondary particles with a multilayer structure having a hollow structure or a space portion with excellent output characteristics, and the output characteristics and mechanical strength of the positive electrode active material are further improved.
[0238] (4) Applications of lithium-ion secondary batteries
[0239] As described above, the lithium ion secondary battery of the present embodiment is excellent in output characteristics and endurance characteristics, and can be suitably used as a power source for electric tools and environmentally friendly vehicles that require high levels of these characteristics.
[0240] Example
[0241] In the following, an embodiment of the present invention is described in detail using examples and comparative examples. In the whole process of the nucleation step and the particle growth step, the pH value of the reaction aqueous solution is measured by a pH controller, and the supply amount of the sodium hydroxide aqueous solution and the sodium carbonate aqueous solution is adjusted according to the measured value, so that the pH value of the reaction aqueous solution in each step is controlled to be within the range of ±0.2.
[0242] (Example 1)
[0243] a) Production of composite hydroxides
[0244] [Nucleation process]
[0245] First, 17 L of water was added to the reaction tank and stirred while the temperature in the tank was set to 40° C. At this time, nitrogen was circulated in the reaction tank for 1 hour to set the reaction environment to a non-oxidizing environment with an oxygen concentration of 2% by volume or less. Next, 25% by mass of an aqueous sodium hydroxide solution, 25% by mass of an aqueous sodium carbonate solution, and 25% by mass of an ammonia solution were appropriately supplied to the reaction tank to adjust the pH value to 12.6 at a liquid temperature of 25° C. and the ammonium ion concentration to 10 g / L, thereby forming a pre-reaction aqueous solution.
[0246] Meanwhile, nickel sulfate, manganese sulfate, and cobalt sulfate were dissolved in water so that the molar ratio of each metal element was Ni:Co:Mn=5:2:3, and a 2 mol / L raw material aqueous solution was prepared.
[0247] W was used as the additive element M. Sodium tungstate dihydrate was dissolved in water so that the molar ratio of each metal element including the additive element M in the obtained composite hydroxide particles was Ni:Mn:Co:W=5.0:2.0:3.0:0.1, thereby preparing a sodium tungstate aqueous solution.
[0248] Then, the raw material aqueous solution was supplied to the aqueous solution before the reaction at 115 mL / min to form an aqueous solution for nucleation, and nucleation was performed for 1 minute. At this time, 25% by mass of an aqueous sodium hydroxide solution, 25% by mass of an aqueous sodium carbonate solution, and 25% by mass of an ammonia solution were appropriately supplied to maintain the pH value and ammonium ion concentration of the aqueous solution for nucleation within the above range.
[0249] [Particle Growth Process]
[0250] After the nucleation is completed, the supply of all aqueous solutions is temporarily stopped, and sulfuric acid is added to adjust the pH value to 11.0 at a liquid temperature of 25°C, thereby forming an aqueous solution for particle growth. After confirming that the pH value is a specified value, the raw material aqueous solution is supplied at the same 100 mL / min and a specified ratio as in the nucleation process to grow the nuclei (particles) generated in the nucleation process. In addition, the sodium tungstate aqueous solution is supplied at 10 mL / min and a specified ratio in the third stage and the fourth stage simultaneously with the raw material aqueous solution.
[0251] As the first stage, crystallization was continued for 35 minutes in a non-oxidizing atmosphere with an oxygen concentration of 2% by volume or less from the start of the particle growth step while stirring using a stirrer.
[0252] As the second stage, while the raw material aqueous solution was continuously supplied, air was circulated in the reaction tank using a SUS diffuser with a pore size of 1.0 mm to adjust the reaction environment to an oxidizing environment with an oxygen concentration of 21 volume % (switching operation 1). After the switching operation 1 was started, crystallization was performed for 20 minutes while stirring with a stirrer.
[0253] As the third stage, while the raw material aqueous solution was continuously supplied, nitrogen was circulated in the reaction tank using a diffuser while the sodium tungstate aqueous solution was supplied, and the reaction environment was adjusted to a non-oxidizing environment with an oxygen concentration of 2 volume % or less (switching operation 2). After the switching operation 2 was started, crystallization was performed for 65 minutes while stirring with a stirrer.
[0254] As the fourth stage, while the raw material aqueous solution and the sodium tungstate aqueous solution were continuously supplied, air was circulated in the reaction tank using a diffuser to adjust the reaction environment to an oxidizing environment with an oxygen concentration of 21 volume % (switching operation 3). After the switching operation 3 was started, crystallization was performed for 40 minutes while stirring with a stirrer.
[0255] As the fifth stage, the supply of the sodium tungstate aqueous solution was stopped, and on the other hand, nitrogen was circulated in the reaction tank using a diffuser while the raw material aqueous solution was continuously supplied, and the reaction environment was adjusted to a non-oxidizing environment with an oxygen concentration of 2 volume % or less (switching operation 4). After the switching operation 4 was started, crystallization was performed for 110 minutes while stirring with a stirrer.
[0256] Then, the particle growth step is terminated by stopping the supply of all aqueous solutions including the raw material aqueous solution. The obtained product is washed with water, filtered, and dried to obtain composite hydroxide particles.
[0257] In the particle growth step, 25 mass % sodium hydroxide aqueous solution, 25 mass % sodium carbonate aqueous solution and 25 mass % ammonia water were appropriately supplied throughout the step to maintain the pH value and ammonium ion concentration of the aqueous solution for particle growth within the above ranges.
[0258] b) Production of positive electrode active material
[0259] The obtained composite hydroxide and lithium hydroxide were fully mixed with a vibration mixer so that Li / Me became 1.10, thereby obtaining a lithium mixture (mixing step).
[0260] The lithium mixture was heated to 970° C. at a heating rate of 1.3° C. / min in an oxygen atmosphere (oxygen concentration: 100% by volume), maintained at this temperature for 3 hours to be fired, and cooled to room temperature (firing step).
[0261] In order to eliminate aggregation or light sintering of the obtained lithium-transition metal-containing composite oxide particles, the positive electrode active material is crushed (crushing step).
[0262] c) Evaluation of positive electrode active materials
[0263] [composition]
[0264] The composition of the positive electrode active material was analyzed by using an ICP emission spectrometer (manufactured by Shimadzu Corporation, ICPE-9000).
[0265] [Particle size distribution]
[0266] The 50% cumulative diameter d50, 10% cumulative diameter d10 and 90% cumulative diameter d90 obtained from the particle size distribution measurement value of the positive electrode active material (secondary particles) were measured using a laser diffraction scattering particle size analyzer (Microtrac MT 3300EXII manufactured by Microtrac BEL Corp., Japan).
[0267] [BET specific surface area and tap density]
[0268] The BET specific surface area of the secondary particles was measured using a flow gas adsorption specific surface area measuring apparatus (Macsorb 1200 series, manufactured by Mountech Co., Ltd.), and the tap density of the secondary particles was measured using a tapping machine (KRS-406, manufactured by Kurachi Scientific Instruments Mfg. Co., Ltd.).
[0269] [Oil absorption]
[0270] The oil absorption of di-n-butylphthalate (DBP) of the positive electrode active material (secondary particles) was measured using an oil absorption measuring apparatus (S-500 manufactured by ASAHI SOUKEN CO., LTD.) in accordance with "JIS K6217-4:2008".
[0271] [Particle structure]
[0272] A portion of the positive electrode active material was embedded in the resin and processed by a cross-section polisher (manufactured by JEOL Ltd., IB-19530CP) to a state where the cross section could be observed. On this basis, SEM (FE-SEM: manufactured by JEOL Ltd., JSM-6360LA) was used for observation. Figure 1 As shown, it is confirmed that the positive electrode active material of this embodiment is formed by secondary particles, which are aggregated by multiple primary particles, have about 6 connecting holes in the periphery of the secondary particles, have about 8 space portions inside the secondary particles, and the connecting holes in the periphery are connected to the internal space portions.
[0273] [Coefficient of variation]
[0274] The cross section of the positive electrode active material (secondary particles) was sliced using an ion milling device (Cryo Ion Slicer, IB-09060CIS, manufactured by JEOL Ltd.) and a TEM (JEM-ARM200F, manufactured by JEOL Ltd.) was used. Figure 2 As shown, in the cross section of the secondary particles, for the primary particles of about 0.5 μm (two connected by the grain boundary), a total of 12 parts randomly selected from the primary particles including the grains in each primary particle and the grain boundary are irradiated with electron beams, and the energy of the characteristic X-rays of W generated is analyzed using EDX (made by Thermo Fisher Scientific Inc., NSS), and the average concentration (μ) of W in the whole of each primary particle, the standard deviation (σ) of the concentration of W, and the coefficient of variation (CV) of the concentration of W are analyzed. Table 1 shows the measurement results of the concentration of W obtained by TEM-EDX analysis of the obtained primary particles.
[0275] As a result, the average concentration (μ) of W was 1.0, the standard deviation (σ) of the concentration of W was 1.1, and the coefficient of variation (CV) of the concentration of W was 1.1.
[0276] Table 1
[0277] Add Element(W) 1 Grain Boundary 3.4 2 Grain Boundary 2.0 3 Grain Boundary 1.7 4 Grain Boundary 1.2 5 Intragranular 2.4 6 Intragranular 0.1 7 Intragranular 0.1 8 Intragranular 0.1 9 Intragranular 0.7 10 Intragranular 0.1 11 Intragranular 0.5 12 Intragranular 0.2 average μ 1.0 Standard Deviation σ 1.1 Coefficient of variation CV 1.1
[0278] [Volume of the connecting part per primary particle]
[0279] After a part of the positive electrode active material was buried in the thermosetting resin, three-dimensional SEM observation was performed under the following conditions.
[0280] <Device used>
[0281] ·Dual beam SEM-FIB device, Scios made by FEI Co., Ltd., Japan
[0282] <SEM observation conditions>
[0283] Accelerating voltage: 2kV
[0284] Current value: 0.1nA
[0285] Working distance: 7mm
[0286] Magnification: 10k (HFW: 20.7μm)
[0287] Number of pixels: X: 1536 × Y: 1024 (pixel size: X: 4.56nm × Y: 4.56nm)
[0288] Tilt angle: 52°
[0289] Dwell time: 30μs (1 scan)
[0290] Detector: Reflected electron detector
[0291] <FIB processing conditions>
[0292] Accelerating voltage: 30 kV
[0293] Current value: 100pA
[0294] Working distance: 19mm
[0295] Processing pitch: 30nm
[0296] The image analysis software "AVIZO" (manufactured by FEI Co., Ltd., Japan) was used to perform Y-axis tilt angle correction, XY alignment, removal of unnecessary areas, and upper and lower brightness adjustment to obtain a three-dimensional observation image. The voxel size of the obtained three-dimensional observation image was X: 13.49nm, Y: 17.12nm, and Z: 30nm.
[0297] A binary image is obtained from the obtained three-dimensional observation image through the following steps, and the obtained binary image is analyzed as follows to determine the volume of the connecting portion of each primary particle.
[0298] <Dimensional equivalence process>
[0299] The pixels were recalculated to make the pixel sizes of the X-axis, Y-axis, and Z-axis equivalent, and the recalculated voxel sizes were X: 13.49 nm, Y: 13.49 nm, and Z: 13.49 nm.
[0300] <Binarization process>
[0301] The three-dimensional observation image is binarized using the brightness difference between the region constituting the secondary particles and other regions (resin regions for embedding) to obtain a binary image. The binary image is smoothed by morphological processing using the above-mentioned image analysis software.
[0302] <Watershed Algorithm>
[0303] The binary image of the secondary particles is processed using the watershed algorithm based on the above-mentioned image analysis software to separate the connecting parts between the primary particles, thereby obtaining a binary image from which the primary particles are extracted (a binary image after the primary particles are separated). Further, based on the binary image before the primary particles are separated and the binary image after the primary particles are separated, a binary image of the connecting part of the primary particles is obtained. With respect to these binary images, a three-dimensional image is constructed based on the two-dimensional image corresponding to the depth direction in the Z-axis direction.
[0304] Next, by labeling processing using the above-mentioned image analysis software, the primary particles are distinguished by numbering from the binary image after the primary particles are separated, and their number is measured.
[0305] The total volume of the connecting part of the primary particles was divided by the number of primary particles obtained to obtain the value of the volume of the connecting part per primary particle. The result was 6.2×10 5 nm 3 .
[0306] d) Manufacturing of secondary batteries
[0307] Made Figure 5 Specifically, 52.5 mg of the positive electrode active material obtained as described above, 15 mg of acetylene black and 7.5 mg of PTFE were mixed and press-molded at a pressure of 100 MPa into a shape of 11 mm in diameter and 100 μm in thickness to produce the positive electrode 1.
[0308] Then, a 2032-type coin-shaped battery is manufactured in a glove box in an Ar environment with a dew point management of -60°C using the positive electrode 1. As the negative electrode 2 of the 2032-type coin-shaped battery, lithium metal with a diameter of 14 mm and a thickness of 1 mm is used, and as the non-aqueous electrolyte, an equal amount of a mixed solution of ethylene carbonate (EC) and diethyl carbonate (DEC) with 1M LiClO4 as a supporting electrolyte (manufactured by Ube Industries, Ltd.) is used. In addition, as a separator 3, a polyethylene porous film with a film thickness of 25 μm is used. As described above, a 2032-type coin-shaped battery 10 having a sealing gasket 4 and a corrugated gasket 5 and having a positive electrode can 6 and a negative electrode can 7 is assembled.
[0309] e) Battery evaluation
[0310] [Positive electrode resistance]
[0311] The positive electrode resistance was measured by charging a 2032-type coin-type battery at 3.8 V using an impedance measurement method, and then measured by an AC impedance method using a frequency response analyzer and a potentio galvanostat (1255B, manufactured by Solartron). Figure 6 The impedance spectrum shown in Figure 1 is shown in Figure 1. Since two semicircles are observed in the high-frequency and medium-frequency regions and a straight line is observed in the low-frequency region in the obtained impedance spectrum, it is possible to construct Figure 7 The equivalent circuit shown in the figure is used to analyze the positive electrode interface resistance. Here, Rs represents the bulk resistance, R1 represents the positive electrode film resistance, and R ctrepresents electrolyte / positive electrode interface resistance, W represents Warburg component, CPE1 and CPE2 represent constant phase angle elements. In addition, the positive electrode active material of Comparative Example 1 described later is used as a reference, and the resistance reduction rate of the positive electrode interface resistance relative to the reference is shown.
[0312] The overall composition and properties of the obtained positive electrode active material and the properties of the obtained lithium ion secondary battery are shown in Table 2. In addition, these properties of Examples 2 to 4 and Comparative Examples 1 and 2 are also shown in Table 1 in the same manner.
[0313] (Example 2)
[0314] A positive electrode active material was obtained and evaluated in the same manner as in Example 1 except that the lithium mixture was heated to 920° C. and maintained at this temperature for 3 hours for calcination.
[0315] (Example 3)
[0316] A positive electrode active material was obtained and evaluated in the same manner as in Example 2 except that a sodium tungstate aqueous solution was prepared so that the molar ratio of each metal element was Ni:Mn:Co:W=5.0:2.0:3.0:0.07.
[0317] (Example 4)
[0318] A positive electrode active material was obtained and evaluated in the same manner as in Example 1 except that crystallization was performed using an aqueous solution prepared by mixing a sodium tungstate aqueous solution with a raw material aqueous solution composed of Ni, Mn, and Co so as to achieve Ni:Mn:Co:W=5.0:2.0:3.0:0.1.
[0319] (Comparative Example 1)
[0320] In the crystallization process, the nucleation process and the switching operation 1 until the particle growth process are adjusted to an oxidizing environment with an oxygen concentration of 21 volume % for crystallization, and then adjusted to a non-oxidizing environment with an oxygen concentration of less than 2 volume % to obtain a composite hydroxide. Otherwise, the same operation as in Example 1 is performed to obtain a positive electrode active material, and it is evaluated. Figure 4 The particle structure of the obtained positive electrode active material is shown. It is confirmed that the positive electrode active material of Comparative Example 1 is formed by secondary particles, which are formed by agglomeration of a plurality of primary particles, and the positive electrode active material is composed of a hollow structure, which has one connecting hole in the peripheral portion of the secondary particle and one space portion inside the secondary particle, and the connecting hole in the peripheral portion is connected to the space portion inside.
[0321] (Comparative Example 2)
[0322] A positive electrode active material was obtained and evaluated in the same manner as in Example 1, except that crystallization was performed using an aqueous solution prepared by mixing a sodium tungstate aqueous solution with a raw material aqueous solution composed of Ni, Mn, and Co to achieve Ni:Mn:Co:W=5.0:2.0:3.0:0.12 and the calcination temperature was set to 900°C.
[0323]
[0324] It was confirmed that, when the positive electrode active materials of Examples 1 to 4 within the scope of the present invention were used in lithium ion secondary batteries, the positive electrode resistance was reduced and the output characteristics were improved compared with Comparative Examples 1 and 2.
[0325] Description of Reference Numerals
[0326] 1 Positive electrode (evaluation electrode)
[0327] 2 Negative electrode
[0328] 3 Spacer
[0329] 4 Gasket
[0330] 5 Wave washer
[0331] 6. Positive electrode tank
[0332] 7 Negative electrode tank
[0333] 10 Coin cell battery.
Claims
1. A positive electrode active material for a lithium ion secondary battery, wherein: The positive electrode active material is composed of composite oxide particles containing lithium transition metals. The composite oxide particles containing lithium transition metals have a general formula (A): Li 1+u Ni x Mn y Co z M t A composition represented by O2 and a layered rock salt type crystal structure, -0.05≤u≤0.5, x+y+z+t=1, 0.3≤x≤0.9, 0≤y≤0.5, 0≤z≤0.5, 0<t≤0.05, M is one or more additive elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta and W, The lithium-transition metal-containing composite oxide particles are composed of secondary particles, which are formed by agglomeration of primary particles. The secondary particles have: a 50% cumulative diameter d50 of 3.0 μm or more and 7.0 μm or less, as determined from a particle size distribution measurement value; 2.0 μm or less 2 / g or more and 5.0m 2 / g or less BET specific surface area; 1.0g / cm 3 Above and 2.0g / cm 3 A tap density of 30 mL / 100 g or more and 60 mL / 100 g or less; and an oil absorption of 30 mL / 100 g or more and 60 mL / 100 g or less, Among the primary particles, for a plurality of primary particles having a primary particle diameter within a range of 0.1 μm or more and 1.0 μm or less, when the concentration of the additional element M is measured at a plurality of locations by cross-sectional STEM or TEM-EDX analysis and a coefficient of variation is calculated, the coefficient of variation is 1.5 or less, the coefficient of variation being a value obtained by dividing the standard deviation of the concentration of the additional element M by the average concentration of the additional element M, Based on the binarized image obtained by binarizing the three-dimensional observation image of the secondary particles, the total volume of the connecting parts between the primary particles in the binarized image and the number of the primary particles in the binarized image are determined using a watershed algorithm. The volume of the connecting part of each primary particle obtained based on the total volume of the connecting parts between the primary particles in the binarized image and the number of the primary particles in the binarized image is 5×10 5 nm 3 Above and 9×10 7 nm 3 the following.
2. The positive electrode active material for lithium ion secondary battery according to claim 1, wherein The volume of the connecting part of each primary particle is 8×10 5 nm 3 Above and 9×10 6 nm 3 the following.
3. The positive electrode active material for lithium ion secondary battery according to claim 1 or 2, wherein The 50% cumulative diameter d50 of the secondary particles is 4.0 μm or more and 6.0 μm or less.
4. The positive electrode active material for lithium ion secondary battery according to claim 1 or 2, wherein [(d90-d10) / d50], which is an index representing the width of the particle size distribution of the secondary particles, is less than 1.0, where d10 is a 10% cumulative diameter obtained from the particle size distribution measurement value, and d90 is a 90% cumulative diameter obtained from the particle size distribution measurement value.
5. The positive electrode active material for lithium ion secondary battery according to claim 1 or 2, wherein The value of d90 / d10 of the secondary particles is 1.0 or more and 2.0 or less, d10 is a 10% cumulative diameter obtained from a particle size distribution measurement value, and d90 is a 90% cumulative diameter obtained from a particle size distribution measurement value.
6. The positive electrode active material for lithium ion secondary battery according to claim 1 or 2, wherein The secondary particle includes: an aggregated portion; one or more communicating holes communicating with the outer periphery of the aggregated portion; and two or more space portions existing inside the aggregated portion and communicating with the communicating holes.
7. The positive electrode active material for lithium ion secondary battery according to claim 1 or 2, wherein The additional element M is at least one selected from the group consisting of Mg, Al, Si, Ti, Zr, Nb, Mo and W.
8. The positive electrode active material for lithium ion secondary battery according to claim 1 or 2, wherein The additional element M is composed of W.
9. A lithium ion secondary battery, wherein: The battery comprises a positive electrode, a negative electrode, a separator and a non-aqueous electrolyte, or a positive electrode, a negative electrode and a solid electrolyte, wherein the positive electrode active material for a lithium ion secondary battery according to any one of claims 1 to 8 is used as a positive electrode active material for the positive electrode.
Citation Information
Patent Citations
Manganese composite hydroxide particle, positive pole active material for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery, and method for producing them
JP2012246199A
Transition metal-containing composite hydroxide particle and production method of the same, and positive electrode active substance for non-aqueous electrolyte secondary cell and production method of the same
JP2018104276A
Nickel-manganese composite hydroxide particles, method for producing same, positive electrode active material for nonaqueous electrolyte secondary batteries, method for producing positive electrode active material for nonaqueous electrolyte secondary
WO2012131881A1
Transition metal composite hydroxide particles, method for producing same, positive electrode active material for non-aqueous electrolyte secondary battery, method for producing same, and non-aqueous electrolyte secondary battery
WO2014181891A1
Nonaqueous Electrolytic Solution Secondary Battery
CN107039653A