Coil sealing resin composition, electronic component device, and method for producing electronic component device

By adding intramolecular salts of magnetic powder and arylphosphine to the resin composition for coil sealing, combined with a mold release agent, the problem of high melt viscosity change rate of resin composition in the prior art is solved, and low change rate and high change rate are achieved Stable resin compositions suitable for the manufacture of efficient electronic parts.

CN114450344BActive Publication Date: 2024-11-05RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080065467.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-09-20
Filing Date
2020-09-07
Publication Date
2024-11-05
Estimated Expiration
2040-09-07

AI Technical Summary

Technical Problem

The conventional resin composition for coil sealing increases the melt viscosity when using the mold, resulting in a high rate of melt viscosity change during long-term use and insufficient storage stability.

Method used

The resin composition containing magnetic powder, epoxy resin, hardener and intramolecular salt with arylphosphine as hardening accelerator is adopted. The magnetic powder content reaches more than 60%. Combined with a mold release agent to improve the hardening performance and fluidity of the resin. .

Benefits of technology

The coil sealing resin composition with low melt viscosity change rate and excellent storage stability is realized, and is suitable for manufacturing efficient electronic parts devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0003552043780000141
    Figure GDA0003552043780000141
  • Figure HDA0003552043790000011
    Figure HDA0003552043790000011
  • Figure HDA0003552043790000012
    Figure HDA0003552043790000012
Patent Text Reader

Abstract

The present invention provides a coil sealing resin composition having a low melt viscosity change rate over time and excellent storage stability, and an electronic component device and a method for manufacturing the electronic component device using the same. A coil sealing resin composition comprises magnetic powder, epoxy resin, a hardener, and a hardening accelerator, wherein the hardening accelerator comprises an intramolecular salt of a phosphine having an aromatic group.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a coil sealing resin composition, an electronic component device and a method for manufacturing the electronic component device. Background Art

[0002] The composite material including the metal powder and the resin composition can be used as a raw material for various industrial products such as inductors, electromagnetic shields, and bonded magnets, depending on the physical properties of the metal powder (see, for example, Patent Document 1).

[0003] In addition, a molded coil is disclosed, in which a coil is sealed using a magnetic molding resin in which magnetic powder is dispersed in the resin, and the magnetic molding resin contains 65 Vol% to 80 Vol% of the magnetic powder mainly comprising metal-based magnetic powder by volume (for example, refer to patent document 2).

[0004] [Prior art literature]

[0005] [Patent Document]

[0006] Patent Document 1: Japanese Patent Application Publication No. 2014-13803

[0007] Patent Document 2: Japanese Patent Application Publication No. 2009-260116 Summary of the invention

[0008] [Problems to be solved by the invention]

[0009] Patent Documents 1 and 2 disclose molded coils in which a coil is sealed using a resin composition containing magnetic powder and a resin. In the resin composition used for sealing such coils, it is desirable that the rate of change of melt viscosity over time is low and storage stability is excellent in order to suppress, for example, the unfilling of the resin composition caused by the increase in melt viscosity when the coil is sealed using a mold.

[0010] An object of one aspect of the present disclosure is to provide a coil sealing resin composition having a low melt viscosity change rate over time and excellent storage stability, and an electronic component device and a method for producing an electronic component device using the same.

[0011] [Technical means to solve the problem]

[0012] The specific means for achieving the above-mentioned subject are as follows.

[0013] <1> A coil sealing resin composition comprising a magnetic powder, an epoxy resin, a hardener, and a hardening accelerator, wherein the hardening accelerator comprises an intramolecular salt of a phosphine having an aromatic group.

[0014] <2> The coil sealing resin composition according to <1>, further comprising a release agent.

[0015] <3> The coil encapsulation resin composition according to <1> or <2>, wherein the content of the magnetic powder is 60% by mass or more based on the total amount of the coil encapsulation resin composition.

[0016] <4> The coil sealing resin composition according to any one of <1> to <3>, wherein the intramolecular salt comprises an intramolecular salt of triphenylphosphine.

[0017] <5> An electronic component device including: a coil; and a cured product of the coil sealing resin composition according to any one of <1> to <4> that seals the coil.

[0018] <6> A method for producing an electronic component device, comprising the step of sealing a coil using the coil sealing resin composition according to any one of <1> to <4>.

[0019] [Effects of the Invention]

[0020] According to one aspect of the present disclosure, there can be provided a coil sealing resin composition having a low melt viscosity change rate over time and excellent storage stability, an electronic component device using the same, and a method for producing the electronic component device. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a graph showing the relationship between the standing time and the minimum melt viscosity retention rate of the coil sealing resin compositions of Example 1 and Example 2 and Comparative Example 1 and Comparative Example 2 under the conditions of 25° C. and a relative humidity of 50%.

[0022] Figure 2 This is a graph showing the relationship between the standing time and the gel time retention rate of the coil sealing resin composition of Example 1 under the conditions of 25° C. and a relative humidity of 50% and 30° C. and a relative humidity of 70%.

[0023] Figure 3 This is a graph showing the relationship between the standing time and the gel time retention rate of the coil sealing resin composition of Example 2 under the conditions of 25° C. and 50% relative humidity and 30° C. and 70% relative humidity.

[0024] Figure 4 This is a graph showing the relationship between the standing time and the gel time retention rate of the coil sealing resin composition of Comparative Example 2 under the conditions of 25° C. and a relative humidity of 50% and 30° C. and a relative humidity of 70%. DETAILED DESCRIPTION

[0025] Hereinafter, the form for implementing the present invention is described in detail. However, the present invention is not limited to the following embodiments. In the following embodiments, its constituent elements (including element steps, etc.) are not necessarily required except for the cases specifically indicated. The same is true about numerical values ​​and their ranges, and the present invention is not limited thereto.

[0026] In the present disclosure, in a numerical range expressed using “to”, the numerical values ​​described before and after “to” are included as the minimum value and the maximum value, respectively.

[0027] In the numerical range recorded in stages in the present disclosure, the upper limit or lower limit recorded in one numerical range may also be replaced by the upper limit or lower limit of the numerical range recorded in other stages. In addition, in the numerical range recorded in the present disclosure, the upper limit or lower limit of the numerical range may also be replaced by the value shown in the embodiment.

[0028] In the present disclosure, each component may include a plurality of equivalent substances. When a plurality of substances equivalent to each component are present in the composition, unless otherwise specified, the content or content of each component refers to the total content or content of the plurality of substances present in the composition.

[0029] In the present disclosure, particles corresponding to each component may include multiple types of particles. When multiple types of particles corresponding to each component are present in the composition, the particle size of each component refers to the value for the mixture of the multiple types of particles present in the composition unless otherwise specified.

[0030] <Resin composition for coil sealing>

[0031] The coil sealing resin composition disclosed herein comprises magnetic powder, epoxy resin, hardener, and hardening accelerator, wherein the hardening accelerator comprises an intramolecular salt of a phosphine having an aromatic group. The coil sealing resin composition may further comprise other components as required. The coil sealing resin composition may also be a resin composition for sealing a coil and manufacturing an electronic component device.

[0032] The coil sealing resin composition disclosed in the present invention comprises an epoxy resin, a hardener, and a hardening accelerator, wherein the hardening accelerator comprises an intramolecular salt of a phosphine having an aromatic group, thereby having a low rate of change of melt viscosity over time and excellent storage stability. For example, the coil sealing resin composition disclosed in the present invention comprises a hardening accelerator, wherein the hardening accelerator comprises an intramolecular salt of a phosphine having an aromatic group, thereby having a low rate of change of melt viscosity over time and excellent storage stability compared with the following coil sealing resin composition, wherein the coil sealing resin composition comprises a hardening accelerator, wherein the hardening accelerator does not contain an intramolecular salt of a phosphine having an aromatic group but comprises an imidazole compound. The detailed reasons may not be clear, but it is believed that by using a hardening accelerator, wherein the hardening accelerator comprises an intramolecular salt of a phosphine having an aromatic group, the reactivity of the epoxy resin is improved in a specific temperature region rather than in a wide temperature range including normal temperature, so the rate of change of melt viscosity over time is low and the storage stability is excellent.

[0033] (Magnetic powder)

[0034] The coil sealing resin composition disclosed herein contains magnetic powder. The magnetic powder preferably contains at least one selected from the group consisting of a metal monomer, an alloy, and a metal compound. The specific gravity (density) of the magnetic powder may be, for example, 5 g / cm 3 The magnetic powder may be, for example, at least one selected from the group consisting of a metal monomer, an alloy, and a metal compound. The alloy may contain at least one selected from the group consisting of a solid solution, a eutectic, and an intermetallic compound. The alloy may be, for example, stainless steel (Fe-Cr alloy, Fe-Ni-Cr alloy, etc.). The metal compound may be, for example, an oxide such as ferrite. The magnetic powder may contain one metal element or multiple metal elements. Examples of the metal elements contained in the magnetic powder include base metal elements, noble metal elements, transition metal elements, and rare earth elements.

[0035] The coil sealing resin composition may contain one kind of magnetic powder or a plurality of kinds of magnetic powder.

[0036] Examples of the metal element contained in the magnetic powder include at least one selected from the group consisting of iron (Fe), copper (Cu), titanium (Ti), manganese (Mn), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), tin (Sn), chromium (Cr), niobium (Nb), barium (Ba), strontium (Sr), lead (Pb), silver (Ag), praseodymium (Pr), neodymium (Nd), samarium (Sm), and dysprosium (Dy). The magnetic powder may also contain elements other than metal elements. The magnetic powder may also contain at least one selected from the group consisting of, for example, carbon (C), oxygen (O), beryllium (Be), phosphorus (P), sulfur (S), boron (B), and silicon (Si).

[0037] The magnetic powder may also be a soft magnetic alloy or a ferromagnetic alloy. The magnetic powder may also be a magnetic powder including at least one selected from the group consisting of, for example, Fe-Si alloys, Fe-Si-Al alloys (such as Sendast alloys), Fe-Ni alloys (such as Permalloy), Fe-Cu-Ni alloys (such as Permalloy), Fe-Co alloys (such as Permendur), Fe-Cr-Si alloys (such as electromagnetic stainless steel), Nd-Fe-B alloys (such as rare earth magnets), Sm-Fe-N alloys (such as rare earth magnets), Al-Ni-Co alloys (such as AlNiCo magnets) and ferrites. Examples of ferrites include spinel ferrites, hexagonal ferrites and garnet ferrites.

[0038] The magnetic powder may also be Fe monomer. The magnetic powder may also be an alloy containing iron (Fe alloy). The Fe alloy may be, for example, a Fe-Si-Cr alloy or a Nd-Fe-B alloy. The magnetic powder may also be at least one of amorphous iron powder and carbonyl iron powder. When the magnetic powder contains at least one of Fe monomer and Fe alloy, it is easy to make a hardened material with a high space factor and excellent magnetic properties from the coil sealing resin composition. The magnetic powder may also be Fe amorphous alloy.

[0039] From the perspective of the magnetic properties when the electronic component device is made and the fluidity of the coil sealing resin composition, the content of the magnetic powder is preferably 60% by mass or more, more preferably 80% to 99% by mass, further preferably 90% to 98% by mass, and particularly preferably 94.5% to 97% by mass, relative to the total amount of the coil sealing resin composition.

[0040] The volume average particle size of the magnetic powder is not particularly limited, and may be, for example, 1 μm to 300 μm, 3 μm to 100 μm, or 4 μm to 50 μm.

[0041] In the present disclosure, the volume average particle size is obtained as the particle size (50%D) at which the accumulation from the small particle size side becomes 50% in the volume cumulative particle size distribution curve obtained by the laser diffraction scattering particle size distribution measurement method. For example, it can be measured using a particle size distribution measurement device using a laser light scattering method (for example, "SALD-3000" produced by Shimadzu Corporation (stock company)).

[0042] The shape of each particle constituting the magnetic powder is not limited, and may be, for example, spherical, flat, prism-shaped, or needle-shaped. The coil encapsulation resin composition may contain a plurality of types of magnetic powders having different volume average particle sizes.

[0043] (Epoxy resin)

[0044] The coil sealing resin composition of the present disclosure contains an epoxy resin. The epoxy resin may be, for example, a resin having two or more epoxy groups in one molecule.

[0045] The epoxy resin may be, for example, a biphenyl epoxy resin, a stilbene epoxy resin, a diphenylmethane epoxy resin, a sulfur-containing epoxy resin, a novolac epoxy resin, a dicyclopentadiene epoxy resin, a salicylaldehyde epoxy resin, a copolymerized epoxy resin of naphthols and phenols, an epoxide of an aralkyl phenol resin, a bisphenol epoxy resin, an epoxy resin containing a bisphenol skeleton, an alcohol glycidyl ether epoxy resin, a paraxylylene and / or metaxylene-modified phenol resin glycidyl ether epoxy resin, a terpene-modified At least one of the group consisting of glycidyl ether type epoxy resin of phenol resin, cyclopentadiene type epoxy resin, glycidyl ether type epoxy resin of polycyclic aromatic ring-modified phenol resin, glycidyl ether type epoxy resin of phenol resin containing naphthalene ring, glycidyl ester type epoxy resin, glycidyl type or methylglycidyl type epoxy resin, alicyclic epoxy resin, halogenated phenol novolac type epoxy resin, o-cresol novolac type epoxy resin, hydroquinone type epoxy resin, trimethylolpropane type epoxy resin, and linear aliphatic epoxy resin obtained by oxidizing olefin bonds with peracid such as peracetic acid.

[0046] From the perspective of fluidity, the epoxy resin may be at least one selected from the group consisting of biphenyl epoxy resins, o-cresol novolac epoxy resins, phenol novolac epoxy resins, bisphenol epoxy resins, epoxy resins having a bisphenol skeleton, salicylaldehyde novolac epoxy resins, and naphthol novolac epoxy resins; it may also be at least one selected from the group consisting of biphenyl epoxy resins and bisphenol epoxy resins; it may also be at least one selected from the group consisting of biphenylene aralkyl epoxy resins and bisphenol A epoxy resins.

[0047] The epoxy resin may also be a crystalline epoxy resin. Although the molecular weight of the crystalline epoxy resin is relatively low, the crystalline epoxy resin has a relatively high melting point and excellent fluidity. The crystalline epoxy resin (highly crystalline epoxy resin) may be, for example, at least one selected from the group consisting of a hydroquinone epoxy resin, a bisphenol epoxy resin, a thioether epoxy resin, and a biphenyl epoxy resin.

[0048] The epoxy equivalent of the epoxy resin is not particularly limited. From the viewpoint of balancing various properties such as moldability, heat resistance, and electrical reliability, the epoxy equivalent of the epoxy resin is preferably 60 g / eq to 1000 g / eq, more preferably 80 g / eq to 500 g / eq, and even more preferably 100 g / eq to 300 g / eq.

[0049] The epoxy resin weighed is dissolved in a solvent such as methyl ethyl ketone, acetic acid and tetraethylammonium bromide acetic acid solution are added, and then potentiometric titration is performed using a perchloric acid acetic acid standard solution to determine the epoxy equivalent of the epoxy resin. An indicator may also be used for the titration.

[0050] From the viewpoints of strength, fluidity, heat resistance, moldability, etc., the content of the epoxy resin in the coil sealing resin composition is preferably 0.5 to 20 mass %, more preferably 1 to 10 mass %, and further preferably 1.5 to 5 mass %.

[0051] (Hardener)

[0052] The coil sealing resin composition of the present disclosure contains a hardener.

[0053] The type of hardener is not particularly limited, and can be selected from hardeners commonly used as components of epoxy resin compositions. One hardener can be used alone, or two or more can be used in combination. Hardeners are classified into hardeners that harden epoxy resins in the range from low temperature to room temperature, and heat-hardening hardeners that harden epoxy resins with heating. Hardeners that harden epoxy resins in the range from low temperature to room temperature are, for example, aliphatic polyamines, polyaminoamides, and polythiol. Heat-hardening hardeners are, for example, aromatic polyamines, acid anhydrides, phenolic resins, and dicyandiamide (DICY).

[0054] When a curing agent that cures epoxy resin at a temperature ranging from low temperature to room temperature is used, the cured product obtained by curing the coil sealing resin composition tends to have a low glass transition temperature and be soft. In addition, a molded body formed from the coil sealing resin composition tends to be soft.

[0055] On the other hand, from the viewpoint of improving the heat resistance and mechanical strength of the molded body, the curing agent is preferably a heat-curing type curing agent, and more preferably a phenol resin.

[0056] The phenol resin may be, for example, at least one selected from the group consisting of aralkyl phenol resin, dicyclopentadiene phenol resin, salicylaldehyde phenol resin, novolac phenol resin, copolymerized phenol resin of benzaldehyde phenol and aralkyl phenol, p-xylene and / or m-xylene modified phenol resin, melamine modified phenol resin, terpene modified phenol resin, dicyclopentadiene naphthol resin, cyclopentadiene modified phenol resin, polycyclic aromatic ring modified phenol resin, biphenyl phenol resin and triphenylmethane phenol resin. In addition, the phenol resin may also include biphenyl phenol resin and triphenylmethane phenol resin. The phenol resin may also be a copolymer including two or more of the above.

[0057] The hardener may be, for example, a compound having two phenolic hydroxyl groups in one molecule. The compound having two phenolic hydroxyl groups in one molecule may be at least one selected from the group consisting of resorcinol, catechol, bisphenol A, bisphenol F, and substituted or unsubstituted diphenols.

[0058] The hydroxyl equivalent of the phenol resin is not particularly limited, but is preferably 10 to 1000 g / eq, more preferably 30 to 500 g / eq, from the viewpoint of balancing various properties such as moldability, heat resistance, and electrical reliability.

[0059] The hydroxyl equivalent of the phenol resin refers to a value calculated based on the hydroxyl value measured in accordance with Japanese Industrial Standards (JIS) K0070:1992.

[0060] The equivalent ratio of epoxy resin to hardener (the number of moles of epoxy groups of epoxy resin / the number of moles of active hydrogen of hardener) is not particularly limited. From the perspective of suppressing the unreacted components of each, it is preferably 0.5 to 1.5, more preferably 0.6 to 1.4, and further preferably 0.8 to 1.2. When the equivalent ratio is 0.5 or more, there is a tendency that the elastic coefficient of the hardened material obtained by hardening the coil sealing resin composition is excellent. On the other hand, when the equivalent ratio is 1.5 or less, there is a tendency that the mechanical strength of the hardened material decreases.

[0061] (hardening accelerator)

[0062] The coil sealing resin composition includes a hardening accelerator, and the hardening accelerator includes an intramolecular salt of a phosphine having an aromatic group. The intramolecular salt of a phosphine having an aromatic group is preferably an intramolecular salt of a phosphine containing at least one aromatic group bonded to a phosphorus element, and more preferably an intramolecular salt of a cation and an anion containing a phosphine skeleton containing at least one aromatic group bonded to a phosphorus element.

[0063] Examples of the aryl group in the phosphine having an aryl group include unsubstituted aryl groups and substituted aryl groups such as phenyl, p-tolyl, m-tolyl, o-tolyl, p-methoxyphenyl, m-methoxyphenyl, o-methoxyphenyl, p-hydroxyphenyl, m-hydroxyphenyl, o-hydroxyphenyl, 2,5-dihydroxyphenyl, 4-(4-hydroxyphenyl)phenyl, 1-naphthyl, 2-naphthyl, 1-(2-hydroxynaphthyl)yl, and 1-(4-hydroxynaphthyl)yl.

[0064] The phosphine having an aromatic group may also have an alkyl group bonded to the phosphorus element. Examples of the alkyl group include linear, branched, and cyclic alkyl groups such as methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, octyl, and cyclohexyl.

[0065] Examples of the phosphine having an aryl group include methyldiphenylphosphine, triphenylphosphine, tri(4-methylphenyl)phosphine, diphenylphosphine, and phenylphosphine. Among them, triphenylphosphine is preferred.

[0066] The intramolecular salt of a phosphine having an aryl group is preferably an intramolecular salt containing triphenylphosphine. As the intramolecular salt of triphenylphosphine, an intramolecular salt of a cation and an anion containing a triphenylphosphine skeleton is preferred.

[0067] Examples of the cation containing a triphenylphosphine skeleton include triphenylphosphine cations, and reaction products of triphenylphosphine and a compound having an aryl group. From the viewpoint of the melt viscosity change rate over time, the cation containing a triphenylphosphine skeleton is preferably a reaction product of triphenylphosphine and a compound having an aryl group.

[0068] The reaction product of triphenylphosphine and a compound having an aryl group is preferably a reaction product of triphenylphosphine and a compound having two hydroxyl groups and an aryl group, and more preferably a reaction product of triphenylphosphine and hydroquinone.

[0069] Examples of the anion include anions of aryl compounds having two or more carboxyl groups, aryl compounds having two or more hydroxyl groups, etc. More specifically, examples of the anion include anions of phthalic acid, benzene-1,2,4,5-tetracarboxylic acid, p-benzoquinone, and the like.

[0070] The content of the intramolecular salt of phosphine having an aromatic group in the hardening accelerator is not particularly limited as long as it is within the range that exhibits the effects of the present invention, and may be, for example, 50% by mass or more, 70% by mass or more, 90% by mass or more, or 100% by mass relative to the total amount of the hardening accelerator.

[0071] The content of the curing accelerator in the coil sealing resin composition is not particularly limited if it is an amount that can obtain a curing acceleration effect. From the viewpoint of the curing acceleration effect and storage stability, the content of the curing accelerator is preferably 0.1 to 10 parts by mass, more preferably 1 to 5 parts by mass, relative to 100 parts by mass of epoxy resin. In addition, from the viewpoint of the curing acceleration effect and storage stability, the content of the curing accelerator is preferably 0.05 to 5 parts by mass, more preferably 0.5 to 2.5 parts by mass, relative to a total of 100 parts by mass of epoxy resin and hardener (such as phenolic resin).

[0072] The hardening accelerator may include hardening accelerators other than the intramolecular salt of phosphine having an aromatic group (hereinafter referred to as "other hardening accelerators"). Other hardening accelerators include cyclic amidine compounds such as 1,8-diazabicyclo[5.4.0]-7-undecene (DBU), 1,5-diazabicyclo[4.3.0]-5-nonene, and 5,6-dibutylamino-1,8-diazabicyclo[5.4.0]-7-undecene; maleic anhydride added to the cyclic amidine compounds, 1,4-benzoquinone, 2,5-toluoquinone, 1,4-naphthoquinone, 2,3-dimethylbenzoquinone, 2,6-dimethylbenzoquinone, 2,3-dimethoxy-5-methyl-1,4-benzoquinone, 2,3-dimethoxy- Compounds with intramolecular polarization formed by quinone compounds such as 1,4-benzoquinone and phenyl-1,4-benzoquinone, compounds with π bonds such as diazonophenylmethane and phenol resins; tertiary amine compounds such as benzyldimethylamine, triethanolamine, dimethylaminoethanol, tris(dimethylaminomethyl)phenol; derivatives of tertiary amine compounds; imidazole compounds such as 2-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole; derivatives of imidazole compounds; organic phosphine compounds such as tributylphosphine; phosphorus compounds with intramolecular polarization formed by adding maleic anhydride to organic phosphine compounds, the quinone compounds, diazonophenylmethane, phenol resins and other compounds with π bonds, etc. Other hardening accelerators can be used alone or in combination of two or more.

[0073] (Release Agent)

[0074] The coil encapsulation resin composition of the present disclosure preferably further comprises a mold release agent. When the coil encapsulation resin composition comprises a mold release agent, the cured product can be easily separated from the mold during the process of producing a cured product from the resin composition using a mold or the like.

[0075] Examples of the release agent include polyolefins, fatty acids such as higher fatty acids, fatty acid esters, partially saponified fatty acid esters, fatty acid salts, fatty acid amides, alcohols, polyethers, polysiloxanes, fluorine compounds, metal soaps, and natural waxes. From the perspective of easily improving the fluidity of the coil sealing resin composition, the release agent preferably contains fatty acids.

[0076] The polyolefin may be, for example, at least one of polyethylene and polypropylene. The polyolefin may be, for example, at least one polar wax selected from the group consisting of oxidized polyethylene, grafted polyolefin, and copolymer. The polyolefin may be, for example, at least one of polyethylene and oxidized polyethylene.

[0077] The mold release agent may be, for example, a fatty acid selected from montanic acid, stearic acid, 12-hydroxystearic acid (12-oxystearic acid), lauric acid, or an ester thereof; a fatty acid salt selected from zinc stearate, calcium stearate, barium stearate, aluminum stearate, magnesium stearate, calcium laurate, zinc laurate, zinc linoleate, calcium ricinoleate, zinc 2-ethylhexanoate, or the like; stearic acid amide, oleic acid amide, erucic acid amide, behenic acid amide, palmitic acid amide, lauric acid amide, hydroxystearic acid amide, methylene bis stearic acid amide, ethylene bis stearic acid amide, ethylene bis lauric acid amide, di-stearic acid amide, ethylene bis stearic acid amide, ethylene bis lauric acid amide, stearic acid amide, oleic acid amide, erucic acid amide, behenic acid amide, palmitic acid amide, lauric acid amide, hydroxystearic acid amide, methylene bis stearic acid amide, ethylene bis stearic acid amide, ethylene bis lauric acid amide, stearic acid amide, ethylene bis lauric acid amide, stearic acid amide, oleic acid amide, erucic acid amide, behenic acid amide, palmitic acid amide, lauric acid amide, hydroxystearic acid amide, m ... Fatty acid amides such as adipic acid amide, ethylenebisoleic acid amide, dioleyl adipamide, N-stearyl stearic acid amide, N-oleyl stearic acid amide, N-stearyl erucic acid amide, hydroxymethyl stearic acid amide, hydroxymethyl behenic acid amide; fatty acid esters such as butyl stearate; alcohols such as ethylene glycol and stearyl alcohol; polyethers including polyethylene glycol, polypropylene glycol, polytetramethylene glycol and their modified products; polysiloxanes such as silicone oil and silicone ester; fluorine compounds such as fluorine oil, fluorine ester and fluorine-containing resin powder; and at least one of the group consisting of waxes such as paraffin wax, amide wax, ester wax, carnauba wax and microcrystalline wax.

[0078] The release agent contained in the coil encapsulating resin composition can be appropriately selected according to the requirements for composition design such as the fluidity and releasability of the coil encapsulating resin composition, the temperature and pressure during molding, the melting point and melt viscosity of the release agent.

[0079] When the coil sealing resin composition contains a release agent, from the viewpoint of the releasability and mechanical strength of the cured product, the content of the release agent is preferably 0.01% by mass to 0.5% by mass, more preferably 0.05% by mass to 0.3% by mass, and further preferably 0.1% by mass to 0.2% by mass relative to the total amount of the coil sealing resin composition.

[0080] When the coil sealing resin composition contains a release agent, the content of the release agent is preferably 0.5% to 20% by mass, more preferably 1% to 10% by mass, and even more preferably 3% to 7% by mass relative to the total amount of the epoxy resin from the viewpoint of the releasability and mechanical strength of the cured product.

[0081] [Various additives]

[0082] In addition to the above components, the coil sealing resin composition may also contain various additives such as resins other than the epoxy resin and hardener exemplified below (hereinafter, also referred to as "other resins"), coupling agents, ion exchangers, mold release agents, flame retardants, colorants, and stress relaxants. In addition to the additives exemplified below, the coil sealing resin composition may also contain various additives known in the technical field as needed.

[0083] (Other resins)

[0084] The coil sealing resin composition may also contain resins other than epoxy resin and hardener, i.e., other resins. Examples of other resins include silicone resins, polyamide resins, polyamide-imide resins, thermoplastic resins, and the like. The thermoplastic resin may be, for example, at least one selected from the group consisting of acrylic resins, polyethylene, polypropylene, polystyrene, polyvinyl chloride, and polyethylene terephthalate. The resin composition may contain both thermosetting resins and thermoplastic resins. The resin composition may also contain silicone resins.

[0085] (Coupling agent)

[0086] When the coil sealing resin composition contains an inorganic filler, a coupling agent may be contained in order to improve the adhesion between the resin component and the magnetic powder. Examples of the coupling agent include silane compounds such as epoxysilane, mercaptosilane, aminosilane, alkylsilane, ureide silane, and vinylsilane, titanium compounds, aluminum chelate compounds, and aluminum / zirconium compounds.

[0087] (Method for preparing coil sealing resin composition)

[0088] There is no particular restriction on the preparation method of the coil sealing resin composition. When the coil sealing resin composition is solid, as a general method, the following method can be cited: after the components of the specified formulation amount are fully mixed by a mixer, etc., melt-kneading is performed by a mixing roller, an extruder, etc., and then cooled and crushed. More specifically, for example, the following method can be cited: the specified amount of the components is uniformly stirred and mixed, and kneaded by a kneader, roller, extruder, etc. pre-heated to 70°C to 140°C, and then cooled and crushed.

[0089] When the coil sealing resin composition is in liquid form, a general method includes weighing the components in a predetermined amount, dispersing and kneading them by a three-roll mill, a pestle, a planetary mixer, a hard mixer, a homogenizer, etc. In addition, in terms of uniform dispersibility and fluidity, it is preferred to use a masterbatch in which each of the ingredients is pre-dispersed and pre-heated.

[0090] The shape of the coil encapsulation resin composition when solid is not particularly limited, and examples thereof include powder, granules, and sheets. From the viewpoint of workability, the coil encapsulation resin composition when in sheet form preferably has dimensions and mass that meet the molding conditions of the package.

[0091] <Electronic components and devices>

[0092] The electronic component device of the present disclosure includes: a coil; and a cured product of the coil sealing resin composition of the present disclosure that seals the coil. The electronic component device of the present disclosure can be obtained, for example, by curing the coil sealing resin composition that covers at least a portion of the coil.

[0093] The cured product can be obtained by, for example, heating the coil sealing resin composition at 100° C. to 250° C. for 1 to 10 hours, preferably at 130° C. to 230° C. for 1 to 8 hours.

[0094] The electronic component device of the present disclosure can be obtained, for example, by filling the coil sealing resin composition of the present disclosure into a mold provided with a coil and curing the coil sealing resin composition filled into the mold. In this case, the coil sealing resin composition of the present disclosure has a low rate of change of melt viscosity over time and excellent storage stability, so it has excellent filling properties into the mold and a tendency to have excellent productivity of the electronic component device.

[0095] The electronic component device disclosed in the present invention may also be a molded coil obtained by sealing the coil using a coil sealing resin composition. For example, a molded coil can be listed as one obtained by sealing the following component parts using a coil sealing resin composition, wherein the component parts are obtained by mounting active components such as semiconductor chips, transistors, diodes, thyristors, capacitors, resistors, etc., and passive components such as the like on supporting members such as lead frames, wired conveyor tapes, wiring boards, glass, silicon wafers, and organic substrates together with the coil.

[0096] <Method for manufacturing electronic component device>

[0097] The method for manufacturing an electronic component device of the present disclosure includes the step of sealing a coil using the coil sealing resin composition of the present disclosure. The coil sealing resin composition of the present disclosure is suitable as a sealing material for a coil.

[0098] Examples of a method for sealing a coil using a solid coil sealing resin composition include a low-pressure transfer molding method, an injection molding method, and a compression molding method.

[0099] [Example]

[0100] Next, the present invention will be specifically described by way of examples, but the scope of the present invention is not limited to these examples. In addition, "parts" and "%" are based on mass unless otherwise specified.

[0101] Details of the epoxy resin, hardener, hardening accelerator, silane compound, release agent, and magnetic powder used in Examples and Comparative Examples are as follows.

[0102] (Epoxy resin)

[0103] Epoxy resin A···Biphenylene aralkyl type epoxy resin (epoxy equivalent 277g / eq)

[0104] Epoxy resin B···Trifunctional bisphenol A type epoxy resin (epoxy equivalent 205g / eq~215g / eq)

[0105] (Hardener)

[0106] Hardener A: Biphenyl type phenol resin (hydroxyl equivalent 202 g / eq)

[0107] Hardener B: Triphenylmethane type phenol resin (hydroxyl equivalent 103 g / eq)

[0108] (hardening accelerator)

[0109] Hardening accelerator A: Intramolecular salt of the reaction product of triphenylphosphine and hydroquinone and phthalate anion

[0110] Hardening accelerator B···Intramolecular salt of triphenylphosphine and p-benzoquinone

[0111] Hardening accelerator C···2-heptadecylimidazole

[0112] Hardening accelerator D···2-phenyl-4-methylimidazole

[0113] Hardening accelerator E···2-phenyl-4-methyl-5-hydroxymethylimidazole

[0114] (Silane compound)

[0115] Silane compound A···3-glycidyloxypropyltrimethoxysilane

[0116] Silane compound B···3-Mercaptopropyltrimethoxysilane

[0117] (Release Agent)

[0118] Release Agent A···Zinc Laurate

[0119] Release agent B···Partially saponified montanic acid ester

[0120] (Magnetic powder)

[0121] Magnetic powder 1...Amorphous iron powder (volume average particle size 24 μm)

[0122] Magnetic powder 2...Amorphous iron powder (volume average particle size 5.3 μm)

[0123] [Example 1]

[0124] (Preparation of resin mixture)

[0125] 50 parts of epoxy resin A, 50 parts of epoxy resin B, 41.6 parts of hardener A, 21.8 parts of hardener B, 2 parts of hardening accelerator A, 4 parts of release agent A and 2 parts of release agent B were put into a plastic container. The resin mixture was prepared by mixing these raw materials in the plastic container for 10 minutes. In the above embodiment, the resin mixture corresponds to all the other components of the coil sealing resin composition except the magnetic powder and the coupling agent.

[0126] (Preparation of Coil Sealing Resin Composition)

[0127] A pressurized twin-shaft kneader (manufactured by Nihon Spindle Manufacturing Co., Ltd., with a capacity of 5 L) was used to mix a total of 4737 parts of magnetic powder 1 and magnetic powder 2 (the mixing ratio was 82:18 by mass) for 5 minutes to prepare magnetic powder. A mixture of 4.5 parts of silane compound A and 1 part of silane compound B (the mixing ratio is as described in Table 1) was added to the magnetic powder in the twin-shaft kneader. Then, the contents of the twin-shaft kneader were heated to 70°C, and the contents of the twin-shaft kneader were mixed for 10 minutes while maintaining the temperature. Then, the resin mixture was added to the contents of the twin-shaft kneader, and the contents were melted and kneaded for 15 minutes while maintaining the temperature of the contents at 90°C. After the mixture obtained by the above melting and kneading was cooled to room temperature, the mixture was crushed with a hammer until the mixture had a specified particle size to prepare a resin composition for coil sealing. The term "melting" means melting of at least a portion of the resin composition in the content of the biaxial kneader. The magnetic powder in the coil sealing resin composition does not melt during the preparation process of the coil sealing resin composition.

[0128] [Example 2]

[0129] In Example 1, a coil sealing resin composition was prepared in the same manner as in Example 1 except that 2.4 parts of curing accelerator B was used instead of 2 parts of curing accelerator A to change the total amount of magnetic powder 1 and magnetic powder 2 so that the mass ratio of the magnetic powder in the coil sealing resin composition became 96.4%.

[0130] [Comparative Example 1]

[0131] In Example 1, except that the hardening accelerator C and the hardening accelerator D in the amounts shown in Table 1 were used instead of the hardening accelerator A, a coil sealing resin composition was prepared in the same manner as in Example 1.

[0132] [Comparative Example 2]

[0133] In Example 1, except that the curing accelerator E was used instead of the curing accelerator A, a coil sealing resin composition was prepared in the same manner as in Example 1.

[0134] In Table 1, "magnetic powder / %" refers to the total content of magnetic powder 1 and magnetic powder 2 relative to the total amount of the coil sealing resin composition. In addition, the numerical values ​​of epoxy resin, hardener, hardening accelerator, silane compound and release agent in Table 1 refer to the mass parts of each used in the preparation of the coil sealing resin composition, and further refer to the mass ratio of each other except the magnetic powder in the coil sealing resin composition.

[0135] In Table 1, blank columns indicate "not blended".

[0136] [Table 1]

[0137] raw material Example 1 Example 2 Comparative Example 1 Comparative Example 2 Epoxy Resin A 50 50 50 50 Epoxy resin B 50 50 50 50 Hardener A 41.6 41.6 41.6 41.6 Hardener B 21.8 21.8 21.8 21.8 Hardening accelerator A 2.0 Hardening accelerator B 2.4 Hardening accelerator C 1.2 Hardening accelerator D 1.2 Hardening accelerator E 2.0 Silane Compound A 4.5 4.5 4.5 4.5 Silane compound B 1.0 1.0 1.0 1.0 Release Agent A 4.0 4.0 4.0 4.0 Release Agent B 2.0 2.0 2.0 2.0 (Magnetic powder / %) 96.4 96.4 96.4 96.4 Magnetic powder 1 3884.3 3893.1 3893.1 3884.3 Magnetic powder 2 852.7 854.6 854.6 852.7

[0138] (Determination of minimum melt viscosity)

[0139] The coil sealing resin composition of each embodiment and comparative example was used to measure the minimum melt viscosity at 130°C. The results are shown in Table 2 below. The minimum melt viscosity was measured using a flow tester CFT-100 (manufactured by Shimadzu Corporation) under the conditions of 130°C, 20 seconds of residual heat, and a load of 100 kg. In addition, the plunger's insertion distance (unit: mm) until the flow of the coil sealing resin composition stops was measured as the stroke. The stroke becomes an indicator of fluidity.

[0140] (Evaluation of Minimum Melt Viscosity Retention Rate over Time)

[0141] The coil sealing resin composition of each embodiment and comparative example was used to evaluate the minimum melt viscosity retention rate over time. The coil sealing resin composition was placed at 25°C and relative humidity of 50% for 24 hours, 48 ​​hours, 72 hours, 96 hours and 120 hours, and the minimum melt viscosity at 130°C was measured. The minimum melt viscosity retention rate was calculated based on the following formula.

[0142] Minimum melt viscosity retention rate = (minimum melt viscosity of the coil sealing resin composition after standing for a predetermined time / minimum melt viscosity of the coil sealing resin composition before standing) × 100

[0143] The results are shown in Figure 1 The smaller the value of the minimum melt viscosity retention rate is, the smaller the change in the minimum melt viscosity over time is, and the better the storage stability is.

[0144] (Determination of gel time)

[0145] The coil sealing resin composition of each example and comparative example was used to measure the gel time at 140° C. The gel time of the coil sealing resin composition was measured using a curelastometer (manufactured by JSR Trading Co., Ltd.) under the conditions of a sample volume of 1.5 ml and 140° C. The time at which the torque in the obtained graph starts to rise was defined as the gel time (sec).

[0146] The results are shown in Table 2 below.

[0147] (Evaluation of Gel Time over Time)

[0148] The coil sealing resin compositions of Example 1, Example 2 and Comparative Example 2 were used to evaluate the gel time over time. The coil sealing resin compositions were placed at 25°C and relative humidity of 50% for 24 hours, 48 ​​hours, 72 hours, 96 hours and 120 hours, respectively, and the coil sealing resin compositions were placed at 30°C and relative humidity of 70% for 12 hours, 24 hours, 48 ​​hours and 72 hours, respectively, and the gel time at 140°C was measured. The gel retention rate was calculated based on the following formula.

[0149] Gel time retention rate = (Gel time of the coil sealing resin composition after being left for a predetermined time / Gel time of the coil sealing resin composition before being left for a predetermined time) × 100

[0150] The results are shown in Figure 2 to Figure 4 middle.

[0151] (High temperature bending test)

[0152] The coil sealing resin composition of each embodiment and comparative example at 140°C was used and a test piece was obtained by transfer molding. The test piece is a rectangular parallelepiped (rod) containing a cured product after the coil sealing resin composition was cured at 180°C for 2 hours. The pressure applied to the composite was 13.5MPa. The dimensions of the test piece were 80mm in length × 10mm in width × 3.0mm in thickness. A three-point support type bending test was performed on the test piece using an autograph with a constant temperature bath. The autograph used was AGS-500A manufactured by Shimadzu Corporation. The temperature of the constant temperature bath was 250°C. In the bending test, one side of the test piece was supported by two fulcrums. A load was applied at the center between the two fulcrums on the other side of the test piece. The load when the test piece was destroyed was measured. The measurement conditions of the bending test are as follows.

[0153] The distance between the two fulcrums Lv: 64.0±0.5mm

[0154] Head speed: 2.0±0.2mm / min

[0155] Chart speed: 100mm / min

[0156] Chart full scale: 490N (50kgf)

[0157] The bending strength σ (unit: MPa) is calculated based on the following formula (A). The bending elastic coefficient E (unit: GPa) is calculated based on the following formula (B). In the following formula, "P" is the load when the test piece is broken (unit: N). "Lv" is the distance between the two fulcrums (unit: mm). "W" is the horizontal width of the test piece (unit: mm). "t" is the thickness of the test piece (unit: mm). "F / Y" is the gradient of the straight line portion of the load-deflection curve (unit: N / mm).

[0158] σ=(3×P×Lv) / (2×W×t 2 ) (A)

[0159] E=[Lv 3 / (4×W×t 3 )]×(F / Y) (B)

[0160] (Evaluation of elastic modulus and strength balance)

[0161] In terms of the reliability of coil sealing, the cured product of the coil sealing resin composition preferably has a low flexural modulus and high flexural strength at high temperatures. Whether the flexural modulus and flexural strength are well balanced can be evaluated based on the calculated values ​​of the reliability index formula shown below.

[0162] Reliability index = (bending strength (MPa) ÷ bending elastic coefficient (GPa))

[0163] Table 2 shows the results.

[0164] Furthermore, the calculated value of the formula of the reliability index can be evaluated as follows.

[0165] The calculated value is less than 10×10 -3 ···Poor balance between elastic modulus and strength.

[0166] The calculated value is 10×10 -3 Above and 11×10 -3 The following... The balance between elastic modulus and strength is slightly excellent.

[0167] The calculated value exceeds 11×10 -3 ···Excellent balance between elastic modulus and strength.

[0168] [Table 2]

[0169]

[0170] like Figure 1 As shown, the coil sealing resin compositions of Examples 1 and 2 have lower minimum melt viscosity retention rates than the coil sealing resin compositions of Comparative Examples 1 and 2. Therefore, the coil sealing resin compositions of Examples 1 and 2 have small changes in minimum melt viscosity over time and are excellent in storage stability.

[0171] Furthermore, if Figure 2 to Figure 4 As shown, the coil sealing resin compositions of Examples 1 and 2 have a larger value of the gel time retention rate than the coil sealing resin composition of Comparative Example 2. Therefore, the coil sealing resin compositions of Examples 1 and 2 are excellent in storage stability.

[0172] As shown in Table 2, the molded products formed using the coil sealing resin compositions of Examples 1 and 2 have greater reliability index values ​​than the molded products formed using the coil sealing resin compositions of Comparative Examples 1 and 2. Therefore, it is shown that by using the coil sealing resin compositions of Examples 1 and 2, a molded product having an excellent balance between the flexural modulus and the flexural strength at high temperatures and high reliability can be obtained.

[0173] The entire contents of the disclosure of Japanese Patent Application No. 2019-171448 filed on September 20, 2019 are incorporated into this specification by reference.

[0174] All documents, patent applications, and technical specifications described in this specification are incorporated into this specification by reference to the same extent as if each document, patent application, or technical specification was specifically and individually described as being incorporated by reference.

Claims

1. A coil sealing resin composition comprising Magnetic powder, Epoxy resin, Hardener, and a hardening accelerator comprising an intramolecular salt of a phosphine having an aromatic group, The intramolecular salt of phosphine having an aromatic group is a triphenylphosphine cation, or a cation of a reaction product of triphenylphosphine and hydroquinone, and an anion of an aromatic compound having two or more carboxyl groups or an aromatic compound having two or more hydroxyl groups. 2 . The coil sealing resin composition according to claim 1 , further comprising a release agent. 3 . The coil sealing resin composition according to claim 1 , wherein the content of the magnetic powder is 60% by mass or more based on the total amount of the coil sealing resin composition. 4 . The coil sealing resin composition according to claim 1 , wherein the anion of the intramolecular salt of the anion contains phthalic acid, benzene-1,2,4,5-tetracarboxylic acid or p-benzoquinone.

5. An electronic component device comprising: Coil; and a cured product of the coil sealing resin composition according to any one of claims 1 to 4 for sealing the coil. 6 . A method for producing an electronic component device, comprising the step of sealing a coil using the coil sealing resin composition according to claim 1 .