A kind of LED transparent circuit board and preparation method thereof

By using pressure-sensitive thermally conductive insulating film and copper foil hot compress and die-cutting technology, LED transparent circuit boards are prepared, combined with multi-stage step-curing technology, the problems of complex processes, high energy consumption and high cost in the existing technology are solved, and high Performance, low-cost LED transparent circuit board preparation.

CN114516204BActive Publication Date: 2024-11-15TONGCHUAN SUPERLUMINAL LAMINATE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210085964.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-25
Publication Date
2024-11-15
Estimated Expiration
2042-01-25

AI Technical Summary

Technical Problem

The production process of existing LED transparent glass displays is complex, with high energy consumption and high cost, and the resistance of the ITO conductive film is large and poor thermal conductivity, making it difficult to apply glass displays on a large scale.

Method used

The pressure-sensitive thermally conductive insulating film and copper foil are used to form glued copper foil. The circuit pattern is prepared through die-cutting technology and is combined with a transparent glass substrate. The LED transparent circuit board is prepared by a multi-stage step curing process to replace the traditional ITO conductive film. and chemical etching process.

Benefits of technology

It improves the dimensional stability and surface appearance of the circuit board, reduces costs, reduces energy consumption, improves processing efficiency and raw material recovery, solves pollution problems in traditional processes, and improves bonding and thermal conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003487941800000121
    Figure BDA0003487941800000121
  • Figure BDA0003487941800000131
    Figure BDA0003487941800000131
Patent Text Reader

Abstract

The present invention discloses a method for preparing a transparent LED circuit board, comprising the following steps: hot-compressing a pressure-sensitive thermally conductive insulating adhesive film and a copper foil to form a copper foil with adhesive; laminating the smooth surface of the copper foil with adhesive on a protective film by a laminating machine, and die-cutting the copper foil with adhesive by a die-cutting technique to obtain a circuit pattern of the copper foil with adhesive; taking a transparent glass substrate and a circuit pattern of the copper foil with adhesive, and compounding the transparent glass substrate with the circuit pattern of the copper foil with adhesive by a hot-compressing machine to bond the transparent glass substrate to the copper foil circuit pattern; removing the protective film after cooling to obtain an uncured glass-based circuit board; and subjecting the uncured glass-based circuit board to a multi-stage step curing process to obtain an LED transparent circuit board. The method for preparing a transparent LED circuit board provided by the present invention solves the problems of complex process, high energy consumption, high cost, pollution, etc. in the traditional process, and the prepared transparent circuit board has excellent performance. The present invention also provides an LED transparent circuit board prepared by the above-mentioned preparation method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of circuit boards, and in particular to an LED transparent circuit board and a preparation method thereof. Background Art

[0002] With the development of science and technology, the types of LED display screens are becoming more and more abundant and more and more common in life. LED transparent glass display screens have the advantages of being waterproof, dustproof and high strength. At the same time, their good light transmittance will not affect the indoor lighting of buildings. They are widely used in the fields of building screens and bridge decoration. Among them, glass display screens not only have the advantages of high transparency, few control lines, and simple control, but also have the characteristics of light weight, low price, easy transportation and installation. Compared with traditional LED display screens, they have further application value.

[0003] The surface of glass treated at high temperature is "smooth", and its surface can be considered "inert", with the characteristics of poor adhesion, low bonding force and high strength. In the prior art, the manufacturing process of glass display screens is mainly: first treat the glass surface, and then coat it with ITO conductive film, which has extremely low resistivity, light transmittance and high color development rate. The ITO coating thickness is 300-500um, and then use laser focusing energy to make the irradiated part of the area to be processed instantly vaporize, and fill or other treatments are performed in the groove to achieve the purpose of etching processing. In general, the circuit occupies 10% of the total area. After ITO coating, the circuit part is retained and the rest is etched away. The ITO conductive film has the disadvantages of high preparation cost, difficulty in large-size production, large square resistance, etc., and the used part is small, which increases the overall cost price, making it difficult for glass display screens to be accepted by the public.

[0004] In addition, there are problems with the electroplating circuit. Its resistance is large, its thermal conductivity is poor, it is more prone to board explosion, and its life is short. The surface deformation of the copper plated layer is greater than 25%, resulting in a large overall cross-sectional area and thus a large resistance. A large amount of heat energy is released during operation, and the photoelectric conversion efficiency is low.

[0005] Therefore, a new thin film material or adhesive material is needed to replace the application of ITO on glass substrates, or a new process is provided to replace the original etching process so that its processing accuracy is much higher than the traditional chemical etching method and it will not cause damage to the substrate. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide an LED transparent circuit board and a preparation method thereof, which solves the problems of complex process, high energy consumption, high cost and the like in traditional processes, and the prepared transparent circuit board has excellent performance.

[0007] In order to solve the above problems, the technical solution of the present invention is as follows:

[0008] A method for preparing an LED transparent circuit board comprises the following steps:

[0009] Step S1, heat-compressing the pressure-sensitive thermally conductive insulating adhesive film and the copper foil together to form an adhesive-coated copper foil;

[0010] Step S2, laminating the smooth surface of the adhesive copper foil on the protective film by a laminating machine, and die-cutting the adhesive copper foil by a die-cutting technology, removing the excess adhesive copper foil after die-cutting, and retaining the required circuit pattern on the protective film to obtain the adhesive copper foil circuit pattern;

[0011] Step S3, taking the transparent glass substrate and the adhesive copper foil circuit pattern, and using a hot compressing machine to compound the transparent glass substrate and the adhesive copper foil circuit pattern, so that the transparent glass substrate and the copper foil circuit pattern are bonded;

[0012] Step S4, removing the protective film after cooling to obtain an uncured glass-based circuit board;

[0013] Step S5, subjecting the uncured glass-based circuit board to a multi-stage step curing process to obtain an LED transparent circuit board.

[0014] Furthermore, in step S5, the multi-stage step curing process is: the first stage is cured at 70-80°C for 40-60 minutes, the second stage is cured at 90-100°C for 40-60 minutes, the third stage is cured at 110-120°C for 20-30 minutes, the fourth stage is cured at 140-150°C for 20-30 minutes, and the fifth stage is cured at 165-170°C for 30-40 minutes.

[0015] Furthermore, the pressure-sensitive thermally conductive insulating adhesive film includes the following components in parts by weight:

[0016] 50-60 parts of GELR125 epoxy resin, 30-40 parts of silicone modified epoxy resin, 10-20 parts of polyurethane modified epoxy resin, 20-30 parts of phenolic resin curing agent, 0.1-0.5 parts of urea accelerator, 200-240 parts of alumina powder, wherein the particle size of the alumina powder is 1-10 μm.

[0017] Furthermore, the preparation process of the pressure-sensitive thermally conductive insulating adhesive film is as follows:

[0018] The raw materials of the pressure-sensitive thermally conductive insulating adhesive film are mixed evenly to obtain a colloid material;

[0019] The obtained colloid material is cast on a release film at 60-70° C. to obtain a pressure-sensitive thermally conductive insulating adhesive film.

[0020] Furthermore, the thickness of the pressure-sensitive thermally conductive insulating adhesive film is 50-80 μm.

[0021] Furthermore, in step S1, a hot compress machine is used to perform hot compress at 55-65° C. to form a copper foil with glue.

[0022] Furthermore, in step S3, the transparent glass substrate and the adhesive copper foil circuit pattern are compounded at 55-65° C. using a hot compress machine.

[0023] The present invention also provides an LED transparent circuit board, which is prepared by the above preparation method.

[0024] Compared with the prior art, the LED transparent circuit board and the preparation method thereof provided by the present invention have the following beneficial effects:

[0025] 1. The preparation method of the LED transparent circuit board provided by the present invention is to compound the circuit pattern obtained by die-cutting the copper foil with glue with a pressure-sensitive thermally conductive insulating adhesive film with a transparent glass substrate, and then pass a multi-stage curing process, so that the prepared circuit board has good dimensional stability and surface appearance; in specific applications, the size of the copper foil circuit pattern that can be die-cut can reach 10m×10m, so it can avoid the patchwork problem in the application of the substrate, improve the integrity and reliability of the product, and complete the assembly line production operation while reducing costs, thereby overcoming the intermittent production efficiency problem of the traditional process. And the preparation method of the present invention adopts a multi-stage step curing process, cancels the traditional vacuum hot pressing of the press, thereby further reducing costs and improving work efficiency by 1 / 4; multi-stage gradient curing, because no pressure is applied during the curing process, the reaction rate is slowed down, thereby improving the compactness of the glue during the reaction process, so that the thickness of the glue layer before and after the reaction remains basically unchanged, thereby improving the peeling strength of the circuit board.

[0026] 2. Compared with the traditional chemical etching process, the preparation method of the LED transparent circuit board provided by the present invention does not require chemical etching, exposure and development processes. There are no toxic and harmful volatile products in the production process, as well as organic acids, alkalis and heavy metal waste liquids generated by etching, which solves the problem of serious pollution and achieves green environmental protection to a great extent. The process of the present invention only involves hot compressing and baking curing, which greatly reduces energy consumption, and at the same time requires less processing equipment and less equipment investment.

[0027] 3. The preparation method of the LED transparent circuit board provided by the present invention is that the copper foil residue after die-cutting is easy to recycle and the recycling process is simple (for example, directly melting it into copper ingots), the reuse rate of raw materials is improved, and compared with the existing etching process, there is no need to purify the etching copper liquid, which improves the recovery rate of raw materials and saves raw materials and energy consumption.

[0028] Fourth, the preparation method of the LED transparent circuit board provided by the present invention adopts a pressure-sensitive thermally conductive insulating adhesive film, which has excellent bonding performance and thermal conductivity, and effectively solves the bonding problem between the insulating medium layer and the circuit copper foil in the traditional process method. The circuit board prepared by the present invention has a greatly improved peeling strength between the copper foil circuit pattern and the glass substrate.

[0029] 5. In the present invention, the high thermal conductivity insulating pressure-sensitive film used has excellent adhesive properties and thermal conductivity. The prepared transparent circuit board has a peel strength of up to 1.42N / mm, a thermal conductivity of 1.7W / m·k, and a transparent glass circuit board with a light transmittance of up to 86%. DETAILED DESCRIPTION

[0030] In order to enable those skilled in the art to better understand the technical solutions in the embodiments of the present invention and to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific implementation modes of the present invention are further described below.

[0031] It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as there is no conflict between them.

[0032] A method for preparing a transparent circuit board comprises the following steps:

[0033] Step S1, heat-compressing the pressure-sensitive thermally conductive insulating adhesive film and the copper foil together to form an adhesive-coated copper foil;

[0034] The pressure-sensitive thermally conductive insulating film includes the following components by weight:

[0035] 50-60 parts of GELR125 epoxy resin, 30-40 parts of silicone modified epoxy resin, 10-20 parts of polyurethane modified epoxy resin, 20-30 parts of phenolic resin curing agent, 0.1-0.5 parts of urea accelerator, and 240 parts of alumina powder, wherein the particle size of the alumina powder is 1-10 μm.

[0036] The preparation process of the pressure-sensitive thermally conductive insulating adhesive film is as follows:

[0037] The raw materials of the pressure-sensitive thermally conductive insulating adhesive film are mixed evenly to obtain a colloid material;

[0038] The obtained colloid material is cast on a release film at 60-70° C. to obtain a pressure-sensitive thermally conductive insulating adhesive film with a thickness of 50-80 μm.

[0039] In the hot compress process, a hot compress machine is used to perform hot compress at 55-65°C to form a copper foil with glue.

[0040] Step S2, laminating the smooth surface of the adhesive copper foil on the protective film by a laminating machine, and die-cutting the adhesive copper foil by a die-cutting technology, removing the excess adhesive copper foil after die-cutting, and retaining the required circuit pattern on the protective film to obtain the adhesive copper foil circuit pattern;

[0041] Step S3, taking the transparent glass substrate and the adhesive copper foil circuit pattern, and using a hot compressing machine to compound the transparent glass substrate and the adhesive copper foil circuit pattern, so that the transparent glass substrate and the copper foil circuit pattern are bonded;

[0042] Specifically, a heat-compression machine is used to compound the transparent glass substrate and the adhesive copper foil circuit pattern at 55-65°C.

[0043] Step S4, removing the protective film after cooling to obtain an uncured glass-based circuit board;

[0044] Step S5, subjecting the uncured glass-based circuit board to a multi-stage step curing process to obtain an LED transparent circuit board;

[0045] Specifically, the multi-stage step curing process is: the first stage is curing at 70-80°C for 40-60 minutes, the second stage is curing at 90-100°C for 40-60 minutes, the third stage is curing at 110-120°C for 20-30 minutes, the fourth stage is curing at 140-150°C for 20-30 minutes, and the fifth stage is curing at 165-170°C for 30-40 minutes.

[0046] The LED transparent circuit board and the preparation method thereof provided by the present invention are described in detail below through specific embodiments.

[0047] Example 1

[0048] A method for preparing an LED transparent circuit board comprises the following steps:

[0049] Step S1, using a hot compress machine to hot compress the pressure-sensitive thermally conductive insulating adhesive film and the copper foil together at 55° C. to form a copper foil with adhesive;

[0050] In this embodiment, the pressure-sensitive thermally conductive insulating adhesive film is prepared by the following steps:

[0051] By weight, 50 parts of GELR125 epoxy resin, 30 parts of silicone-modified epoxy resin, 10 parts of polyurethane-modified epoxy resin, 20 parts of phenolic resin curing agent, 0.1 parts of urea accelerator, and 200 parts of alumina powder (5 μm) were mixed uniformly at room temperature to obtain a colloidal material;

[0052] The obtained colloid material was cast on a release film at 70° C. to obtain a pressure-sensitive thermally conductive insulating adhesive film with a thickness of 50 μm.

[0053] Step S2, laminating the smooth surface of the adhesive copper foil on the protective film by a laminating machine, and die-cutting the adhesive copper foil by a die-cutting technology, removing the excess adhesive copper foil after die-cutting, and retaining the required circuit pattern on the protective film to obtain the adhesive copper foil circuit pattern;

[0054] Step S3, taking a transparent glass substrate and a copper foil circuit pattern with adhesive, and compounding the transparent glass substrate and the copper foil circuit pattern with adhesive at 55° C. using a hot compressing machine, so that the transparent glass substrate and the copper foil circuit pattern are bonded by a pressure-sensitive thermally conductive insulating adhesive film;

[0055] Step S4, removing the protective film after cooling to obtain an uncured glass-based circuit board;

[0056] Step S5, subjecting the uncured glass-based circuit board to a multi-stage step curing process to obtain an LED transparent circuit board;

[0057] In this embodiment, the multi-stage gradient curing process is:

[0058] The first stage is cured at 70°C for 60 minutes, the second stage is cured at 90°C for 60 minutes, the third stage is cured at 110°C for 30 minutes, the fourth stage is cured at 140°C for 30 minutes, and the fifth stage is cured at 165°C for 40 minutes. After the curing is completed, it is naturally cooled to obtain a transparent base circuit board.

[0059] Example 2

[0060] A method for preparing an LED transparent circuit board comprises the following steps:

[0061] Step S1, using a hot compress machine to hot compress the pressure-sensitive thermally conductive insulating adhesive film and the copper foil together at 60° C. to form a copper foil with adhesive;

[0062] In this embodiment, the pressure-sensitive thermally conductive insulating adhesive film is prepared by the following steps:

[0063] By weight, 50 parts of GELR125 epoxy resin, 30 parts of silicone-modified epoxy resin, 10 parts of polyurethane-modified epoxy resin, 25 parts of phenolic resin curing agent, 0.3 parts of urea accelerator, and 220 parts of alumina powder (5 μm) were mixed uniformly at room temperature to obtain a colloidal material;

[0064] The obtained colloid material was cast on a release film at 55° C. to obtain a pressure-sensitive thermally conductive insulating adhesive film with a thickness of 65 μm.

[0065] Step S2, laminating the smooth surface of the adhesive copper foil on the protective film by a laminating machine, and die-cutting the adhesive copper foil by a die-cutting technology, removing the excess adhesive copper foil after die-cutting, and retaining the required circuit pattern on the protective film to obtain the adhesive copper foil circuit pattern;

[0066] Step S3, taking a transparent glass substrate and a copper foil circuit pattern with adhesive, and compounding the transparent glass substrate and the copper foil circuit pattern with adhesive at 60° C. using a hot compressing machine, so that the transparent glass substrate and the copper foil circuit pattern are bonded by a pressure-sensitive thermally conductive insulating adhesive film;

[0067] Step S4, removing the protective film after cooling to obtain an uncured glass-based circuit board;

[0068] Step S5, subjecting the uncured glass-based circuit board to a multi-stage step curing process to obtain an LED transparent circuit board;

[0069] In this embodiment, the multi-stage gradient curing process is:

[0070] The first stage is cured at 75°C for 50 minutes, the second stage is cured at 95°C for 50 minutes, the third stage is cured at 115°C for 25 minutes, the fourth stage is cured at 145°C for 25 minutes, and the fifth stage is cured at 167°C for 35 minutes. After the curing is completed, it is naturally cooled to obtain a transparent base circuit board.

[0071] Example 3

[0072] A method for preparing an LED transparent circuit board comprises the following steps:

[0073] Step S1, using a hot compress machine to hot compress the pressure-sensitive thermally conductive insulating adhesive film and the copper foil together at 65° C. to form a copper foil with adhesive;

[0074] In this embodiment, the pressure-sensitive thermally conductive insulating adhesive film is prepared by the following steps:

[0075] By weight, 50 parts of GELR125 epoxy resin, 30 parts of silicone-modified epoxy resin, 10 parts of polyurethane-modified epoxy resin, 30 parts of phenolic resin curing agent, 0.5 parts of urea accelerator, and 240 parts of alumina powder (5 μm) were mixed uniformly at room temperature to obtain a colloidal material;

[0076] The obtained colloid material was cast on a release film at 55° C. to obtain a pressure-sensitive thermally conductive insulating adhesive film with a thickness of 80 μm.

[0077] Step S2, laminating the smooth surface of the adhesive copper foil on the protective film by a laminating machine, and die-cutting the adhesive copper foil by a die-cutting technology, removing the excess adhesive copper foil after die-cutting, and retaining the required circuit pattern on the protective film to obtain the adhesive copper foil circuit pattern;

[0078] Step S3, taking a transparent glass substrate and a copper foil circuit pattern with adhesive, and compounding the transparent glass substrate and the copper foil circuit pattern with adhesive at 65° C. using a hot compressing machine, so that the transparent glass substrate and the copper foil circuit pattern are bonded by a pressure-sensitive thermally conductive insulating adhesive film;

[0079] Step S4, removing the protective film after cooling to obtain an uncured glass-based circuit board;

[0080] Step S5, subjecting the uncured glass-based circuit board to a multi-stage step curing process to obtain an LED transparent circuit board;

[0081] In this embodiment, the multi-stage gradient curing process is:

[0082] The first stage is cured at 80°C for 40 minutes, the second stage is cured at 100°C for 40 minutes, the third stage is cured at 120°C for 20 minutes, the fourth stage is cured at 150°C for 20 minutes, and the fifth stage is cured at 170°C for 30 minutes. After the curing is completed, it is naturally cooled to obtain a transparent base circuit board.

[0083] Example 4

[0084] A method for preparing an LED transparent circuit board comprises the following steps:

[0085] Step S1, using a hot compress machine to hot compress the pressure-sensitive thermally conductive insulating adhesive film and the copper foil together at 58° C. to form a copper foil with adhesive;

[0086] In this embodiment, the pressure-sensitive thermally conductive insulating adhesive film is prepared by the following steps:

[0087] By weight, 55 parts of GELR125 epoxy resin, 35 parts of silicone-modified epoxy resin, 15 parts of polyurethane-modified epoxy resin, 20 parts of phenolic resin curing agent, 0.1 parts of urea accelerator, and 200 parts of alumina powder (5 μm) were mixed uniformly at room temperature to obtain a colloidal material;

[0088] The obtained colloid material was cast on a release film at 70° C. to obtain a pressure-sensitive thermally conductive insulating adhesive film with a thickness of 50 μm.

[0089] Step S2, laminating the smooth surface of the adhesive copper foil on the protective film by a laminating machine, and die-cutting the adhesive copper foil by a die-cutting technology, removing the excess adhesive copper foil after die-cutting, and retaining the required circuit pattern on the protective film to obtain the adhesive copper foil circuit pattern;

[0090] Step S3, taking a transparent glass substrate and a copper foil circuit pattern with adhesive, and compounding the transparent glass substrate and the copper foil circuit pattern with adhesive at 58° C. using a hot compressing machine, so that the transparent glass substrate and the copper foil circuit pattern are bonded by a pressure-sensitive thermally conductive insulating adhesive film;

[0091] Step S4, removing the protective film after cooling to obtain an uncured glass-based circuit board;

[0092] Step S5, subjecting the uncured glass-based circuit board to a multi-stage step curing process to obtain an LED transparent circuit board;

[0093] In this embodiment, the multi-stage gradient curing process is:

[0094] The first stage is cured at 70°C for 60 minutes, the second stage is cured at 90°C for 60 minutes, the third stage is cured at 110°C for 30 minutes, the fourth stage is cured at 140°C for 30 minutes, and the fifth stage is cured at 165°C for 40 minutes. After the curing is completed, it is naturally cooled to obtain a transparent base circuit board.

[0095] Example 5

[0096] A method for preparing an LED transparent circuit board comprises the following steps:

[0097] Step S1, using a hot compress machine, hot compressing the pressure-sensitive thermally conductive insulating adhesive film and the copper foil together at 62° C. to form a copper foil with adhesive;

[0098] In this embodiment, the pressure-sensitive thermally conductive insulating adhesive film is prepared by the following steps:

[0099] By weight, 55 parts of GELR125 epoxy resin, 35 parts of silicone-modified epoxy resin, 15 parts of polyurethane-modified epoxy resin, 25 parts of phenolic resin curing agent, 0.3 parts of urea accelerator, and 220 parts of alumina powder (5 μm) were mixed uniformly at room temperature to obtain a colloidal material;

[0100] The obtained colloid material was cast on a release film at 60° C. to obtain a pressure-sensitive thermally conductive insulating adhesive film with a thickness of 65 μm.

[0101] Step S2, laminating the smooth surface of the adhesive copper foil on the protective film by a laminating machine, and die-cutting the adhesive copper foil by a die-cutting technology, removing the excess adhesive copper foil after die-cutting, and retaining the required circuit pattern on the protective film to obtain the adhesive copper foil circuit pattern;

[0102] Step S3, taking a transparent glass substrate and a copper foil circuit pattern with adhesive, and compounding the transparent glass substrate and the copper foil circuit pattern with adhesive at 62° C. using a hot compressing machine, so that the transparent glass substrate and the copper foil circuit pattern are bonded by a pressure-sensitive thermally conductive insulating adhesive film;

[0103] Step S4, removing the protective film after cooling to obtain an uncured glass-based circuit board;

[0104] Step S5, subjecting the uncured glass-based circuit board to a multi-stage step curing process to obtain an LED transparent circuit board;

[0105] In this embodiment, the multi-stage gradient curing process is:

[0106] The first stage is cured at 75°C for 50 minutes, the second stage is cured at 95°C for 50 minutes, the third stage is cured at 115°C for 25 minutes, the fourth stage is cured at 145°C for 25 minutes, and the fifth stage is cured at 167°C for 35 minutes. After the curing is completed, it is naturally cooled to obtain a transparent base circuit board.

[0107] Example 6

[0108] A method for preparing an LED transparent circuit board comprises the following steps:

[0109] Step S1, using a hot compress machine to hot compress the pressure-sensitive thermally conductive insulating adhesive film and the copper foil together at 65° C. to form a copper foil with adhesive;

[0110] In this embodiment, the pressure-sensitive thermally conductive insulating adhesive film is prepared by the following steps:

[0111] By weight, 55 parts of GELR125 epoxy resin, 35 parts of silicone-modified epoxy resin, 15 parts of polyurethane-modified epoxy resin, 30 parts of phenolic resin curing agent, 0.5 parts of urea accelerator, and 240 parts of alumina powder (5 μm) were mixed uniformly at room temperature to obtain a colloidal material;

[0112] The obtained colloid material was cast on a release film at 70° C. to obtain a pressure-sensitive thermally conductive insulating adhesive film with a thickness of 80 μm.

[0113] Step S2, laminating the smooth surface of the adhesive copper foil on the protective film by a laminating machine, and die-cutting the adhesive copper foil by a die-cutting technology, removing the excess adhesive copper foil after die-cutting, and retaining the required circuit pattern on the protective film to obtain the adhesive copper foil circuit pattern;

[0114] Step S3, taking a transparent glass substrate and a copper foil circuit pattern with adhesive, and compounding the transparent glass substrate and the copper foil circuit pattern with adhesive at 65° C. using a hot compressing machine, so that the transparent glass substrate and the copper foil circuit pattern are bonded by a pressure-sensitive thermally conductive insulating adhesive film;

[0115] Step S4, removing the protective film after cooling to obtain an uncured glass-based circuit board;

[0116] Step S5, subjecting the uncured glass-based circuit board to a multi-stage step curing process to obtain an LED transparent circuit board;

[0117] In this embodiment, the multi-stage gradient curing process is:

[0118] The first stage is cured at 80°C for 40 minutes, the second stage is cured at 100°C for 40 minutes, the third stage is cured at 120°C for 20 minutes, the fourth stage is cured at 150°C for 20 minutes, and the fifth stage is cured at 170°C for 30 minutes. After the curing is completed, it is naturally cooled to obtain a transparent base circuit board.

[0119] Example 7

[0120] A method for preparing an LED transparent circuit board comprises the following steps:

[0121] Step S1, using a hot compress machine to hot compress the pressure-sensitive thermally conductive insulating adhesive film and the copper foil together at 55° C. to form a copper foil with adhesive;

[0122] In this embodiment, the pressure-sensitive thermally conductive insulating adhesive film is prepared by the following steps:

[0123] By weight, 60 parts of GELR125 epoxy resin, 40 parts of silicone-modified epoxy resin, 20 parts of polyurethane-modified epoxy resin, 20 parts of phenolic resin curing agent, 0.1 parts of urea accelerator, and 200 parts of alumina powder (5 μm) were mixed uniformly at room temperature to obtain a colloidal material;

[0124] The obtained colloid material was cast on a release film at 62° C. to obtain a pressure-sensitive thermally conductive insulating adhesive film with a thickness of 50 μm.

[0125] Step S2, laminating the smooth surface of the adhesive copper foil on the protective film by a laminating machine, and die-cutting the adhesive copper foil by a die-cutting technology, removing the excess adhesive copper foil after die-cutting, and retaining the required circuit pattern on the protective film to obtain the adhesive copper foil circuit pattern;

[0126] Step S3, taking a transparent glass substrate and a copper foil circuit pattern with adhesive, and compounding the transparent glass substrate and the copper foil circuit pattern with adhesive at 55° C. using a hot compressing machine, so that the transparent glass substrate and the copper foil circuit pattern are bonded by a pressure-sensitive thermally conductive insulating adhesive film;

[0127] Step S4, removing the protective film after cooling to obtain an uncured glass-based circuit board;

[0128] Step S5, subjecting the uncured glass-based circuit board to a multi-stage step curing process to obtain an LED transparent circuit board;

[0129] In this embodiment, the multi-stage gradient curing process is:

[0130] The first stage is cured at 70°C for 60 minutes, the second stage is cured at 90°C for 60 minutes, the third stage is cured at 110°C for 30 minutes, the fourth stage is cured at 140°C for 30 minutes, and the fifth stage is cured at 165°C for 40 minutes. After the curing is completed, it is naturally cooled to obtain a transparent base circuit board.

[0131] Example 8

[0132] A method for preparing an LED transparent circuit board comprises the following steps:

[0133] Step S1, using a hot compress machine to hot compress the pressure-sensitive thermally conductive insulating adhesive film and the copper foil together at 55° C. to form a copper foil with adhesive;

[0134] In this embodiment, the pressure-sensitive thermally conductive insulating adhesive film is prepared by the following steps:

[0135] By weight, 60 parts of GELR125 epoxy resin, 40 parts of silicone-modified epoxy resin, 20 parts of polyurethane-modified epoxy resin, 25 parts of phenolic resin curing agent, 0.3 parts of urea accelerator, and 220 parts of alumina powder (5 μm) were mixed uniformly at room temperature to obtain a colloidal material;

[0136] The obtained colloid material was cast on a release film at 67° C. to obtain a pressure-sensitive thermally conductive insulating adhesive film with a thickness of 65 μm.

[0137] Step S2, laminating the smooth surface of the adhesive copper foil on the protective film by a laminating machine, and die-cutting the adhesive copper foil by a die-cutting technology, removing the excess adhesive copper foil after die-cutting, and retaining the required circuit pattern on the protective film to obtain the adhesive copper foil circuit pattern;

[0138] Step S3, taking a transparent glass substrate and a copper foil circuit pattern with adhesive, and compounding the transparent glass substrate and the copper foil circuit pattern with adhesive at 55° C. using a hot compressing machine, so that the transparent glass substrate and the copper foil circuit pattern are bonded by a pressure-sensitive thermally conductive insulating adhesive film;

[0139] Step S4, removing the protective film after cooling to obtain an uncured glass-based circuit board;

[0140] Step S5, subjecting the uncured glass-based circuit board to a multi-stage step curing process to obtain an LED transparent circuit board;

[0141] In this embodiment, the multi-stage gradient curing process is:

[0142] The first stage is cured at 75°C for 50 minutes, the second stage is cured at 95°C for 50 minutes, the third stage is cured at 115°C for 25 minutes, the fourth stage is cured at 145°C for 25 minutes, and the fifth stage is cured at 167°C for 35 minutes. After the curing is completed, it is naturally cooled to obtain a transparent base circuit board.

[0143] Example 9

[0144] A method for preparing an LED transparent circuit board comprises the following steps:

[0145] Step S1, using a hot compress machine to hot compress the pressure-sensitive thermally conductive insulating adhesive film and the copper foil together at 65° C. to form a copper foil with adhesive;

[0146] In this embodiment, the pressure-sensitive thermally conductive insulating adhesive film is prepared by the following steps:

[0147] By weight, 60 parts of GELR125 epoxy resin, 40 parts of silicone-modified epoxy resin, 20 parts of polyurethane-modified epoxy resin, 30 parts of phenolic resin curing agent, 0.5 parts of urea accelerator, and 240 parts of alumina powder (5 μm) were mixed uniformly at room temperature to obtain a colloidal material;

[0148] The obtained colloid material was cast on a release film at 64° C. to obtain a pressure-sensitive thermally conductive insulating adhesive film with a thickness of 80 μm.

[0149] Step S2, laminating the smooth surface of the adhesive copper foil on the protective film by a laminating machine, and die-cutting the adhesive copper foil by a die-cutting technology, removing the excess adhesive copper foil after die-cutting, and retaining the required circuit pattern on the protective film to obtain the adhesive copper foil circuit pattern;

[0150] Step S3, taking a transparent glass substrate and a copper foil circuit pattern with adhesive, and compounding the transparent glass substrate and the copper foil circuit pattern with adhesive at 65° C. using a hot compressing machine, so that the transparent glass substrate and the copper foil circuit pattern are bonded by a pressure-sensitive thermally conductive insulating adhesive film;

[0151] Step S4, removing the protective film after cooling to obtain an uncured glass-based circuit board;

[0152] Step S5, subjecting the uncured glass-based circuit board to a multi-stage step curing process to obtain an LED transparent circuit board;

[0153] In this embodiment, the multi-stage gradient curing process is:

[0154] The first stage is cured at 80°C for 40 minutes, the second stage is cured at 100°C for 40 minutes, the third stage is cured at 120°C for 20 minutes, the fourth stage is cured at 150°C for 20 minutes, and the fifth stage is cured at 170°C for 30 minutes. After the curing is completed, it is naturally cooled to obtain a transparent base circuit board.

[0155] Comparative Example 1

[0156] On the basis of Example 1, the raw material composition of the pressure-sensitive thermally conductive insulating adhesive film is modified so that the composition of Comparative Example 1 does not contain aluminum oxide powder, and other processes and parameters are the same as those of Example 1.

[0157] Comparative Example 2

[0158] On the basis of Example 1, the raw material composition of the pressure-sensitive thermally conductive insulating adhesive film was modified by replacing the mixture of 35 parts of silicone-modified epoxy resin / 15 parts of polyurethane-modified epoxy resin with 50 parts of epoxy resin. Other processes and parameters were the same as those in Example 1.

[0159] Comparative Example 3

[0160] Based on Example 5, the multi-stage step curing process was modified, and the curing was carried out in two stages, wherein the first stage was cured at 70° C. for 30 min, and the second stage was cured at 170° C. for 40 min.

[0161] The LED transparent circuit boards prepared in the above Examples 1-9 and Comparative Examples 1-3 were subjected to performance tests, and the test results are as follows:

[0162] LED transparent circuit board performance test results

[0163]

[0164]

[0165] From the experimental data, we can see that:

[0166] 1. The pressure-sensitive thermally conductive insulating adhesive film of Comparative Example 1 does not contain alumina powder, and its thermal conductivity is smaller than that of Example 1, indicating that the addition of alumina powder can change the thermal conductivity of the material. After adding alumina powder, its heat resistance will be improved, and the more alumina powder is added, the lower the dielectric constant and dielectric loss will be; the more alumina powder is added, the lower the viscosity density of the film, and the lower the peel strength.

[0167] 2. After replacing the silicone-modified epoxy resin and polyurethane-modified epoxy resin with an equal amount of epoxy resin, the peel strength and thermal conductivity of the circuit board are significantly reduced. The polyurethane-modified epoxy resin mainly increases the toughness of the material, and the silicone-modified epoxy resin improves the weather resistance of the material, thereby increasing its overall stability.

[0168] 3. A multi-stage stepped curing process is adopted to slow down the reaction rate, thereby improving the compactness of the glue during the reaction, making the thickness of the glue layer basically unchanged before and after the reaction, thereby improving the glass strength and thermal conductivity of the circuit board. In the present invention, the prepared circuit board has a peel strength of up to 1.42N / mm and a thermal conductivity of 1.7W / m·k. In Comparative Example 3, the curing process is modified to two-stage curing, and the glass strength and thermal conductivity of the obtained circuit board are significantly reduced, the reaction rate is too fast, and the compactness of the glue layer is poor, so that the copper-containing tin-bleaching performance is significantly reduced.

[0169] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations made to these embodiments without departing from the principles and spirit of the present invention are still within the protection scope of the present invention.

Claims

1. A method for preparing a LED transparent circuit board, characterized in that: The steps include: Step S1, heat-compressing a pressure-sensitive thermally conductive insulating adhesive film and a copper foil together to form an adhesive-coated copper foil; the pressure-sensitive thermally conductive insulating adhesive film comprises the following components in parts by weight: 50-60 parts of GELR125 epoxy resin, 30-40 parts of silicone modified epoxy resin, 10-20 parts of polyurethane modified epoxy resin, 20-30 parts of phenolic resin curing agent, 0.1-0.5 parts of urea accelerator, 200-240 parts of alumina powder, wherein the particle size of the alumina powder is 1-10 μm; Step S2, laminating the smooth surface of the adhesive copper foil on the protective film by a laminating machine, and die-cutting the adhesive copper foil by a die-cutting technology, removing the excess adhesive copper foil after die-cutting, and retaining the required circuit pattern on the protective film to obtain the adhesive copper foil circuit pattern; Step S3, taking the transparent glass substrate and the adhesive copper foil circuit pattern, and using a hot compressing machine to compound the transparent glass substrate and the adhesive copper foil circuit pattern, so that the transparent glass substrate and the copper foil circuit pattern are bonded; Step S4, removing the protective film after cooling to obtain an uncured glass-based circuit board; Step S5, subjecting the uncured glass-based circuit board to a multi-stage step curing process to obtain an LED transparent circuit board; the multi-stage step curing process is: the first stage is cured at 70-80°C for 40-60min, the second stage is cured at 90-100°C for 40-60min, the third stage is cured at 110-120°C for 20-30min, the fourth stage is cured at 140-150°C for 20-30min, and the fifth stage is cured at 165-170°C for 30-40min.

2. The method for preparing a transparent LED circuit board according to claim 1, characterized in that: The preparation process of the pressure-sensitive thermally conductive insulating film is as follows: The raw materials of the pressure-sensitive thermally conductive insulating adhesive film are mixed evenly to obtain a colloid material; The obtained colloid material is cast on a release film at 60-70° C. to obtain a pressure-sensitive thermally conductive insulating adhesive film.

3. The method for preparing a transparent LED circuit board according to claim 2, characterized in that: The thickness of the pressure-sensitive thermally conductive insulating adhesive film is 50-80 μm.

4. The method for preparing a transparent LED circuit board according to claim 1, characterized in that: In step S1, a hot compress machine is used to perform hot compress at 55-65° C. to form a copper foil with glue.

5. The method for preparing a transparent LED circuit board according to claim 1, characterized in that: In step S3, the transparent glass substrate and the adhesive copper foil circuit pattern are compounded at 55-65° C. using a hot compress machine.

6. A LED transparent circuit board, characterized in that: The method is prepared according to any one of claims 1 to 5.