Hydrocarbon adsorption and desorption composites comprising zeolites having controlled cation ratios and methods for preparing the same

By controlling the molar ratio of sodium to aluminum in zeolite particles and impregnating metal ions, a composite with excellent hydrocarbon adsorption and oxidation properties is formed, the problem of insufficient performance of existing HC traps in low temperature and high moisture environments is solved, and the problem of insufficient performance of existing HC traps is achieved. High efficient hydrocarbon treatment and hydrothermal stability during cold start-up period.

CN114534687BActive Publication Date: 2024-11-26KOREA UNIV MATHEMATICAL COOP GRP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202111394716.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-11-24
Filing Date
2021-11-23
Publication Date
2024-11-26
Estimated Expiration
2041-11-23

AI Technical Summary

Technical Problem

The existing HC traps have insufficient adsorption and oxidation capacity of hydrocarbons at lower than the three-way catalyst activation temperature, and their performance deteriorates in high moisture environments, making it difficult to effectively treat hydrocarbons emitted by gasoline vehicles during the cold start period.

Method used

By controlling the molar ratio of sodium to aluminum (Na/Al) in the zeolite particles to below 0.7, combining metal ions and metal oxides to form a composite with excellent hydrocarbon adsorption and oxidation properties, it is prepared by ion exchange method and wet impregnation method. Improve hydrothermal stability.

Benefits of technology

It realizes efficient adsorption and oxidation of hydrocarbons at lower than the three-way catalyst activation temperature, and maintains excellent performance after hydrothermal treatment. It is suitable for hydrocarbon treatment during the cold start period, improving hydrothermal stability and heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114534687B_ABST
    Figure CN114534687B_ABST
Patent Text Reader

Abstract

The present invention discloses a hydrocarbon adsorption and desorption composite that exhibits hydrocarbon adsorption and oxidation performance by controlling the cation ratio in zeolite and a preparation method thereof. The hydrocarbon adsorption and desorption composite controls the cation ratio so as to exhibit excellent hydrocarbon adsorption capacity and oxidation performance even at a temperature lower than the catalyst activation temperature, and improves the hydrothermal stability of the hydrocarbon adsorption and desorption composite by hydrothermal treatment so as to exhibit excellent hydrocarbon adsorption and desorption performance even in the presence of water at a high temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a hydrocarbon adsorption and desorption composite comprising zeolite, and more particularly, to such a hydrocarbon adsorption and desorption composite in which metal ions and metal oxides formed on zeolite are effectively dispersed by controlling the cation ratio in zeolite, and a preparation method thereof. Background Art

[0002] With the growing concern over air pollution, regulations on exhaust gases such as carbon monoxide (CO), nitrogen oxides (NOx), hydrocarbons (HC), particulate matter (PM), etc. emitted from gasoline and diesel vehicles are being tightened in the United States, Europe, and other places. In particular, from Euro 1 in 1992 to Euro 6 in 2020, hydrocarbon (HC) emissions should be reduced by at least 80% compared to 1992. Among the HCs emitted by gasoline vehicles, 50% to 80% of the hydrocarbons emitted during operation are emitted during the cold start period when the three-way catalyst (TWC, which acts on HC oxidation) is inactive. Hydrocarbon adsorbents (HC traps) are being studied to reduce hydrocarbons emitted during cold starts. The HC trap is a device that adsorbs hydrocarbons emitted during the cold start period and desorbs the adsorbed hydrocarbons when the three-way catalyst reaches the activation temperature (about 200 to 300°C).

[0003] There is a lot of research being done on using physically and chemically stable zeolites as HC traps. The performance of HC traps is tested by measuring the adsorption and desorption of propylene and toluene, which are representative hydrocarbon emissions from gasoline vehicles. The performance of HC traps has been studied based on the zeolite structure, Si / Al value, and the presence or absence of metal impregnation. The higher the Al content of the zeolite (i.e., the smaller the Si / Al value), the more hydrocarbons are adsorbed onto the zeolite. In addition, among the various zeolite structures, ZSM-5 (zeolite socony Mobil-5) and β-structured zeolites exhibit high performance. However, HC traps made solely of zeolite have low adsorption and oxidation capabilities for hydrocarbons below 300°C, which may lead to problems of insufficient treatment of hydrocarbons generated during cold start before the three-way catalyst reaches the activation temperature, and in addition, the performance of the HC trap deteriorates when a large amount of water (about 10 mol%) is present.

[0004] In order to solve the above problems, it is necessary to develop an adsorbent that adsorbs and oxidizes hydrocarbons at a temperature lower than the activation temperature of the three-way catalyst and exhibits excellent hydrocarbon adsorption and oxidation capabilities even in the presence of a large amount of water.

[0005] An example of the related art is disclosed in Japanese Unexamined Patent Application Publication No. 2012-512022 (date: May 31, 2012). Summary of the invention

[0006] Technical issues

[0007] An object of the present invention is to provide a hydrocarbon adsorption and desorption composite which exhibits hydrocarbon adsorption and oxidation performance by controlling the cation ratio in zeolite, and a method for preparing the same.

[0008] Technical Solution

[0009] According to one aspect of the present invention, a hydrocarbon adsorption and desorption composite is provided, which comprises: zeolite particles containing cations; metal ions chemically bonded to the zeolite particles; and a metal oxide provided on the outer surface of the zeolite particles, wherein the cations include cations of sodium and hydrogen, and the molar ratio of sodium to aluminum (Na / Al) of the zeolite particles is less than 0.7.

[0010] According to another aspect of the present invention, there is provided a method for preparing a hydrocarbon adsorption and desorption composite, comprising:

[0011] controlling a cation ratio in the zeolite particles by using an ion exchange method; and forming metal ions and metal oxides by mixing the zeolite particles having the controlled cation ratio with a solution containing metal ions;

[0012] In controlling the cation ratio, the molar ratio of sodium to aluminum (Na / Al) of the zeolite particles is controlled to be less than 0.7.

[0013] According to still another aspect of the present invention, there is provided a hydrocarbon adsorption and desorption composite for a vehicle, comprising the hydrocarbon adsorption and desorption composite according to the above aspect.

[0014] Beneficial Effects

[0015] The hydrocarbon adsorption and desorption composite according to the present invention can control the cation ratio, so that excellent hydrocarbon adsorption capacity and oxidation performance can be exhibited even at a temperature lower than the catalyst activation temperature.

[0016] Furthermore, the hydrocarbon adsorption and desorption composite according to the present invention can increase the hydrothermal stability, so that it can exhibit excellent hydrocarbon adsorption and desorption performance even after undergoing a hydrothermal treatment process in which a high temperature is applied in the presence of water. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 and Figure 2 Shown are images of a hydrocarbon adsorption and desorption composite according to an embodiment of the present invention, which were captured using a scanning electron microscope (SEM) and an X-ray diffraction analysis (XRD) pattern.

[0018] Figure 3is a graph of cold start test results for a hydrocarbon adsorption and desorption composite according to an embodiment of the present invention.

[0019] Figure 4 and 5 Graph showing cold start test results for propylene and toluene for hydrocarbon adsorption and desorption composites according to embodiments of the present invention.

[0020] Figure 6 and 7 A graph showing cold start test results of total hydrocarbon adsorption for a hydrocarbon adsorption and desorption composite according to an embodiment of the present invention.

[0021] Figure 8 Graph showing cold start test results for carbon monoxide and carbon dioxide for a hydrocarbon adsorption and desorption composite according to an embodiment of the present invention.

[0022] Fig. 9 and 10 A graph showing hydrocarbon treatment efficiencies of propylene, toluene, and total hydrocarbons and adsorption amounts of propylene and toluene with respect to a molar ratio of sodium to aluminum and with or without hydrothermal treatment in a hydrocarbon adsorption and desorption composite according to an embodiment of the present invention.

[0023] Fig.11 and 12 Graph showing total hydrocarbon adsorption and onset oxidation temperature for a hydrocarbon adsorption and desorption composite according to an embodiment of the present invention. DETAILED DESCRIPTION

[0024] Hereinafter, in order to more specifically describe the present invention, preferred embodiments according to the present invention will be described in more detail with reference to the accompanying drawings. However, the present invention is not limited to the embodiments described herein and may be embodied in other forms.

[0025] In the present specification, "total hydrocarbons" refers to hydrocarbons based on methane. Specifically, total hydrocarbons are obtained by converting propylene, toluene, etc. into values ​​corresponding to methane by gas chromatography (GC FID) and quantifying the converted values ​​as the amount of methane.

[0026] Hitherto, HC traps have been reported in which a copper-impregnated zeolite is provided through an ion exchange process, or a relatively large amount of copper is used for ion exchange and some of the remaining copper exists in the form of copper oxide in order to improve hydrocarbon adsorption performance.

[0027] The development of HC traps in the related art has been studied by controlling the Si / Al value, structure and type of impregnated metal of zeolite; however, the present invention relates to an HC trap having excellent hydrocarbon adsorption and oxidation capabilities by controlling the distribution of metal ions and metal oxides by controlling the ratio of cations present in active sites of the same type of zeolite.

[0028] The present invention provides a hydrocarbon adsorption and desorption composite, which comprises: zeolite particles;

[0029] Metal ions chemically bonded to the zeolite particles; and

[0030] A metal oxide is provided on the outer surface of the zeolite particles, wherein

[0031] The cations include cations of sodium and hydrogen, and the molar ratio of sodium to aluminum (Na / Al) of the zeolite particles is 0.7 or less.

[0032] The zeolite particles may be ZSM-5 zeolite.

[0033] Specifically, the molar ratio of sodium to aluminum (Na / Al) of the zeolite particles may be 0.6 or less, 0.01 to 0.6, 0.1 to 0.5, or 0.2 to 0.5. Zeolite particles having the above molar ratio of sodium to aluminum may have excellent cold start performance even during hydrothermal treatment, thereby achieving high adsorption capacity and hydrocarbon oxidation capacity even in the presence of water. Sodium and hydrogen cations are chemically bonded to the zeolite active sites.

[0034] Zeolite is a zeolite having a Si / Al value of about 25, and cations are bound to its active sites. As described above, when cations are bound to the zeolite active sites, the content of metal ions bound to the zeolite pores is high, and the size of the metal oxide formed on the zeolite surface is small, so the adsorption performance of the hydrocarbon adsorption and desorption composite is improved.

[0035] The size of the hydrocarbon adsorption and desorption complex may be 50 to 5000 nm. Specifically, the size of the hydrocarbon adsorption and desorption complex may be 50 to 2000 nm or 300 to 1500 nm.

[0036] In addition, the hydrocarbon adsorption and desorption composite is a composite in which fine pores are formed in zeolite particles, metal ions are impregnated in the pores formed in the zeolite particles, and metal oxides are provided on the surface of the zeolite particles. Specifically, the micropore volume of the hydrocarbon adsorption and desorption composite can be 0.1 to 0.2 cm 3 / g, 0.1~0.15cm 3 / g or 0.12~0.13cm 3 As described above, the adsorption capacity for hydrocarbons such as propylene and toluene can be improved by the micropores formed in the zeolite particles and the metal ions impregnated into the micropores.

[0037] The metal ion may be a cation of any one or more metals of Groups 3 to 12. Specifically, the metal ion may be a cation of any one or more metals of iron, cobalt, nickel, copper, zinc, rhodium, and cadmium. More specifically, the metal ion may be a cation of monovalent iron, divalent iron, trivalent iron, monovalent cobalt, divalent cobalt, monovalent nickel, divalent nickel, monovalent copper, or divalent copper. The metal ion may be incorporated into the interior of the pores formed in the zeolite particles to improve the hydrocarbon adsorption capacity.

[0038] The metal oxide may be an oxide of any one or more metals of Groups 3 to 12. Specifically, the metal oxide may be an oxide of any one or more metals of iron, cobalt, nickel, copper, zinc, rhodium, and cadmium. More specifically, the metal oxide may be FeO, Fe3O4, Fe2O3, Co3O4, CoO, NiO, Cu2O, Cu2O3, or CuO.

[0039] For example, the metal oxide is formed on the zeolite particles and may have an average diameter of 1 to 10 nm. Specifically, the average diameter of the metal oxide may be 1 to 9 nm, 1 to 7 nm, 2 to 8 nm, or 2 to 6 nm. By forming the metal oxide on the zeolite particles as described above, the hydrocarbon adsorption and desorption composite according to the present invention may have a low hydrocarbon oxidation temperature and high hydrothermal stability.

[0040] In the hydrocarbon adsorption and desorption composite according to the present invention, the volume V1 of the micropores having a size of 1 nm or less may be 0.1 cm 3 / g or more, the metal cation may be present in an amount of 50 to 90% by weight of the maximum that can be impregnated into the zeolite, and the metal oxide may be present in an amount of 60 to 80% by weight of the maximum that can be impregnated into the zeolite.

[0041] The hydrocarbon adsorption and desorption composite according to the present invention having the above characteristics may satisfy the following formula 1:

[0042] [Formula 1]

[0043]

[0044] in

[0045] Q In represents the amount of hydrocarbon injected into the hydrocarbon adsorption and desorption complex,

[0046] Q Out represents the amount of hydrocarbon released by the hydrocarbon adsorption and desorption complex, and

[0047] A is a number of 40 or more, and represents hydrocarbon processing efficiency.

[0048] The hydrocarbon adsorption capacity of the hydrocarbon adsorption and desorption complex is calculated by measuring the amount of hydrocarbon injected into the hydrocarbon adsorption and desorption complex and the amount of hydrocarbon released from the hydrocarbon adsorption and desorption complex, and by the ratio between the amount of hydrocarbon injected into the hydrocarbon adsorption and desorption complex and the amount of hydrocarbon released from the hydrocarbon adsorption and desorption complex until the temperature reaches 300° C., resulting in Formula 1. In this case, the hydrocarbon treatment efficiency A may represent 40 or more, 45 or more, 50 or more, 55 or more, or 60 or more.

[0049] In addition, the hydrocarbon adsorption and desorption composite according to the present invention can represent the adsorption of hydrocarbons at a temperature of 300°C or less, and can represent the oxidation of hydrocarbons at a temperature of 200°C or more. Specifically, the hydrocarbon adsorption and desorption composite according to the present invention can represent the adsorption of hydrocarbons at a temperature of 70°C to 300°C or 100°C to 300°C, or can represent the oxidation of hydrocarbons at a temperature of 210°C or more, 220°C or more, 230°C or more, 240°C or more, or 250°C or more. Typically, 50% to 80% of the total hydrocarbons emitted during driving occur during the cold start period (below 300°C), and due to the above-mentioned characteristics, the hydrocarbon adsorption and desorption composite according to the present invention can effectively adsorb and oxidize hydrocarbons even during cold start, and exhibit high hydrothermal stability.

[0050] Furthermore, the hydrocarbon adsorption and desorption composite according to the present invention may have 0.32 to 1.5 mmol CH4 / g hydrocarbon adsorption and hydrocarbon oxidation starting temperature of 180 to 350° C. Specifically, the hydrocarbon adsorption and desorption composite of the present invention may have 0.32 to 1.0 mmol CH4 / g, 0.32 to 0.8 mmol CH4 / g or 0.32 to 0.4mmol CH4 / g of hydrocarbon adsorption, and may have a hydrocarbon oxidation starting temperature of 180 to 320° C., 180 to 300° C., or 180 to 250° C. In this case, the oxidation starting temperature refers to a temperature at which the amount of CO2 generated is 5% or more of the total hydrocarbons.

[0051] The hydrocarbon adsorption and desorption composite according to the present invention can be hydrothermally treated at 600°C to 900°C for 1 hour to 36 hours. Specifically, the hydrocarbon adsorption and desorption composite can be hydrothermally treated at a temperature of 600°C to 850°C, 600°C to 800°C, 600°C to 750°C, or 700°C to 800°C for 1 hour to 24 hours, 12 hours to 36 hours, or 12 hours to 24 hours. At this time, the hourly gas flow rate of the simulated exhaust gas including water vapor relative to the weight of the hydrocarbon adsorption and desorption composite can be 10,000 to 200,000 mL / g·h or 100,000 to 200,000 mL / g·h, which is a serious situation similar to when a vehicle is running for a long time. The hydrocarbon adsorption and desorption composite hydrothermally treated as described above may have reduced performance of adsorbing and oxidizing hydrocarbons in the presence of water vapor, and may have reduced durability.

[0052] For example, in the hydrothermally treated hydrocarbon adsorption and desorption composite, A as the hydrocarbon treatment efficiency in Formula 1 may be 5 or more, 10 or more, 15 or more, 20 or more, 25 or more, or 30 or more. Compared with the hydrocarbon adsorption and desorption composite that has not been hydrothermally treated (fresh hydrocarbon adsorption and desorption composite), the hydrothermally treated hydrocarbon adsorption and desorption composite exhibits a lower hydrocarbon treatment efficiency; however, in the comparison after the hydrothermal treatment, the hydrocarbon adsorption and desorption composite having a sodium to aluminum molar ratio (Na / Al) of 0.7 or less exhibits improved heat resistance and more excellent hydrocarbon treatment efficiency than the hydrocarbon adsorption and desorption composite having a sodium to aluminum molar ratio (Na / Al) of 0.7 or more.

[0053] In addition to the hydrocarbon adsorption properties, the hydrocarbon adsorption and desorption composite according to the invention can be used as a selective catalytic reduction (SCR) and, in this case, can effectively remove nitrogen oxides (NO x ), thus showing air purification ability.

[0054] The present invention provides a method for preparing a hydrocarbon adsorption and desorption composite, the method comprising: controlling the cation ratio in zeolite particles by using an ion exchange method; and

[0055] The metal ions and the metal oxide are formed by mixing zeolite particles having a controlled cation ratio with a solution containing the metal ions; wherein

[0056] In controlling the cation ratio, the molar ratio of sodium to aluminum (Na / Al) of the zeolite particles is controlled to be less than 0.7.

[0057] The zeolite particles may be ZSM-5 (zeolite socony mobil-5) zeolite.

[0058] In the control of the cation ratio, the zeolite may include a zeolite containing hydrogen cations (H-type zeolite) and a zeolite containing sodium cations (Na-type zeolite). The zeolite in which the molar ratio of sodium to aluminum (Na / Al) is controlled is prepared by replacing the sodium cations in the active sites of the zeolite with hydrogen cations or by replacing the hydrogen cations with sodium cations by calcining the zeolite precursor after ion exchange.

[0059] Controlling the cation ratio may include mixing an aqueous ammonium salt solution or an aqueous sodium salt solution with the zeolite particles, the aqueous ammonium salt solution may include any one or more of ammonium sulfate, ammonium nitrate, ammonium chloride, ammonium acetate, ammonium persulfate, aqueous ammonia, ammonium bicarbonate and ammonium formate, and the aqueous sodium salt solution may include any one or more of sodium nitrate, sodium chloride, sodium acetate, sodium persulfate, sodium bicarbonate and sodium formate.

[0060] The ammonium salt aqueous solution can be mixed with the zeolite containing sodium cations (Na-type zeolite), and when the ammonium salt aqueous solution and the zeolite containing sodium cations are mixed, the ammonium ions are replaced by the sodium cations contained in the zeolite. Then, through the calcination process, the replaced ammonium ions become hydrogen ions. In this way, the molar ratio of sodium to aluminum of the zeolite particles can be reduced, and the molar ratio of sodium to aluminum of the zeolite particles can be controlled by controlling the concentration of the ammonium salt aqueous solution and the reaction time between the ammonium salt aqueous solution and the zeolite particles.

[0061] The sodium salt solution can be mixed with a zeolite containing hydrogen cations (H-type zeolite), and when the sodium salt solution and the zeolite containing hydrogen cations are mixed, the sodium cations are replaced by the ammonium ions contained in the zeolite. Then, through the calcination process, the ammonium ions of the zeolite particles become hydrogen ions. In this way, the molar ratio of sodium to aluminum of the zeolite particles can be increased, and the molar ratio of sodium to aluminum of the zeolite particles can be controlled by controlling the concentration of the sodium salt solution and the reaction time between the sodium salt solution and the zeolite particles.

[0062] Specifically, the concentration of the aqueous ammonium salt solution may be 0.001M to 1M, 0.005M to 1M, or 0.001M to 0.9M, and the aqueous ammonium salt solution and the zeolite particles may be mixed and stirred at a temperature of 20°C to 30°C for 20 hours to 30 hours, 25 hours to 30 hours, or 20 hours to 25 hours. As described above, when the aqueous ammonium salt solution and the zeolite particles are stirred for a predetermined time to control the molar ratio of sodium to aluminum of the zeolite particles, the hydrothermal stability of the prepared hydrocarbon adsorption and desorption composite may be improved.

[0063] Specifically, the concentration of the sodium salt aqueous solution may be 0.001M to 1M, 0.005M to 1M, or 0.001M to 0.9M, and the mixture of the sodium salt aqueous solution and the zeolite particles may be stirred and mixed at a temperature of 20° C. to 30° C. for 20 hours to 30 hours, 25 hours to 30 hours, or 20 hours to 25 hours. As described above, when the sodium salt aqueous solution and the zeolite particles are stirred for a predetermined time to control the molar ratio of sodium to aluminum of the zeolite particles, the hydrothermal stability of the prepared hydrocarbon adsorption and desorption composite may be improved.

[0064] In the hydrocarbon adsorption and desorption composite prepared according to the preparation method of the present invention, the molar ratio of sodium to aluminum (Na / Al) of the zeolite particles may be 0.6 or less, 0.01 to 0.6, 0.1 to 0.5, or 0.2 to 0.5. Forming the zeolite particles having the above-mentioned molar ratio of sodium to aluminum can make the cold start test performance excellent even during the hydrothermal treatment, and thus, higher adsorption capacity and hydrocarbon oxidation capacity can be obtained even in the presence of water.

[0065] For zeolite particles in which the cation ratio is controlled as described above, the ratio of zeolite containing sodium cations may be 70% or less, 60% or less, 1% to 60%, 10% to 50%, or 20% to 50%.

[0066] Then, the method is repeated once or twice or more, wherein the mixed solution of the zeolite particles and the aqueous ammonium salt solution is centrifuged and decanted to obtain a precipitate, and the obtained precipitate is mixed with the aqueous ammonium salt solution to obtain a precipitate again.

[0067] The obtained precipitate can be calcined at a temperature of 500 to 700° C. for 10 to 20 hours under a gas flow of 300 mL / min. Specifically, the obtained precipitate can be calcined for 10 to 17 hours or 10 to 15 hours by heating the obtained precipitate at a temperature of 500 to 650° C. or 500 to 600° C. at a heating rate of about 1° C. / min under a gas flow of 300 mL / min. Through the above process, zeolite particles with a controlled sodium cation ratio can be prepared, and micropores can be formed in the zeolite particles.

[0068] The zeolite is a zeolite having a Si / Al value of about 25, and hydrogen and sodium cations are bonded to its active sites. When the cations of the active sites of the zeolite are replaced by hydrogen cations as described above, the content of the impregnated metal ions increases, which may lead to an improvement in adsorption performance, and the size of the metal oxide formed on the surface of the zeolite decreases, which may lead to an improvement in oxidation performance of the HC trap.

[0069] The formation of metal ions and metal oxides may include impregnating a metal precursor solution containing metal ions with zeolite particles having a controlled sodium to aluminum molar ratio by using a wet impregnation method, wherein the metal content may be 1 to 9 wt%, 2 to 8 wt%, 3 to 8 wt%, or 4 to 7 wt%. In addition, drying and calcination may also be included.

[0070] Specifically, in the formation of metal ions and metal oxides, the zeolite particles can be impregnated with metal ions and metal oxides by calcining the zeolite particles impregnated with the metal precursor at a temperature of 500 to 700° C. for 2 to 10 hours under a gas flow of 300 mL / min using a wet impregnation method. Specifically, the zeolite particles impregnated with the metal precursor can be calcined by heating the zeolite particles at a temperature of 500 to 650° C. or 500 to 600° C. under a gas flow of 300 mL / min at a heating rate of about 1° C. / min for 2-8 hours or 3-7 hours. Through the above process, the zeolite particles with a controlled molar ratio of sodium to aluminum can include metal ions and metal oxides, and more specifically, the metal ions can be impregnated into the micropores of the zeolite particles, and the metal oxides can be formed on the surface of the zeolite particles.

[0071] The metal ions may include cations of any one or more metals of Groups 3 to 12. Specifically, the metal ions include cations of any one or more metals of iron, cobalt, nickel, copper, zinc, rhodium and cadmium. Specifically, the metal ions may be cations of monovalent iron, divalent iron, trivalent iron, monovalent cobalt, divalent cobalt, monovalent nickel, divalent nickel, monovalent copper or divalent copper.

[0072] The metal oxide formed by impregnating a solution containing metal ions into the zeolite may be an oxide of any one or more metals of Groups 3 to 12. Specifically, the metal oxide may be an oxide of any one or more metals of iron, cobalt, nickel, copper, zinc, rhodium and cadmium. Specifically, the metal oxide may be FeO, Fe3O4, Fe2O3, Co3O4, CoO, NiO, Cu2O, Cu2O3 or CuO.

[0073] The metal oxide may be formed on the zeolite particles by the formation of metal ions and metal oxides, and the average diameter of the formed metal oxide may be 1 to 10 nm. Specifically, the average diameter of the metal oxide may be 1 to 9 nm, 1 to 7 nm, 2 to 8 nm, or 2 to 6 nm. By impregnating the metal ions into the zeolite particles and forming the metal oxide on the zeolite particles as described above, the HC trap according to the present invention may have excellent hydrocarbon adsorption performance, low hydrocarbon oxidation temperature, and high hydrothermal stability.

[0074] The HC trap prepared by the above method has micropores with a size of 1 nm or less and a volume (V1) of 0.1 cm3 / g or more, 0.1 to 0.2cm 3 / g, 0.1 to 0.15 cm 3 / g, or 0.12 to 0.13 cm 3 / g, the metal cation may be present in an amount of 50 to 80% of the maximum weight that can be impregnated into the zeolite, and the metal oxide may be formed from the remaining metal that is not impregnated into the zeolite as the metal cation.

[0075] The method for preparing the HC trap according to the present invention further comprises, after forming the metal ions and the metal oxide, injecting 5-15 mol% of water vapor at a temperature of 600 to 900°C for 1 to 36 hours for hydrothermal treatment. Specifically, the hydrothermal treatment may be performed by injecting 5 to 15 mol% of water vapor at a temperature of 600 to 800°C, 600 to 750°C, 600 to 700°C, or 700 to 800°C for heat treatment for 1 to 24 hours, 12 to 36 hours, or 12 to 24 hours. At this time, the water vapor hourly gas flow rate may be 10,000 to 200,000 mL / g·h or 100,000 to 200,000 mL / g·h relative to the weight of the hydrocarbon adsorption and desorption composite, which is a severe case similar to those applied to the HC trap when the vehicle is driven for a long time.

[0076] The hydrocarbon adsorption and desorption composite obtained by hydrothermal treatment exhibits lower hydrocarbon treatment efficiency compared with the fresh hydrocarbon adsorption and desorption composite; however, in the comparison after hydrothermal treatment, the hydrocarbon adsorption and desorption composite having a sodium to aluminum molar ratio (Na / Al) of 0.7 or less exhibits more improved heat resistance and excellent hydrocarbon treatment efficiency than the hydrocarbon adsorption and desorption composite having a sodium to aluminum molar ratio (Na / Al) of 0.7 or higher.

[0077] In addition, the present invention provides a hydrocarbon adsorption and desorption composite for a vehicle, which includes the hydrocarbon adsorption and desorption composite according to the above aspect. The hydrocarbon adsorption and desorption composite according to the present invention exhibits excellent hydrocarbon adsorption and exhibits hydrocarbon oxidation at a temperature of about 200°C, so that the adsorbed hydrocarbons are oxidized even at lower temperatures, and ensures hydrothermal stability at high temperatures. Therefore, the hydrocarbon adsorption and desorption composite according to the present invention can be applied to the removal of hydrocarbons emitted from automobile exhaust, and exhibits excellent hydrocarbon adsorption and oxidation capabilities even during cold start before the three-way catalyst has sufficient activity, thereby producing an atmospheric purification effect.

[0078] Hereinafter, embodiments of the present invention will be described. However, the following embodiments are merely preferred embodiments of the present invention, and the scope of the present invention is not limited by the following embodiments.

[0079] [Example]

[0080] Example 1 (CuNaZ (0.5))

[0081] Synthesis of NaZ

[0082] 2.25 g of water was added to 3.75 g of tetrapropylammonium hydroxide (TPAOH, 40 wt.%, in H2O, Sigma-Aldrich) and stirred for about 10 minutes. Then, 6.25 g of tetraethyl orthosilicate (TEOS, 98%, Sigma-Aldrich) was added dropwise. This is called mixture A. Another mixture B contained 1.81 g of water, 0.45 g of aluminum nitrate nonahydrate (Al(NO3)3·9H2O, Sigma-Aldrich) and 0.12 g of sodium hydroxide (NaOH, Sigma-Aldrich). Mixture B was added to mixture A and sealed with an autoclave. It was then placed in an oven preheated to 160°C for hydrothermal synthesis for 24 hours. Then, it was washed four times with deionized water to remove impurities, and vacuum filtered using 500 mL of water to remove sodium that was not contained in the zeolite structure. Then, it was dried at 70°C overnight and calcined at 550°C for 12 hours under an air flow of 300 mL / min. By Figure 1 Scanning electron microscopy images and X-ray diffraction analysis confirmed its shape and composition. Figure 1 It can be seen that the zeolite particles have micropores on the surface through the scanning electron microscope image, and the zeolite particles have an MFI type structure through the X-ray diffraction analysis diagram.

[0083] Synthesis of NaZ(0.5)

[0084] Then, the molar ratio of sodium to aluminum of zeolite particles is controlled by ion exchange process. Specifically, 1g of calcined sodium cation-containing zeolite particles (NaZ) is added to 100mL 0.005M ammonium nitrate solution, which is prepared by dissolving 0.04g ammonium nitrate (NH4NO3, 99%, Sigma-Aldrich) in about 100g deionized water. The resulting suspension is stirred in an oscillator (SI-300R, Lab Companion) for one day to obtain an ion exchange sample. The sample obtained is recovered by centrifugation, decantation and washing once with deionized water. The recovered sample is dried and calcined at 550°C for 12 hours at a heating rate of 1°C / min under an air flow of 300mL / min to prepare zeolite particles with a controlled sodium cation ratio.

[0085] Synthesis of CuNaZ(0.5)

[0086] Then, 5 wt% copper was impregnated into zeolite particles with a controlled sodium cation ratio by a wet impregnation method to prepare a hydrocarbon adsorption and desorption composite. Specifically, a 0.04 M copper II nitrate (Cu(NO3)2) solution was prepared by dissolving copper nitrate trihydrate (Cu(NO3)2·3H2O, 98%, Sigma-Aldrich) in approximately 80 g of deionized water. Zeolite particles with a controlled sodium cation ratio were added to the copper nitrate solution to finally be impregnated with approximately 5 wt% Cu. Then, the mixture was placed in a rotary evaporator to remove all moisture, and then the copper-impregnated zeolite particles (CuNaZ(0.5)) were recovered, dried at 100°C overnight, and calcined at 550°C for 6 hours at a heating rate of 1°C / min under an air flow of 300 mL / min in a box furnace to prepare a hydrocarbon adsorption and desorption composite.

[0087] Example 2 (CuNaZ (0.2))

[0088] In the above Example 1, 1 g of calcined sodium cation-containing zeolite particles (NaZ) was added to 100 mL of 1 M ammonium nitrate solution prepared by dissolving 8 g of ammonium nitrate (NH4NO3, 99%, Sigma-Aldrich) in about 100 g of deionized water. A hydrocarbon adsorption and desorption composite was prepared in the same manner as in Example 1, except that the resulting suspension was stirred in a shaker (SI-300R, Lab Companion) for 24 hours to obtain an ion exchange sample.

[0089] Example 3 (CuNaZ (0.0))

[0090] In the above Example 1, 1 g of calcined sodium cation-containing zeolite particles (NaZ) was added to 100 mL of 1 M ammonium nitrate solution prepared by dissolving 8 g of ammonium nitrate (NH4NO3, 99%, Sigma-Aldrich) in about 100 g of deionized water. The process of stirring the resulting suspension in a shaker (SI-300R, Lab Companion) for 24 hours to obtain an ion exchange sample was repeated 3 times, and a hydrocarbon adsorption and desorption composite was prepared in the same manner as in Example 1.

[0091] Example 4 (CuNaZ(0.5)_HT)

[0092] The hydrocarbon adsorption and desorption composite prepared in Example 1 was hydrothermally treated with 10 mol % H2O vapor at 800°C for 24 hours under air flow to prepare a hydrothermally-treated hydrocarbon adsorption and desorption composite. At this time, the hourly gas flow rate of the simulated exhaust gas containing water vapor was 100,000 mL / g·h relative to the weight of the hydrocarbon adsorption and desorption composite.

[0093] Example 5 (CuNaZ(0.2)_HT)

[0094] The hydrocarbon adsorption and desorption composite prepared in Example 2 was hydrothermally treated with 10 mol % H2O vapor at 800°C for 24 hours under air flow to prepare a hydrothermally-treated hydrocarbon adsorption and desorption composite. At this time, the hourly gas flow rate of the simulated exhaust gas containing water vapor was 100,000 mL / g·h relative to the weight of the hydrocarbon adsorption and desorption composite.

[0095] Example 6 (CuNaZ(0.0)_HT)

[0096] The hydrocarbon adsorption and desorption composite prepared in Example 3 was hydrothermally treated with 10 mol % H2O vapor at 800°C for 24 hours under air flow to prepare a hydrothermally-treated hydrocarbon adsorption and desorption composite. At this time, the hourly gas flow rate of the simulated exhaust gas containing water vapor was 100,000 mL / g·h relative to the weight of the hydrocarbon adsorption and desorption composite.

[0097] Comparative Example 1 (CuNaZ (1.0))

[0098] A hydrocarbon adsorption and desorption composite was prepared in the same manner as in Example 1, except that the ion exchange reaction in Example 1 was not performed.

[0099] Comparative Example 2 (CuNaZ (0.8))

[0100] In the above-mentioned Example 1, 1 g of calcined sodium cation-containing zeolite particles (NaZ) was added to 100 mL of 0.001 M ammonium nitrate solution prepared by dissolving 0.008 g of ammonium nitrate (NH4NO3, 99%, Sigma-Aldrich) in about 100 g of deionized water. A hydrocarbon adsorption and desorption composite was prepared in the same manner as in Example 1, except that the resulting suspension was stirred in a shaker (SI-300R, Lab Companion) for 24 hours to obtain an ion exchange sample.

[0101] Comparative Example 3 (CuNaZ(1.0)_HT)

[0102] The hydrocarbon adsorption and desorption composite prepared in Comparative Example 1 was hydrothermally treated with 10 mol % H2O vapor at 800°C for 24 hours under air flow to prepare a hydrocarbon adsorption and desorption composite. At this time, the hourly gas flow rate of the simulated exhaust gas containing water vapor was 100,000 mL / g·h relative to the weight of the hydrocarbon adsorption and desorption composite.

[0103] Comparative Example 4 (CuNaZ(0.8)_HT)

[0104] The hydrocarbon adsorption and desorption composite prepared in Comparative Example 2 was hydrothermally treated with 10 mol% H2O vapor at 800°C for 24 hours under air flow to prepare a hydrocarbon adsorption and desorption composite. At this time, the hourly gas flow rate of the simulated exhaust gas containing water vapor was 100,000 mL / g·h relative to the weight of the hydrocarbon adsorption and desorption composite.

[0105] Hereinafter, a hydrocarbon adsorption and desorption composite was prepared by a method different from that described above.

[0106] Example 7 (CuNaZ (0.7))

[0107] Synthesis of NaZ(0.7)

[0108] First, 1 g of commercially available ammonium ZSM-5 zeolite was mixed with 100 mL of 0.1 M sodium nitrate (NaNO3) solution, and the mixture was stirred at room temperature for 24 hours to obtain a sample. The sample obtained was recovered by centrifugation, decantation and washing once with deionized water. The recovered sample was dried and calcined at 550° C. for 12 hours at a heating rate of 1° C. / min under an air flow of 300 mL / min to prepare zeolite particles with a controlled sodium cation ratio.

[0109] The shape and composition of ammonium ZSM-5 zeolite (Si / Al=25) are determined by Figure 2 The scanning electron microscope images and X-ray diffraction analysis patterns confirmed. Figure 2 , it can be seen that the zeolite particles with micropores on the surface are identified by the scanning electron microscope image, and it can be seen from the X-ray diffraction analysis diagram that the zeolite particles have an MFI type structure.

[0110] Synthesis of CuNaZ(0.7)

[0111] Then, 5 wt% copper was impregnated into zeolite particles with a controlled sodium cation ratio by a wet impregnation method to prepare a hydrocarbon adsorption and desorption composite. Specifically, a 0.04 M copper nitrate II (Cu(NO3)2) solution was prepared by dissolving copper nitrate trihydrate (Cu(NO3)2·3H2O, 98%, Sigma-Aldrich) in approximately 80 g of deionized water. Zeolite particles with a controlled sodium cation ratio were added to the copper nitrate solution to finally be impregnated with approximately 5 wt% Cu. Then, the mixture was placed in a rotary evaporator to remove all moisture, and the copper-impregnated zeolite particles (CuNaZ(0.7)) were recovered, dried at 100°C overnight, and calcined at 550°C for 6 hours at a heating rate of 1°C / min under an air flow of 300 mL / min in a box furnace to prepare a hydrocarbon adsorption and desorption composite.

[0112] Example 8 (CuNaZ (0.4))

[0113] A hydrocarbon adsorption and desorption composite was prepared in the same manner as in Example 7, except that a 0.01 M sodium nitrate (NaNO 3 ) solution was used instead of a 0.1 M sodium nitrate (NaNO 3 ) solution.

[0114] Example 9 (CuNaZ (0.1))

[0115] A hydrocarbon adsorption and desorption composite was prepared in the same manner as in Example 7, except that a 0.001 M sodium nitrate (NaNO 3 ) solution was used instead of a 0.1 M sodium nitrate (NaNO 3 ) solution.

[0116] Example 10 (CuNaZ(0))

[0117] A hydrocarbon adsorption and desorption composite was prepared in the same manner as in Example 7, except that the sodium nitrate (NaNO 3 ) solution was not used.

[0118] Example 11 (CuNaZ(0.7)_HT)

[0119] The hydrocarbon adsorption and desorption composite prepared in Example 7 was hydrothermally treated with 10 mol % H2O vapor at 800°C for 24 hours under air flow to prepare a hydrocarbon adsorption and desorption composite. At this time, the hourly gas flow rate of the simulated exhaust gas containing water vapor was 100,000 mL / g·h relative to the weight of the hydrocarbon adsorption and desorption composite.

[0120] Example 12 (CuNaZ(0.4)_HT)

[0121] The hydrocarbon adsorption and desorption composite prepared in Example 8 was hydrothermally treated with 10 mol % H2O vapor at 800°C for 24 hours under air flow to prepare a hydrocarbon adsorption and desorption composite. At this time, the hourly gas flow rate of the simulated exhaust gas containing water vapor was 100,000 mL / g·h relative to the weight of the hydrocarbon adsorption and desorption composite.

[0122] Example 13 (CuNaZ(0.1)_HT)

[0123] The hydrocarbon adsorption and desorption composite prepared in Example 9 was hydrothermally treated with 10 mol % H2O vapor at 800°C for 24 hours under air flow to prepare a hydrocarbon adsorption and desorption composite. At this time, the hourly gas flow rate of the simulated exhaust gas containing water vapor was 100,000 mL / g·h relative to the weight of the hydrocarbon adsorption and desorption composite.

[0124] Example 14 (CuNaZ(0)_HT)

[0125] The hydrocarbon adsorption and desorption composite prepared in Example 10 was hydrothermally treated with 10 mol % H2O vapor at 800°C for 24 hours under air flow to prepare a hydrocarbon adsorption and desorption composite. At this time, the hourly gas flow rate of the simulated exhaust gas containing water vapor was 100,000 mL / g·h relative to the weight of the hydrocarbon adsorption and desorption composite.

[0126] Comparative Example 5 (CuNaZ (1.1))

[0127] A hydrocarbon adsorption and desorption composite was prepared in the same manner as in Example 7, except that in Example 7, a 1.0 M sodium nitrate (NaNO 3 ) solution was used instead of a 0.1 M sodium nitrate (NaNO 3 ) solution and the stirring was repeated three times.

[0128] Comparative Example 6 (CuNaZ(1.1)_HT)

[0129] The hydrocarbon adsorption and desorption composite prepared in Comparative Example 5 was hydrothermally treated with 10 mol % H2O vapor at 800°C for 24 hours under air flow to prepare a hydrocarbon adsorption and desorption composite. At this time, the hourly gas flow rate of the simulated exhaust gas containing water vapor was 100,000 mL / g·h relative to the weight of the hydrocarbon adsorption and desorption composite.

[0130] [Experimental example]

[0131] Experimental Example 1 – Elemental Analysis Results

[0132] Elemental analysis was performed on the hydrocarbon adsorption and desorption composites of Examples 1 to 14 and Comparative Examples 1 to 6 to confirm the element ratios of the hydrocarbon adsorption and desorption composites according to the present invention, and the results are shown in Tables 1 and 2.

[0133] [Table 1]

[0134]

[0135] [Table 2]

[0136]

[0137]

[0138] Referring to Tables 1 and 2, the Si / Al molar ratio, Na / Al molar ratio and Cu loading of the HC trap according to the present invention, which is obtained by ion exchange reaction of zeolite containing sodium cations (Na-type ZSM-5) and copper loaded therein, are confirmed by elemental analysis. The Na / Al molar ratio is controlled by the ion exchange reaction. Specifically, it can be seen that although there is no significant difference in the Si / Al molar ratio and the copper content between the embodiment and the comparative example, the Na / Al molar ratio varies according to the ion exchange reaction time.

[0139] Experimental Example 2

[0140] In order to confirm the adsorption amount of hydrocarbons and the hydrocarbon treatment efficiency in the hydrocarbon adsorption and desorption composite according to the present invention with respect to the molar ratio of sodium to aluminum and with or without a copper support, a cold start test (CST) was conducted for Comparative Example 1 (CuNaZSM-5), Example 3 (CuHZSM-5), a zeolite containing sodium cations (NaZSM-5), and a zeolite containing hydrogen cations (HZSM-5), and the results are shown in FIG. Figure 3 Displayed in.

[0141] In the cold start test, 100 mL / min of simulated exhaust gas feed was flowed into 0.06 g of zeolite particles, which had been pretreated at 600°C for 30 minutes under the condition of 30 mL / min He. At this time, the simulated exhaust gas feed composition was 100 ppm propylene, 100 ppm toluene, 1 mol% oxygen (O2) and 10 mol% water vapor (H2O), and the balance was helium (He), totaling 100 mL / min, where feed / weight = 100,000 mL / g·h, and exposed at 70°C for 5 minutes, then under a temperature increase condition of 53°C / min for 10 minutes, and then exposed at 600°C for 5 minutes, and then the adsorption and desorption behavior of propylene, toluene and total hydrocarbons of hydrocarbons were determined by mass spectrometry and gas chromatography.

[0142] The adsorption amount was calculated as the amount of propylene and toluene adsorbed until the concentration of released propylene became equal to the concentration of injected propylene and toluene (inlet concentration, 100 ppm).

[0143] Figure 3 Graph showing cold start test results of the hydrocarbon adsorption and desorption composite according to the present invention and the hydrocarbon adsorption and desorption composite of a comparative example. Figure 3 , the concentrations of propylene, toluene, and total hydrocarbons of Example 3, Comparative Example 1, zeolite containing sodium cations (NaZSM-5), and zeolite containing hydrogen cations (HZSM-5) during the cold start period can be confirmed. Specifically, in the case of zeolite containing sodium cations (NaZSM-5) and zeolite containing hydrogen cations (HZSM-5), it was confirmed that propylene was not adsorbed. On the other hand, in the case of toluene, it was confirmed that toluene was adsorbed to about 150°C and then released. In the case of copper loading in Example 3 and Comparative Example 1, reference Figure 3 (a1) and (a2) of Example 3, confirming that Example 3 shows similar results to the zeolite containing sodium cations before 300°C, and referring to Figure 2(b1) and (b2), Example 3 shows that, unlike the zeolite containing hydrogen cations, propylene is adsorbed and the desorption amount of toluene is reduced. In the case of the copper-loaded HC trap, propylene and toluene were not detected at a temperature of 300°C or higher, which can be seen to be the result of copper oxide formed during the copper loading process.

[0144] Experimental Example 3

[0145] In order to confirm the hydrocarbon adsorption performance related to the molar ratio of sodium to aluminum in the zeolite of the hydrocarbon adsorption and desorption composite according to the present invention, the HC traps prepared in Examples 1 to 5 and Comparative Examples 1 to 4 were subjected to cold start tests (CST), and the results are shown in Figures 4 to 12 middle.

[0146] The adsorption amount was calculated as the amount of hydrocarbon adsorbed until the released propylene concentration was equal to the concentration of injected hydrocarbon (inlet concentration, 100 ppm), and the hydrocarbon treatment efficiency was expressed by calculating the ratio of the concentration of adsorbed and oxidized hydrocarbons (In-Out) to the concentration of injected hydrocarbons (In), which indicates that hydrocarbon emissions can reach 300°C, at which time the TWC starts to work.

[0147] Figure 4 Graphs showing the results of cold start tests of propylene and toluene on the hydrocarbon adsorption and desorption composites according to the present invention and the hydrocarbon adsorption and desorption composites of comparative examples. Specifically, (a) is a graph of propylene adsorption and desorption in the cold start test of the fresh hydrocarbon adsorption and desorption composites of Examples 1 to 3 and Comparative Examples 1 and 2, (b) is a graph of propylene adsorption and desorption in the cold start test of the hydrocarbon adsorption and desorption composites of Examples 4 to 6 and Comparative Examples 3 and 4 subjected to hydrothermal treatment (hydrothermal treated hydrocarbon adsorption and desorption composites), (c) is a graph of toluene adsorption and desorption in the cold start test of the hydrothermally treated hydrocarbon adsorption and desorption composites of Examples 1 to 3 and Comparative Examples 1 and 2, and (d) is a graph of toluene adsorption and desorption in the cold start test of the hydrothermally treated hydrocarbon adsorption and desorption composites of Examples 4 to 6 and Comparative Examples 3 and 4.

[0148] refer to Figure 4 , it can be confirmed that the adsorption amount increases with the decrease of the molar ratio of sodium to aluminum (Na / Al) in the hydrocarbon adsorption and desorption composite, and in particular, the adsorption amount is most excellent when the molar ratio of sodium to aluminum is 0.5. In addition, it can be seen that in the case of the hydrothermally treated HC trap, the adsorption amount is not higher than that of the fresh HC trap, but Examples 4 to 6 adsorb propylene and toluene even after the hydrothermal treatment. However, it can be seen that Comparative Examples 3 and 4 adsorb only toluene and do not adsorb propylene.

[0149] Figure 5The figures are the cold start test results of propylene and toluene of the hydrocarbon adsorption and desorption composites of the present invention and the hydrocarbon adsorption and desorption composites of the comparative examples. Specifically, (a) is a figure of propylene adsorption and desorption of the hydrothermally treated hydrocarbon adsorption and desorption composites of Examples 7 to 10 and Comparative Example 5 in the cold start test, (b) is a figure of propylene adsorption and desorption of the hydrothermally treated hydrocarbon adsorption and desorption composites of Examples 11 to 14 and Comparative Example 6 in the cold start test, (c) is a figure of toluene adsorption and desorption of the hydrothermally treated hydrocarbon adsorption and desorption composites of Examples 7 to 10 and Comparative Example 5 in the cold start test, and (d) is a figure of toluene adsorption and desorption of the hydrothermally treated hydrocarbon adsorption and desorption composites of Examples 11 to 14 and Comparative Example 6 in the cold start test.

[0150] refer to Figure 5 , in the case of fresh hydrocarbon adsorption and desorption composites (Examples 7 to 10 and Comparative Example 5), the adsorption amount increases as the molar ratio of sodium to aluminum (Na / Al) decreases. It can be seen that when each hydrocarbon adsorption and desorption composite (Examples 11 to 14 and Comparative Example 6) is hydrothermally treated, the adsorption amount is not higher than that of the fresh hydrocarbon adsorption and desorption composite, but Examples 11 to 14 adsorb propylene and toluene even after hydrothermal treatment. However, it can be seen that Comparative Example 6 adsorbs only toluene but not propylene. Among them, it was confirmed that in the case of propylene, the adsorption amount was the most excellent when the molar ratio of sodium to aluminum was 0.4 (Example 12), and in the case of toluene, the adsorption amount was the most excellent when the molar ratio of sodium to aluminum was 0.7 (Example 11).

[0151] Figure 6 Graphs showing cold start test results of total hydrocarbons for the hydrocarbon adsorption and desorption composites according to the present invention and the HC traps of comparative examples. Specifically, (a) is a graph of total hydrocarbon adsorption and desorption in the cold start test for the fresh hydrocarbon adsorption and desorption composites of Examples 1 to 3 and Comparative Examples 1 and 2, and (b) is a graph of total hydrocarbon adsorption and desorption in the cold start test for the hydrothermally treated hydrocarbon adsorption and desorption composites of Examples 4 to 6 and Comparative Examples 3 and 4.

[0152] refer to Figure 6 , it can be seen that the total hydrocarbon adsorption increases as the sodium to aluminum molar ratio of the hydrocarbon adsorption and desorption composite decreases, and it can be seen that in the case of hydrothermal treatment the adsorption amount is not higher than that in the fresh HC trap, but even after hydrothermal treatment the total hydrocarbons are adsorbed.

[0153] Figure 7Graphs showing cold start test results of total hydrocarbons for the hydrocarbon adsorption and desorption composites according to the present invention and the HC traps of comparative examples. Specifically, (a) is a graph of total hydrocarbon adsorption and desorption in the cold start test for the fresh hydrocarbon adsorption and desorption composites of Examples 7 to 10 and Comparative Example 5, and (b) is a graph of total hydrocarbon adsorption and desorption in the cold start test for the hydrothermally treated hydrocarbon adsorption and desorption composites of Examples 11 to 14 and Comparative Example 6.

[0154] refer to Figure 7 , it can be seen that the total hydrocarbon adsorption increases as the sodium to aluminum molar ratio of the hydrocarbon adsorption and desorption composite decreases, and it can be seen that in the case of hydrothermal treatment the adsorption amount is not higher than that in the fresh HC trap, but hydrocarbons are adsorbed even after hydrothermal treatment.

[0155] Figure 8 Graphs showing the results of cold start tests of carbon dioxide and carbon monoxide for the hydrocarbon adsorption and desorption composites according to the present invention and the hydrocarbon adsorption and desorption composites of comparative examples. Specifically, (a) is a graph showing the change in the amount of carbon dioxide in the cold start test of the fresh hydrocarbon adsorption and desorption composites of Examples 7 to 10 and Comparative Example 5, (b) is a graph showing the change in the amount of carbon dioxide in the cold start test of the hydrothermally treated hydrocarbon adsorption and desorption composites of Examples 11 to 14 and Comparative Example 6, (c) is a graph showing the change in the amount of carbon monoxide in the cold start test of the hydrothermally treated hydrocarbon adsorption and desorption composites of Examples 7 to 10 and Comparative Example 5, and (d) is a graph showing the change in the amount of carbon monoxide in the cold start test of the hydrothermally treated hydrocarbon adsorption and desorption composites of Examples 11 to 14 and Comparative Example 6. Figure 8 The graph of is measured by MS, and the temperature at which oxidation starts is assigned based on the time at which 200 ppm CO2 is released.

[0156] refer to Figure 8 It can be seen that as the molar ratio of sodium to aluminum of the hydrocarbon adsorption and desorption composite decreases, the generation of carbon dioxide and carbon monoxide increases, and in particular, it can be confirmed that when the Na / Al value is 0.7 or less, the generation of carbon dioxide and carbon monoxide is large. In addition, it can be seen that in the case of hydrothermal treatment, the generation of carbon monoxide and carbon dioxide is significantly lower than that of the fresh HC trap.

[0157] Fig. 9 Graph showing the adsorption and desorption efficiency and the adsorption amount of propylene and toluene before reaching 300° C. with respect to the molar ratio of sodium to aluminum and with or without hydrothermal treatment in the hydrocarbon adsorption and desorption composite according to the present invention. Fig. 9 Graph 1 is a graph in which toluene, propylene, and total hydrocarbon processing efficiencies are summarized according to Na / Al values.

[0158] See also Fig. 9, the first figure shows the hydrocarbon treatment efficiency of the hydrocarbon adsorption and desorption composite with respect to the molar ratio of sodium to aluminum, wherein it can be seen that as the molar ratio of sodium to aluminum decreases, the hydrocarbon treatment efficiency is excellent. Specifically, it can be seen that in the case of the hydrothermal treatment composite, the efficiency is highest when the molar ratio of sodium to aluminum is 0.5, and the efficiency decreases as the molar ratio decreases. The second figure shows the adsorption amount of propylene of the hydrocarbon adsorption and desorption composite with respect to the molar ratio of sodium to aluminum, wherein it can be seen that as the molar ratio of sodium to aluminum decreases, the adsorption amount of propylene increases, and the fresh composite generally shows a better adsorption amount. The third figure shows the adsorption amount of toluene of the hydrocarbon adsorption and desorption composite with respect to the molar ratio of sodium to aluminum, wherein it can be seen that when the molar ratio of sodium to aluminum is 0.5, the adsorption amount of toluene is the largest, and the fresh composite shows a better adsorption amount.

[0159] Fig.10 A graph showing hydrocarbon treatment efficiency for propylene, toluene and total hydrocarbons before reaching 300° C. in a hydrocarbon adsorption and desorption composite according to the present invention with respect to the molar ratio of sodium to aluminum and with or without hydrothermal treatment. Fig.10 Graph 1 is a graph in which toluene, propylene, and total hydrocarbon processing efficiencies are summarized according to Na / Al values.

[0160] Reference Fig.10 , which shows the hydrocarbon treatment efficiency of the hydrocarbon adsorption and desorption composite with respect to the molar ratio of sodium to aluminum, wherein it can be seen that as the molar ratio of sodium to aluminum decreases, the hydrocarbon treatment efficiency is excellent. In particular, it can be confirmed that when the molar ratio of sodium to aluminum is 0 to 0.7, the hydrocarbon treatment efficiency is better than that at 1.1.

[0161] Fig.11 A graph showing the total hydrocarbon adsorption and the onset oxidation temperature of hydrocarbon adsorption and desorption composites according to the present invention and hydrocarbon adsorption and desorption composites of comparative examples, graphs of Comparative Examples 1 to 4 and Examples 1 to 6, wherein the molar ratio of sodium to aluminum is controlled by replacing sodium cations with hydrogen cations. Fig.11 The x-axis of the graph represents calculated data values ​​of the total hydrocarbon adsorption amount obtained by a flame ionization detector (GC), and the y-axis represents the starting oxidation temperature, which represents the temperature at which the CO 2 generation amount is 5% or more relative to the total hydrocarbon.

[0162] Reference Fig.11, it can be confirmed that the hydrocarbon adsorption and desorption composite of Example 3 exhibits the lowest initial oxidation temperature by exhibiting an initial oxidation temperature of about 200°C, while exhibiting the highest hydrocarbon adsorption amount. In particular, it can be seen that the hydrocarbon adsorption and desorption composites of Examples 1 to 3 exhibit an initial oxidation temperature of about 200°C to 210°C and have a higher initial oxidation temperature as the molar ratio of sodium to aluminum increases. In addition, it can be seen that in the case of the hydrothermally treated hydrocarbon adsorption and desorption composites, the initial oxidation temperature increases compared to those that have not been hydrothermally treated, but in the hydrocarbon adsorption and desorption composites of Examples 4 to 6, the oxidation proceeds to a certain level or more at a temperature of about 240°C, which is lower than that of the comparative example. Therefore, it can be seen that the hydrocarbon adsorption and desorption composite of the present embodiment has a smaller copper oxide particle size for hydrocarbon oxidation and therefore has the lowest hydrocarbon oxidation temperature. In addition, it can be confirmed that the HC traps of Examples 1 to 3 show 0.33 mmol CH4 / g or more, and even when subjected to hydrothermal treatment, the hydrocarbon adsorption amount is higher than that of the hydrocarbon adsorption and desorption composite of the comparative example.

[0163] Fig.12 A graph showing the total hydrocarbon adsorption and onset oxidation temperature for hydrocarbon adsorption and desorption composites according to the present invention and hydrocarbon adsorption and desorption composites of comparative examples, graphs for Comparative Examples 5 and 6 and Examples 7 to 14, wherein the molar ratio of sodium to aluminum is controlled by replacing hydrogen cations with sodium cations. Fig.12 The x-axis of the graph represents calculated data values ​​of the total hydrocarbon adsorption amount obtained by a flame ionization detector (GC), and the y-axis represents the starting oxidation temperature, which represents the temperature at which the CO 2 generation amount is 5% or more relative to the total hydrocarbon.

[0164] Reference Fig.12 , it can be confirmed that the hydrocarbon adsorption and desorption composite of Example 9 exhibits the lowest initial oxidation temperature by exhibiting an initial oxidation temperature of about 180°C, while exhibiting the highest hydrocarbon adsorption amount. In particular, it can be seen that the hydrocarbon adsorption and desorption composites of Examples 7 to 10 exhibit an initial oxidation temperature of about 180°C to 220°C and have a higher initial oxidation temperature as the molar ratio of sodium to aluminum increases. In addition, it can be seen that in the case of the hydrothermally treated hydrocarbon adsorption and desorption composites, the initial oxidation temperature increases compared to those that are not hydrothermally treated, but in the hydrocarbon adsorption and desorption composites of Examples 13 and 14, the oxidation is carried out at a temperature of about 240°C, which is a lower temperature than that in the comparative example, at a temperature of 210°C to 230°C, which is a lower temperature than that in the comparative example. Therefore, it can be seen that the hydrocarbon adsorption and desorption composite of the present embodiment has a smaller copper oxide particle size for hydrocarbon oxidation and therefore has the lowest hydrocarbon oxidation temperature. In addition, it can be confirmed that the HC traps of Examples 7 to 10 show 0.35 mmol CH4 / g or more, and even when subjected to hydrothermal treatment, the hydrocarbon adsorption amount is higher than that of the hydrocarbon adsorption and desorption composite of the comparative example.

[0165] Therefore, it can be seen that the hydrocarbon adsorption and desorption composite according to the present invention improves the hydrothermal stability by controlling the molar ratio of sodium to aluminum of the zeolite particles and impregnating copper, and adsorbs a large amount of hydrocarbons and oxidized hydrocarbons at a temperature below the activation temperature of the three-way catalyst by lowering the temperature at which oxidation is performed.

Claims

1. A hydrocarbon adsorption and desorption composite comprising: Zeolite particles containing cations; metal ions chemically bonded to the zeolite particles; and providing a metal oxide on the outer surface of said zeolite particles, wherein the cations include cations of sodium and hydrogen, and the Na / Al molar ratio of the zeolite particles is less than 0.7, wherein the zeolite particles are ZSM-5 zeolite, wherein the Si / Al molar ratio of the hydrocarbon adsorption and desorption composite is from 20.6 to 30.6, The hydrocarbon adsorption and desorption complex satisfies the following formula 1: in Q In represents the total amount of hydrocarbon injected into the hydrocarbon adsorption and desorption complex at a temperature of 300°C, Q Out represents the total amount of hydrocarbons released by the hydrocarbon adsorption and desorption composite at a temperature of 300°C, and A is a number greater than 40 and represents the hydrocarbon treatment efficiency, wherein the size of the hydrocarbon adsorption and desorption complex is 50 to 5000 nm, and the size of the metal oxide is 1 to 10 nm, The volume V1 of micropores with a size of 1 nm or less is 0.1 cm 3 / g or greater, and The feed gas composition in Formula 1 is 100 ppm propylene, 100 ppm toluene, 1 mol% oxygen and 10 mol% water vapor, with the remainder being helium, totaling 100 mL / min, wherein feed gas / weight = 100,000 mL / g·h, and is exposed at 70°C for 5 minutes, then at a temperature rise condition of 53°C / min for 10 minutes, and then at 600°C for 5 minutes.

2. The hydrocarbon adsorption and desorption composite according to claim 1, further comprising obtaining the hydrothermally-treated hydrocarbon adsorption and desorption composite by the steps of: hydrothermally treating the hydrocarbon adsorption and desorption composite using 5 to 15 mol% of water vapor at 600°C to 900°C for 1 hour to 36 hours, and For the hydrothermally-treated hydrocarbon adsorption and desorption composite, A in Formula 1 is a number greater than 5.

3. The hydrocarbon adsorption and desorption composite according to claim 1, wherein the metal ions are chemically bound inside pores formed in the zeolite particles.

4. The hydrocarbon adsorption and desorption composite according to claim 1, wherein the hydrocarbon adsorption and desorption composite exhibits hydrocarbon adsorption at temperatures below 300°C, and Hydrocarbon oxidation is exhibited at temperatures above 180°C.

5. The hydrocarbon adsorption and desorption composite according to claim 1, wherein the hydrocarbon adsorption amount of the hydrocarbon adsorption and desorption composite is 0.32 to 1.5 mmol CH4 / g, and The hydrocarbon oxidation onset temperature of the hydrocarbon adsorption and desorption composite is 180 to 350°C.

6. The hydrocarbon adsorption and desorption composite according to claim 1, wherein the metal ion is a cation of any one or more metals of Groups 3 to 12 elements, and The metal oxide is an oxide of any one or more metals of Group 3 to 12 elements.

7. The hydrocarbon adsorption and desorption composite according to claim 6, wherein the metal ions include cations of any one or more metals of iron, cobalt, nickel, copper, zinc, rhodium and cadmium, and The metal oxide is an oxide of any one or more metals selected from the group consisting of iron, cobalt, nickel, copper, zinc, rhodium and cadmium.

8. A method for preparing a hydrocarbon adsorption and desorption composite, comprising: Controlling the cation ratio of the zeolite particles by using an ion exchange method; and forming metal ions and metal oxides by mixing the zeolite particles having a controlled cation ratio with a solution containing metal ions; wherein in controlling the cation ratio, the Na / Al molar ratio of the zeolite particles is controlled to be less than 0.7, wherein the zeolite particles are ZSM-5 zeolite, wherein the Si / Al molar ratio of the hydrocarbon adsorption and desorption composite is from 20.6 to 30.6, The hydrocarbon adsorption and desorption complex satisfies the following formula 1: in Q In represents the total amount of hydrocarbon injected into the hydrocarbon adsorption and desorption complex at a temperature of 300°C, Q Out represents the total amount of hydrocarbons released by the hydrocarbon adsorption and desorption composite at a temperature of 300°C, and A is a number greater than 40 and represents the hydrocarbon treatment efficiency, wherein the size of the hydrocarbon adsorption and desorption complex is 50 to 5000 nm, and the size of the metal oxide is 1 to 10 nm, The volume V1 of micropores with a size of 1 nm or less is 0.1 cm 3 / g or greater, and The feed gas composition in Formula 1 is 100 ppm propylene, 100 ppm toluene, 1 mol% oxygen and 10 mol% water vapor, with the remainder being helium, totaling 100 mL / min, wherein feed gas / weight = 100,000 mL / g·h, and is exposed at 70°C for 5 minutes, then at a temperature rise condition of 53°C / min for 10 minutes, and then at 600°C for 5 minutes.

9. The method for preparing a hydrocarbon adsorption and desorption composite according to claim 8, wherein controlling the cation ratio comprises mixing the zeolite particles with an aqueous ammonium salt solution or an aqueous sodium salt solution, The ammonium salt aqueous solution contains any one or more of ammonium sulfate, ammonium nitrate, ammonium chloride, ammonium acetate, ammonium persulfate, ammonium bicarbonate and ammonium formate, and The sodium salt aqueous solution contains any one or more of sodium nitrate, sodium chloride, sodium acetate, sodium persulfate, sodium bicarbonate and sodium formate.

10. The method for preparing a hydrocarbon adsorption and desorption composite according to claim 8, wherein controlling the cation ratio comprises mixing the zeolite particles with aqueous ammonia.

11. The method for preparing a hydrocarbon adsorption and desorption composite according to claim 8, wherein a wet impregnation method is used for the formation of the metal ions and the metal oxide.

12. The method for preparing a hydrocarbon adsorption and desorption composite according to claim 8, further comprising, after forming the metal ions and the metal oxide, performing a hydrothermal treatment by injecting 5 to 15 mol % of water vapor at a temperature of 600° C. to 900° C. for 1 to 36 hours, The hourly gas flow rate of the simulated exhaust gas including water vapor is 10,000 to 200,000 mL / (g·h) relative to the weight of the hydrocarbon adsorption and desorption composite.

13. The method for preparing a hydrocarbon adsorption and desorption composite according to claim 8, further comprising metal ions, wherein the metal ions include cations of any one or more metals of Groups 3 to 12 elements.

14. A hydrocarbon adsorption and desorption composite for a vehicle, comprising the hydrocarbon adsorption and desorption composite according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Adsorbent medium containing lithium-exchanged zeolite

    JP2012512022A

  • Hydrocarbon adsorbent with metal-impregnated zeolite particle having regular mesopore and manufacturing method therefor

    CN111542388A

  • Modified large pore zeolites for trapping alkenes

    EP0639400A1

  • Novel zeolite and hydrocarbon adsorbent containing the same

    JP2019137560A

  • Hydrocarbon adsorbent

    US20200324268A1