FeS@C composite material rapidly prepared by microwave method, method and application thereof
The preparation of FeS@C composite materials is simplified through microwave reaction, and the complex and high energy consumption problems in the prior art are solved, and the rapid and low-cost preparation of FeS@C composite materials is realized, which is suitable for negative electrode materials in the secondary battery field.
Patent Information
- Application Number
- CN202210300376.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-03-24
AI Technical Summary
The existing methods for preparing FeS@C composites are complex, high energy consumption and long time-consuming, and it is difficult to meet the fast and low-cost production needs.
FeS@C composite materials are prepared by microwave reaction using strong acid cation exchange resin, sulfonated coal or sulfonated asphalt and trivalent ion solution, simplifying the process flow and reducing high-temperature carbonization and vulcanization steps.
It realizes the preparation of FeS@C composite materials with simple and efficient processes, with short reaction time and low energy consumption, and is suitable for negative electrode materials in the secondary battery field.
Smart Images

Figure CN114613967B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials, and specifically relates to a method for preparing a FeS@C composite material by microwave reaction using strongly acidic cation exchange resin, sulfonated coal or sulfonated asphalt and a trivalent iron ion solution as raw materials, and application thereof. Background Art
[0002] Ferrous sulfide (FeS) exists naturally in the form of pyrrhotite, with hexagonal and monoclinic crystal forms, and is abundant in reserves. In addition to being cheap and readily available, the unique structural characteristics give ferrous sulfide excellent photoelectric properties, surface activity and catalytic activity, making it show broad application prospects in the fields of organic wastewater treatment, direct coal liquefaction catalysts, heavy metal contaminated water or soil treatment. In addition, FeS also has excellent electrochemical lithium and sodium storage properties. With its high theoretical specific capacity (609mAh / g), environmental friendliness, and abundant resources, it has quickly become one of the hot candidate materials for the next generation of lithium and sodium ion electrode materials.
[0003] The composite of FeS and carbon can effectively increase the dispersibility of catalytic or adsorption active centers, improve the stability of catalytic or adsorption active centers, enhance the environmental compatibility of FeS main materials, and improve the electronic conductivity of composite materials, thereby improving their adsorption performance, catalytic performance and electrochemical performance. For example: Chinese patent CN112850836A discloses the preparation and application of a chitosan-stabilized ferrous sulfide composite biochar material, using highland barley crop straw as biochar raw material, chitosan as a stabilizer for ferrous sulfide, improving the stability of ferrous sulfide, making ferrous sulfide more evenly loaded on biochar, and enhancing the treatment effect of hexavalent chromium in polluted wastewater. Chinese patent CN112442378A discloses an adsorbent for heavy metal contaminated soil, a preparation method thereof, and a method for repairing soil using the adsorbent. Using soil heavy metal adsorption particles and sodium alginate carboxymethyl chitosan ferrous sulfide composite materials as raw materials, it can effectively improve the pH of the soil, and the adsorption capacity of various heavy metals in the soil can reach more than 95%. After repairing the soil, it can significantly reduce the compactness and bulk density of the soil, increase the looseness and porosity of the contaminated soil, and significantly improve the air permeability and water permeability of the soil. Chinese patent CN110302746A discloses a composite material for the repair of hexavalent chromium contaminated water or soil and a preparation method thereof, providing an easy-to-operate, efficient, environmentally friendly, and economically feasible hexavalent chromium contaminated water or soil repair material. Chinese patent CN110635125A discloses a method for preparing a ferrous sulfide / carbon composite positive electrode material, in which cotton products are selected as a carbon source, and the ferrous sulfide material is in situ loaded in its carbonized three-dimensional network structure. The lithium-ion battery prepared by using the composite material as a positive electrode material has better cycle performance and rate performance.
[0004] At present, there are two main methods for preparing FeS@C composite materials. One is the direct pyrolysis method, which directly obtains FeS@C composite materials by pyrolyzing the iron source. Chinese patent CN110600710A discloses a method for obtaining FeS@C composite materials by one-step carbonization, using iron p-toluenesulfonate hexahydrate as the iron source, and obtaining FeS@C composite materials by high-temperature pyrolysis at 600-700°C for 1-2h. Another method is to first prepare a Fe@C precursor, and then obtain the FeS@C composite material by sulfurization. Chinese patent CN110600710A discloses a method for obtaining FeS@C composite materials by one-step carbonization, using iron p-toluenesulfonate hexahydrate as the iron source, and obtaining FeS@C composite materials by high-temperature pyrolysis at 600-700°C for 1-2h. Chinese patent CN111584871A discloses a method for preparing a metal organic framework derived ferrous sulfide @ carbon nanocomposite material, using fumaric acid and ferric nitrate as raw materials, first obtaining spindle-shaped MIL 88 nanoparticles by a hydrothermal reaction method, then doping with sulfur, and calcining at 450°C for 4h to obtain a carbon-coated, sulfur-doped ferrous sulfide @ carbon nanocomposite material with a core-shell structure.
[0005] However, these methods are complex, energy-intensive and time-consuming in preparation process. Compared with the prior art, the present invention provides a method for preparing FeS@C composite material with simple operation and rapidity. Summary of the invention
[0006] The purpose of the present invention is to provide a preparation method of a FeS@C composite material and application thereof.
[0007] The object of the present invention is achieved by the following methods:
[0008] The present invention provides a method for preparing FeS@C composite material by using strong acid cation exchange resin, sulfonated coal or sulfonated asphalt through microwave method. The method uses strong acid cation exchange resin, sulfonated coal or sulfonated asphalt as raw materials, mixes with a solution containing trivalent iron ions, and then prepares FeS@C composite material by microwave method. The preparation method is time-saving, simple to operate and low in production cost.
[0009] The method for rapidly preparing FeS@C composite material by microwave method mainly comprises the following steps:
[0010] A strongly acidic cation exchange resin, sulfonated coal or sulfonated asphalt is added to a solution containing trivalent iron ions, stirred and mixed for a period of time, filtered and dried to obtain an iron exchange complex, which is added to an organic reagent, stirred and mixed for a period of time, and the obtained solid product is subjected to microwave reaction for a period of time under an inert gas atmosphere to obtain a final product;
[0011] Furthermore, the solution containing trivalent iron ions is one of ferric chloride solution, ferric sulfate solution, and ferric nitrate solution, or a mixture of two or more thereof.
[0012] Furthermore, the organic reagent is one of pyrrole and aniline or a mixture of the two.
[0013] Furthermore, the mass ratio of the strongly acidic cation exchange resin, sulfonated coal or sulfonated asphalt to the trivalent iron salt is 10:1-100.
[0014] Furthermore, the stirring and mixing time is 0.5 to 24 hours.
[0015] Furthermore, the drying conditions are: drying at 60-120° C. for 8-24 hours.
[0016] Furthermore, the mass ratio of the iron-exchanged complex to the organic reagent is 1:1-10.
[0017] Furthermore, the iron-exchanged complex is stirred and mixed in the organic reagent for 2 to 24 hours.
[0018] Furthermore, the inert gas is nitrogen, argon or a mixture of the two.
[0019] Furthermore, the microwave frequency is 100-1000W.
[0020] Furthermore, the microwave duty cycle is 0.1-1.
[0021] Furthermore, the microwave reaction time is 2 to 60 minutes.
[0022] Another aspect of the present invention is to provide a FeS@C composite material prepared by the above method.
[0023] Another aspect of the present invention is to provide the above-mentioned FeS@C composite material which can be applied in the fields of lithium ion battery negative electrode materials, sodium ion battery negative electrode materials, etc.
[0024] The beneficial effects of the present invention compared with the prior art are as follows:
[0025] 1. The preparation method of the present invention is simple and efficient, avoiding the long-term, high-temperature carbonization treatment and sulfurization steps that are usually required, with a short reaction time and low energy consumption.
[0026] 2. Ion exchange resins or sulfonated heavy organic components have the advantages of wide sources, low prices and high carbon yields. The present invention uses ion exchange resins or sulfonated heavy organic components as raw materials to prepare FeS@C composite materials, providing a method for their high added value utilization.
[0027] 3. The product FeS@C composite material can be used in the field of secondary batteries and used as battery negative electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention, the drawings related to the embodiments are briefly introduced below.
[0029] Figure 1 This is the XRD spectrum of the FeS@C composite material prepared in Example 2.
[0030] Figure 2 This is the SEM image of the FeS@C composite material prepared in Example 2.
[0031] Figure 3 This is a charge and discharge rate performance diagram of the lithium ion battery prepared in Example 8 at different current densities. DETAILED DESCRIPTION
[0032] The present invention is described in detail below with reference to the embodiments, but the embodiments of the present invention are not limited thereto. Obviously, the embodiments described below are only partial embodiments of the present invention. For those skilled in the art, other similar embodiments obtained without creative labor all fall within the protection scope of the present invention.
[0033] Example 1
[0034] At room temperature, 4 g of ion exchange resin (732 strong acid styrene cation exchange resin) and a solution containing 4 g of ferric chloride were stirred and mixed for 0.5 h, then filtered and dried at 60° C. for 24 h to obtain product A. Product A and an organic reagent pyrrole in a mass ratio of 1:1 were stirred and mixed for 2 h to obtain product B; the obtained product B was subjected to microwave reaction under a nitrogen atmosphere, with a microwave frequency of 100 W, a microwave duty cycle of 1, and a microwave time of 60 min.
[0035] Example 2
[0036] At room temperature, 5 g of sulfonated asphalt (FT-1) and a solution containing 50 g of ferric chloride were stirred and mixed for 12 h, then filtered and dried at 80°C for 12 h to obtain product A. Product A and an organic reagent pyrrole were taken at a mass ratio of 1:10 and stirred and mixed for 24 h to obtain product B; the obtained product B was subjected to microwave reaction under a nitrogen atmosphere, with a microwave frequency of 1000 W, a microwave duty cycle of 1, and a microwave time of 5 min.
[0037] The FeS@C composite material prepared in this embodiment was analyzed by X-ray diffraction using an X-ray diffractometer. Figure 1 As shown by Figure 1It can be seen that there are clearly visible diffraction peaks in the spectrum, and all diffraction peaks can be indexed as FeS phase. The surface morphology and microstructure of FeS@C material were observed by scanning electron microscopy. Figure 2 shown.
[0038] Example 3
[0039] At room temperature, 5 g of sulfonated asphalt (FT-1) and a solution containing 0.5 g of ferric sulfate were stirred and mixed for 12 h, then filtered and dried at 60°C for 8 h to obtain product A. Product A and organic reagent aniline were taken in a mass ratio of 1:1 and stirred and mixed for 4 h to obtain product B; the obtained product B was subjected to microwave reaction under a nitrogen atmosphere, with a microwave frequency of 200 W, a microwave duty cycle of 0.3, and a microwave time of 30 min.
[0040] Example 4
[0041] At room temperature, 4 g of sulfonated coal (ZG-S77) and a solution containing 4 g of ferric sulfate were stirred and mixed for 24 h, then filtered and dried at 120°C for 12 h to obtain product A. Product A and organic reagent aniline were taken at a mass ratio of 1:5 and stirred and mixed for 12 h to obtain product B; the obtained product B was subjected to microwave reaction under argon atmosphere, with a microwave frequency of 1000 W, a microwave duty cycle of 1, and a microwave time of 2 min.
[0042] Example 5
[0043] At room temperature, 4 g of sulfonated coal (ZG-S77) and a solution containing 0.4 g of ferric nitrate were stirred and mixed for 24 h, then filtered and dried at 100 ° C for 8 h to obtain product A. Product A and organic reagent aniline were taken at a mass ratio of 1:10, and the two were stirred and mixed for 24 h to obtain product B; the obtained product B was subjected to microwave reaction under a nitrogen and argon mixed atmosphere, with a microwave frequency of 800 W, a microwave duty cycle of 0.1, and a microwave time of 20 min.
[0044] Example 6
[0045] At room temperature, 4 g of sulfonated coal (ZG-S77) and a solution containing 40 g of ferric nitrate were stirred and mixed for 6 h, then filtered and dried at 80 ° C for 24 h to obtain product A. Product A and organic reagent pyrrole were taken at a mass ratio of 1:5, and the two were stirred and mixed for 2 h to obtain product B; the obtained product B was subjected to microwave reaction under argon atmosphere, with a microwave frequency of 600 W, a microwave duty cycle of 0.8, and a microwave time of 10 min.
[0046] Example 7
[0047] At room temperature, 5 g of sulfonated lignite (SMC) and a solution containing 1 g of ferric chloride were stirred and mixed for 8 h, then filtered and dried at 120°C for 24 h to obtain product A. Product A and an organic reagent pyrrole were taken at a mass ratio of 1:1 and stirred and mixed for 20 h to obtain product B; the obtained product B was subjected to microwave reaction under a nitrogen and argon mixed atmosphere, with a microwave frequency of 400 W, a microwave duty cycle of 0.4, and a microwave time of 50 min.
[0048] Example 8
[0049] The FeS@C composite material prepared in Example 2 was used as an electrode material active material in an energy storage battery. The working electrode was a copper foil electrode sheet with a diameter of 14 mm attached with active material, conductive agent acetylene black and binder polyvinylidene fluoride (mass ratio = 7:2:1). The assembly of the half-cell was carried out in a glove box filled with argon and with water and oxygen content less than 0.1 ppm. A metal lithium sheet was used as the counter electrode, a Celgard2400 polypropylene PP film was used as a diaphragm, and a 10 wt% FEC ethylene carbonate (EC): diethyl carbonate (DEC) = 1:1 vol.% 1M LiPF6 mixed solution was added as the electrolyte to assemble a half-cell with a battery model of CR2016. The assembled battery was placed in a constant temperature incubator at 25°C for 12 hours before the electrochemical performance test was carried out.
[0050] The lithium ion button battery prepared in this example was tested for charge and discharge at current densities of 0.1A / g, 0.2A / g, 0.5A / g, 1A / g, 2A / g, 3A / g, 5A / g and 0.1A / g at 0.1-3V. The charge and discharge specific capacities of the lithium ion battery prepared in this example at different current densities are shown in FIG. Figure 3 As shown by Figure 3 It can be seen that the battery capacity can reach 196.3mAh / g at a high current density of 5A / g.
Claims
1. A method for rapidly preparing FeS@C composite materials by microwave method, characterized in that: The following steps are involved: A strongly acidic cation exchange resin, sulfonated coal or sulfonated asphalt is added to a solution containing trivalent iron ions, stirred and mixed for a period of time, filtered and dried to obtain an iron exchange complex, which is added to an organic reagent, stirred and mixed for a period of time, and the obtained solid product is subjected to microwave reaction for a period of time under an inert gas atmosphere to obtain a final product; The solution containing trivalent iron ions is one of ferric chloride solution, ferric sulfate solution and ferric nitrate solution or a mixture of two or more thereof; the organic reagent is one of pyrrole and aniline or a mixture of two or more thereof.
2. The method according to claim 1, characterized in that The mass ratio of the strong acid cation exchange resin, sulfonated coal or sulfonated asphalt to the trivalent iron salt is 10:1-100, and the stirring and mixing time of the strong acid cation exchange resin, sulfonated coal or sulfonated asphalt in the trivalent iron ion solution is 0.5-24 hours; the drying conditions are: drying at 60-120°C for 8-24 hours; the mass ratio of the iron-exchanged complex to the organic reagent is: 1:1-10; the stirring and mixing time of the iron-exchanged complex in the organic reagent is: 2-24 hours.
3. The method according to claim 1 or 2, characterized in that: The inert gas is one of nitrogen and argon or a mixture of the two; the microwave frequency is 100-1000W; the microwave duty cycle is 0.1-1; and the microwave reaction time is 2-60min.
4. FeS@C composite material rapidly prepared by microwave method, characterized in that: The FeS@C composite material rapidly prepared by microwave method is prepared by the method described in any one of claims 1-3.
5. Use of the FeS@C composite material rapidly prepared by microwave method as claimed in claim 4 in the preparation of lithium ion batteries and sodium ion batteries.