A rinsing and drying process and a crushing and drying device for electrolytic manganese dioxide powder

By combining hot water rinsing, powder alkali washing, and acid washing processes with cyclone drying technology, the problem of sulfate and calcium and magnesium residues in electrolytic manganese dioxide was solved. Furthermore, the material conveying difficulties were resolved through a twin-screw feeder and a crushing system, thus achieving the production of high-purity and high-efficiency electrolytic manganese dioxide.

CN114634207BActive Publication Date: 2024-11-15GUANG XI XIA TIAN MENG KUANG YOU XIAN ZE REN GONG SI +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202210277298.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-17
Publication Date
2024-11-15
Estimated Expiration
2042-03-17

AI Technical Summary

Technical Problem

In the existing electrolytic manganese dioxide production process, the residual sulfate and calcium and magnesium substances are too high, which leads to a decrease in battery performance. In addition, the filter cake after powder washing is very sticky and easily sticks to the conveying equipment, causing conveying difficulties.

Method used

The process combines hot water rinsing, powder alkali washing, and powder acid washing with cyclone drying technology to remove sulfate and calcium and magnesium impurities through multiple rinsing and acid washing. A twin-screw feeder and crushing system are used to prevent material sticking.

Benefits of technology

It improves the purity and particle size distribution uniformity of electrolytic manganese dioxide, reduces production costs and energy consumption, solves the problem of difficult transportation, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114634207B_ABST
    Figure CN114634207B_ABST
Patent Text Reader

Abstract

The invention relates to the field of electrolytic manganese dioxide production, and specifically discloses a rinsing and drying process for electrolytic manganese dioxide powder, including: hot water acid washing, grinding, powder alkali washing, acid washing, water washing, filter pressing and drying, iron removal and other steps, and discloses an electrolytic manganese dioxide powder crushing and drying device, including: a drying cylinder with an air inlet and an air outlet, a crushing system with a crushing rotor, a feeder with a twin screw and a sealing disc assembly. The present invention uses hot water to rinse the manganese dioxide fragments multiple times and powder alkali washing to remove sulfate on the surface and inside of the manganese dioxide, and then uses powder acid washing to remove calcium and magnesium substances in the manganese dioxide powder, thereby improving the purity of the manganese dioxide; and the twin screw structure of the feeder in the electrolytic manganese dioxide powder crushing and drying device can ensure that the material is prevented from sticking during the material transportation process, and the phenomenon of holding the rod occurs, and the material can be crushed by the crushing system, thereby improving the drying effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electrolytic manganese dioxide production, and particularly relates to an electrolytic manganese dioxide powder rinsing and drying process and a crushing and drying device. Background Art

[0002] Electrolytic manganese dioxide (EMD) is the positive active material of the battery, directly participating in the discharge reaction of the battery, and is a key material for manufacturing batteries. The mercury-free battery has put forward higher and higher requirements for electrolytic manganese dioxide. As a special electrolytic manganese dioxide for lithium manganate, it must have high chemical purity and very strict requirements on the content of heavy metal impurities such as iron, copper, cobalt, nickel, lead, potassium, arsenic, etc., and it is required to have low sulfate, high chemical purity, and excellent physical properties. The finished product processing of electrolytic manganese dioxide includes grinding, rinsing, drying, mixing and other processes. The operation of finished product processing is directly related to the pH value, fineness and particle size distribution, impurity content and other important parameters of the product.

[0003] The existing technology for the finished product processing of electrolytic manganese dioxide has undergone several generations of technical iterations in the rinsing and drying methods. How to dry the powder after rinsing has become a key technology in the post-processing of the finished electrolytic manganese dioxide.

[0004] The first generation of powder washing and drying process has been eliminated because it relies on sunny weather and solar energy for drying, which is prone to environmental pollution, has high labor intensity for operators, and has a high iron content in the product.

[0005] The second generation of powder washing and drying process is the steam drying method. Although it does not rely on weather for production, it is eliminated again because it requires manual use of iron shovels to turn the powder on the drying bed. The labor intensity is high, the product has a high iron content, and the working environment is poor.

[0006] The third generation of converter drying technology places the electrolytic manganese dioxide filter cake after powder rinsing into a continuously rotating drying furnace and passes hot air into the drying furnace to dry the product. Although this can solve the problem of high labor intensity, the filter cake is in a paste-like state with high viscosity, sticks to the inner wall of the converter, is difficult to clean, has low production efficiency, and the moisture content of the product is difficult to control and has a high iron content, so it was eliminated again. Therefore, the fourth generation of particle rinsing and drying-free technology came into being.

[0007] The fourth generation of particle rinsing, after three-stage rinsing of hot water washing-alkali washing-hot water washing, uses the temperature of hot water to evaporate the water on the surface of the electrolytic manganese dioxide particles naturally, and can be directly ground without drying, and the finished product can be obtained after magnetization iron removal and mixing. Although this method omits the drying process, since the electrolytic manganese dioxide crude product particles are rinsed, only impurities such as sulfate remaining on the surface of the particles can be neutralized and removed, and impurities such as sulfate remaining inside the particles cannot be completely removed, resulting in a high amount of residual sulfate in the electrolytic manganese dioxide. In addition, in the existing process, during the preparation of manganese sulfate solution, calcium and magnesium ions enter the manganese sulfate solution with the acid decomposition of the raw materials and calcium and magnesium ions introduced by using stone powder as a neutralizer, so that the calcium and magnesium ion content of the manganese sulfate solution is high and difficult to remove, so that more calcium and magnesium substances remain in the electrolytic manganese dioxide, affecting the capacity and cycle performance of the battery.

[0008] In order to overcome the shortcomings of the prior art, the present invention improves the technology of the electrolytic manganese dioxide rinsing and drying process, adopts powder rinsing and cyclone drying technology to solve the problem of high residual sulfate and calcium and magnesium substances in the electrolytic manganese dioxide and insufficient purity in the traditional process, and solves the problem that the filter cake after powder rinsing is sticky and easily adheres to the spiral shaft, and is adhered to the spiral to form a "holding rod", causing transportation difficulties, and the wet material cannot enter the dryer for drying, so as to produce high-performance lithium manganese oxide type electrolytic manganese dioxide, and has the characteristics of low cost and low energy consumption, and is suitable for large-scale industrial production.

[0009] The disclosure of the above background technology content is only used to assist in understanding the inventive concept and technical solution of the present invention. It does not necessarily belong to the prior art of this patent application. In the absence of clear evidence that the above content has been disclosed on the filing date of this patent application, the above background technology should not be used to evaluate the novelty and creativity of the present application. Summary of the invention

[0010] The object of the present invention is to provide a rinsing and drying process for electrolytic manganese dioxide powder, so as to overcome the defects of the conventional process in which the electrolytic manganese dioxide contains high residual sulfate, calcium and magnesium impurities and has low purity.

[0011] Another object of the present invention is to provide an electrolytic manganese dioxide powder crushing and drying device, so as to overcome the defect that the existing dryer is prone to produce holding rods when transporting filter cakes, causing transportation difficulties.

[0012] To achieve the above object, the present invention provides a rinsing and drying process for electrolytic manganese dioxide powder, comprising the following steps:

[0013] S1. Hot water acid washing: Place the coarse electrolytic manganese dioxide product fragments stripped from the anode of the electrolytic cell of the automatic stripping machine into a rinsing bucket, inject 65℃-75℃ hot water into the rinsing bucket, and continue to heat it to 95℃-100℃. After multiple rinses, until SO4 2- The content is less than 1%;

[0014] S2, grinding: grinding the electrolytic manganese dioxide fragments rinsed in step S1, controlling the particle size to be more than 95% passing through a 325-mesh sieve, and adjusting the fan pressure and the classifier speed to control the particle size distribution of the electrolytic manganese dioxide to be within the range of D10 (3.5-4.5), D50 (16-18), and D90 (33-37);

[0015] S3, powder alkali washing: pump 65℃-75℃ hot water into the powder washing barrel, add the manganese dioxide powder ground in step S2 into the powder washing barrel, continue to heat up to 95℃-100℃, add sodium hydroxide solution, stir, and neutralize. Stop the reaction when the pH value reaches 7-8; let it stand to allow the manganese dioxide powder to precipitate, and discharge the upper clarified liquid. The discharged liquid can be recycled and reused;

[0016] S4, powder pickling: add the prepared acetic acid solution with a concentration of about 3% into the above powder washing bucket, stir with the manganese dioxide powder slurry obtained in step S3, react for 1 hour, and control the temperature at 90 o C-100 o C dissolves the calcium, magnesium and other substances remaining in the manganese dioxide powder;

[0017] S5, filter pressing: performing solid-liquid separation on the manganese dioxide slurry obtained in step S4;

[0018] S6, washing, washing the filter cake obtained in S5 with water, and controlling the temperature at 70 o C-80 o C. Stir for 30 min, wash with water 2-3 times, and adjust the pH value to 6.5-7;

[0019] S7, filter pressing and drying: the rinsed electrolytic manganese dioxide slurry is pumped into the filter press for solid-liquid separation, so that the moisture content of the filter cake is 15%-19%, the filtrate is used for recycling, and the filter cake is transported to the horizontal crushing type airflow dryer through a belt conveyor for crushing and drying;

[0020] S8, iron removal: the electrolytic manganese dioxide powder after crushing and drying is transported to the iron remover through the dense phase conveying system for magnetic iron removal;

[0021] S9. Discharging: After the products are mixed evenly by gravity mixing bin, pure electrolytic manganese dioxide finished products are finally obtained.

[0022] Preferably, in the above technical solution, the coarse electrolytic manganese dioxide product fragments in step S1 need to be rinsed twice, the first rinsing time is 1 hour, and the second rinsing time is 2 hours.

[0023] Preferably, in the above technical solution, in step S3, the neutralization reaction time is 0.5h.

[0024] On the other hand, to achieve the above-mentioned purpose, the present invention provides an electrolytic manganese dioxide powder crushing and drying device, comprising: a drying cylinder, one end of which is provided with an air inlet, and the other end of which is provided with an air outlet; a crushing system, which is arranged at the other end of the drying cylinder, and a rotatable crushing rotor is arranged in the crushing system, and a plurality of rake teeth are arranged around the circumference of the crushing rotor; a feeder, which comprises a feeding cabin, and the feeding cabin comprises a loading port and a unloading port, and the unloading port is connected to one end of the drying cylinder, and two rotatable screws are arranged between the loading port and the unloading port, and the two screws are arranged in parallel with a certain interval and can rotate in opposite directions, and the rotation directions of the two screws are opposite.

[0025] Preferably, in the above technical solution, a rotating shaft is respectively provided at both ends of the crushing rotor, the ends of the rotating shaft respectively pass through both sides of the drying cylinder and are fixed by a bracket, and a sealing disk assembly is provided between the rotating shaft and the drying cylinder.

[0026] Preferably, in the above technical solution, the sealing disc assembly includes: a disc seat, one end of which is fixedly arranged on both sides of the drying cylinder, a seat hole is provided in the disc seat, the rotating shaft passes through the seat hole, and a packing is provided between the seat hole and the rotating shaft; a sealing cover, which is arranged at the other end of the disc seat and presses the packing into the seat hole; a compressed gas pipe, which is arranged on the disc seat and connected with the seat hole, and the compressed gas pipe is used to introduce compressed air.

[0027] Preferably, in the above technical solution, the crushing system further comprises a first motor, and the first motor is connected to the end of one of the rotating shafts through a pulley set.

[0028] Preferably, in the above technical solution, the rake teeth are detachably mounted on the crushing rotor.

[0029] Preferably, in the above technical solution, the outside of the drying cylinder is coated with a thermal insulation layer, and the thermal insulation layer is made of aluminum silicate material.

[0030] Preferably, in the above technical solution, the feeder further includes a second motor, and the second motor is connected to the ends of the two screws through a reduction box.

[0031] Compared with the existing technology, the present invention has the following beneficial effects:

[0032] 1. The electrolytic manganese dioxide powder rinsing and drying process of the present invention uses hot water to rinse the manganese dioxide fragments multiple times and alkali wash the powder to remove sulfate on the surface and inside of the manganese dioxide, and uses powder acid washing to remove calcium and magnesium substances in the manganese dioxide powder, thereby improving the purity of the manganese dioxide; and the twin-screw structure of the feeder in the electrolytic manganese dioxide powder crushing and drying device can ensure that the materials are prevented from sticking and holding the rod during the material transportation process, and the crushing system can break the materials into pieces, thereby improving the drying effect.

[0033] 2. In the electrolytic manganese dioxide powder rinsing and drying process step S2 of the present invention, the particle size distribution of the electrolytic manganese dioxide is controlled within the range of D10 (3.5-4.5), D50 (16-18), and D90 (33-37) by adjusting the air pressure and speed of the fan. The particle size distribution of the electrolytic manganese dioxide is concentrated, which is conducive to its uniform mixing with lithium carbonate and improves the reaction uniformity in the synthesis process of lithium manganate.

[0034] 3. The electrolytic manganese dioxide powder rinsing and drying process of the present invention adds an S4 powder acid washing step after the powder alkali washing, so that the insoluble manganese sulfate and magnesium sulfate mixed in the electrolytic manganese dioxide product react with sodium hydroxide to generate calcium hydroxide and magnesium hydroxide, and then add acetic acid in a weakly alkaline environment to make them soluble substances, which can be separated from the manganese dioxide solid powder through the subsequent filter pressing and water washing steps.

[0035] 4. In step S1 of the electrolytic manganese dioxide powder rinsing and drying process of the present invention, the sulfate on the surface of the coarse manganese dioxide product particles can be dissolved and washed away by two rinses, and in order to ensure the dissolution amount of the sulfate, the rinsing time is gradually increased; in step S3, the powder alkaline washing step, the sulfate inside the manganese dioxide can be neutralized by sodium hydroxide solution, so that the sulfate can be removed more thoroughly, thereby improving the removal effect of the sulfate.

[0036] 5. The rake teeth in the crushing rotor of the crushing system of the electrolytic manganese dioxide powder crushing and drying device of the present invention are made of GCr15 bearing steel material, which has the characteristics of high strength and high wear resistance, can improve the durability and fatigue resistance of the crushing rotor, and the rake teeth can also be easily disassembled, which can reduce the production cost of the equipment while ensuring the overall strength and durability of the crushing rotor.

[0037] 6. The two ends of the crushing rotor in the electrolytic manganese dioxide powder crushing and drying device of the present invention are connected to the side wall of the drying cylinder through a rotating shaft, and are sealed at the connection by a sealing disk assembly. A packing for sealing the rotating shaft is arranged in the seat hole of the sealing disk assembly, and compressed air is introduced into the seat hole from the outside to prevent the manganese dioxide powder from leaking from the sealing disk assembly.

[0038] 7. The feeder in the electrolytic manganese dioxide powder crushing and drying device of the present invention is provided with two parallel screws and the blades in the two screws rotate in opposite directions. When conveying materials, the two screws rotate in opposite directions, and the materials adhered to the blades can be squeezed and removed while conveying the materials, thereby preventing the materials from adhering to the blades and preventing the occurrence of the phenomenon of holding the rod.

[0039] 8. The blade surface of the screw in the feeder and the inner wall of the drying cylinder in the electrolytic manganese dioxide powder crushing and drying device of the present invention are sprayed with 0.8mm thick ceramic material, which can prevent the iron ions in the carbon steel from entering the product and ensure that the iron increment in the product is less than 10ppm.

[0040] 9. The outside of the drying cylinder of the electrolytic manganese dioxide powder crushing and drying device in the present invention is coated with a 50 mm thick insulation layer, the material of the insulation layer is aluminum silicate wool, which can insulate the drying cylinder and reduce energy consumption and loss. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 It is a process flow chart of the electrolytic manganese dioxide powder rinsing and drying process in Example 1.

[0042] Figure 2 It is a cross-sectional view of the electrolytic manganese dioxide powder crushing and drying device in the second embodiment in the front viewing direction.

[0043] Figure 3 It is a top view of the electrolytic manganese dioxide powder crushing and drying device in Example 2.

[0044] Figure 4 It is a partial enlarged view of the crushing system in the second embodiment.

[0045] Figure 5 It is a partial enlarged view of the feeder in the second embodiment.

[0046] Description of main reference numerals:

[0047] 1-drying cylinder, 11-air inlet, 12-air outlet, 13-insulation layer;

[0048] 2-crushing system, 21-crushing rotor, 22-rake teeth, 23-rotating shaft, 24-bracket, 25-first motor, 26-pulley group;

[0049] 3-feeder, 31-feeding chamber, 32-loading port, 33-unloading port, 34-screw, 35-second motor, 36-reduction box;

[0050] 4-sealing disc assembly, 41-disc seat, 42-seat hole, 43-sealing cover, 44-compressed gas pipe, 45-packing. DETAILED DESCRIPTION

[0051] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0052] In the description of the present invention, it should be noted that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "top", "bottom", "top surface", "bottom surface", "inside", "outside", "inside", "outside" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention.

[0053] In the description of the present invention, "several" means one or more, "more" means more than two, "greater than", "less than", "exceed" etc. are understood to exclude the number itself, and "above", "below", "within" etc. are understood to include the number itself. If the terms "first", "second", "third" are described, they are only used for the purpose of description and distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.

[0054] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", and "set" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal connection of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances. The following is an explanation of the embodiments of the present invention based on its overall structure.

[0055] Embodiment 1:

[0056] like Figure 1 As shown, the electrolytic manganese dioxide powder rinsing and drying process in this embodiment includes the following steps:

[0057] S1. Hot water acid washing: Place the coarse electrolytic manganese dioxide product fragments (about 5-40mm in size) stripped from the anode of the electrolytic cell of the automatic stripping machine into a rinsing bucket, inject 70℃ hot water into the rinsing bucket, and continue to heat it to 95℃-100℃. Rinse twice, the first rinse for 1h, the second rinse for 2h, until SO4 2- The content is less than 1%;

[0058] S2, grinding: grinding the electrolytic manganese dioxide fragments rinsed in step S1, controlling the particle size to be more than 95% passing through a 325-mesh sieve, and adjusting the fan pressure and the classifier speed to control the particle size distribution of the electrolytic manganese dioxide to be within the range of D10 (3.5-4.5), D50 (16-18), and D90 (33-37);

[0059] S3, powder alkali washing: pump 70℃ hot water into the powder washing barrel, put the ground manganese dioxide powder into the powder washing barrel, continue to heat up to 95℃-100℃, add sodium hydroxide solution, stir, neutralize, stop the reaction when the pH value reaches 7-8; let it stand to allow the manganese dioxide powder to precipitate, discharge the upper clarified liquid, and the discharged liquid can be recycled and reused;

[0060] S4, powder pickling: add the prepared acetic acid solution with a concentration of about 3% into the above powder washing bucket, stir with the manganese dioxide powder slurry obtained in step S3, react for 1 hour, and control the temperature at 90 o C-100 o C dissolves the calcium, magnesium and other substances remaining in the manganese dioxide powder;

[0061] S5, filter pressing: performing solid-liquid separation on the manganese dioxide slurry obtained in step S4;

[0062] S6, washing, washing the filter cake obtained in S5 with water, and controlling the temperature at 70o C-80 o C. Stir for 30 min, wash with water 2-3 times, and adjust the pH value to 6.5-7;

[0063] S7, filter pressing and drying: the rinsed electrolytic manganese dioxide slurry is pumped into the filter press for solid-liquid separation, so that the moisture content of the filter cake is 17%, the filtrate is used for recycling, and the filter cake is transported to the horizontal crushing type airflow dryer by a belt conveyor for crushing and drying;

[0064] S8, iron removal: the electrolytic manganese dioxide powder after crushing and drying is transported to the iron remover through the dense phase conveying system for magnetic iron removal;

[0065] S9, discharging: After the products are mixed evenly by gravity mixing bin, pure lithium manganese oxide type electrolytic manganese dioxide finished product is finally obtained.

[0066] Embodiment 2:

[0067] like Figures 2 to 5 As shown, the electrolytic manganese dioxide powder crushing and drying device in this embodiment includes: a drying cylinder 1, an air inlet 11, an air outlet 12, an insulation layer 13, a crushing system 2, a crushing rotor 21, rake teeth 22, a rotating shaft 23, a bracket 24, a first motor 25, a pulley group 26, a feeder 3, a feeding cabin 31, a loading port 32, a unloading port 33, a screw 34, a second motor 35, a reduction box 36, a sealing disc assembly 4, a disc seat 41, a seat hole 42, a sealing cover 43, and a compressed gas pipe 44.

[0068] The drying cylinder 1 is a cylindrical barrel, and the inner wall of the drying cylinder 1 is made of 4mm carbon steel plate. The cylinder of the drying cylinder 1 is assembled end to end by 9 sections of monomers. Both ends of each section of the monomer are connected by flange surfaces and bolts. A 4mm neoprene coating is provided on the inner surface of the drying cylinder 1. An air inlet 11 is opened on the side of one end of the drying cylinder 1, and an air outlet 12 is opened on the side of the other end of the drying cylinder 1.

[0069] The crushing system 2 is installed at the other end of the drying cylinder 1 and is located at a position corresponding to the air outlet 12. A rotatable crushing rotor 21 is provided in the crushing system 2. A plurality of rake teeth 22 are installed around the crushing rotor 21. A rotating shaft 23 is provided at each end of the crushing rotor 21. The ends of the rotating shaft 23 pass through the two sides of the drying cylinder 1 and are installed on the bracket 24 through the rolling bearing seat. A sealing disk assembly 4 is installed between the rotating shaft 23 and the drying cylinder 1. The sealing disk assembly 4 includes: a disk seat 41, a sealing cover 43 and compressed gas pipe 44; one end of the disc seat 41 is fixedly mounted on both sides of the drying cylinder 1, a seat hole 42 is opened in the disc seat 41, the rotating shaft 23 passes through the seat hole 42, and a packing 45 is installed between the seat hole 42 and the rotating shaft 23; the sealing cover 43 is installed at the other end of the disc seat 41 by screws, so that the disc seat 41 presses the packing 45 in the seat hole 42, thereby sealing the packing 45 between the rotating shaft 23 and the seat hole 42; one end of the compressed gas pipe 44 is installed on the disc seat 41 and communicates with the seat hole 42, and the compressed gas The other end of the tube 44 is interconnected with compressed air, and the compressed gas tube 44 is used to introduce compressed air into the seat hole 42, so as to prevent the manganese dioxide powder from leaking from the gap between the rotating shaft 23 and the seat hole 42; the rake teeth 22 are made of GCr15 material, and the rake teeth 22 are detachably mounted on the crushing rotor 21 by bolts, and the distance between the rake teeth 22 and the inner cylinder is 5mm. When the material falls to the position of the rake teeth 22, it is crushed by the high-speed rotating rake teeth. The crushed material is carried by hot air into the drying cylinder for drying, and the small particles that meet the drying requirements enter the subsequent process section, and the large particles continue to rotate and dry in the cylinder; the crushing system 2 also includes a first motor 25 installed on the ground, and the output end of the first motor 25 is connected to the end of one of the rotating shafts 23 through a pulley group 26, which is used to drive the crushing rotor 21 to rotate; the outside of the drying cylinder 1 is coated with an insulation layer 13, and the insulation 13 is made of aluminum silicate wool material with a thickness of 50mm, which can not only play the function of fire prevention and heat preservation, but also play the function of sound insulation.

[0070] The feeder 3 includes a feeding cabin 31, which is a horizontal cylindrical structure. The feeding cabin 31 includes an upper feeding port 32 and a lower feeding port 33. The lower feeding port 33 is connected to one end of the drying cylinder 1. Two rotatable screws 34 are installed between the upper feeding port 32 and the lower feeding port 33. The two screws 34 are arranged in parallel at a certain interval and can rotate in opposite directions. The rotation directions of the blades of the two screws 34 are opposite, and the blades of the two screws 34 are interlaced with each other. The feeder 3 also includes a second motor 35, which is connected to the ends of the two screws 34 through a reduction box 36. The second motor 35 is coaxially connected to the input end of the reduction box 36. The reduction box 36 has two output ends, and the two output ends are coaxially connected to the ends of the two screws 34 respectively. A pair of mutually meshing transmission gears are respectively arranged between the two output ends.

[0071] The screw 34 and the inner wall of the drying cylinder 1 are sprayed with 0.8 mm ceramic to prevent the iron ions in the carbon steel used to manufacture the device from entering the product, ensuring that the iron increase in the product is less than 10 ppm.

[0072] Next, the working principle of an electrolytic manganese dioxide powder crushing and drying device in this embodiment is described in detail so that those skilled in the art can better understand the technical solution in this embodiment.

[0073] When in use, the manganese dioxide wet material with a water content of about 17% and a temperature of 20°C is sent to the charging cabin 31 through the feeding port 32 through the previous process, and the material is evenly transported to the crushing system 2 through the opposite rotation of the two screws 34. The blower sends hot air (about 220°C) into the drying cylinder 1 from the air inlet 11; the manganese dioxide wet material entering the drying cylinder 1 is quickly broken up by the rake teeth 22 of the crushing rotor 21; the crushed material is carried by the hot air into the drying cylinder for drying, and the small particles that meet the drying requirements enter the subsequent process stage, and the large particles continue to rotate and dry in the cylinder.

[0074] In summary, the electrolytic manganese dioxide powder rinsing and drying process of the present invention removes sulfate on the surface and inside of the manganese dioxide by multiple rinsing of the manganese dioxide fragments with hot water and powder alkali washing, and removes calcium and magnesium substances in the manganese dioxide powder by powder acid washing, thereby improving the purity of the manganese dioxide; and the twin-screw structure of the feeder in the electrolytic manganese dioxide powder crushing and drying device can ensure that the material is prevented from sticking and holding the rod during the material transportation process, and the material can be broken up by the crushing system, thereby improving the drying effect.

[0075] The foregoing descriptions of specific exemplary embodiments of the present invention are for the purpose of explanation and illustration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is obvious that many changes and variations can be made based on the above teachings. Although an embodiment of the present invention has been shown and described, this specific embodiment is only an explanation of the present invention and is not a limitation of the invention. The specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments or examples. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can make modifications, substitutions, variations and various selections and changes to the embodiments without creative contribution as needed without departing from the principles and purpose of the present invention after reading this specification, but they are protected by patent law as long as they are within the scope of the claims of the present invention.

Claims

1. An electrolytic manganese dioxide powder crushing and drying device, characterized in that: include: A drying cylinder (1), wherein one end of the drying cylinder (1) is provided with an air inlet (11), and the other end of the drying cylinder (1) is provided with an air outlet (12); A crushing system (2) is arranged at the other end of the drying cylinder (1), wherein a rotatable crushing rotor (21) is arranged in the crushing system (2), and a plurality of rake teeth (22) are arranged around the crushing rotor (21); A feeder (3), comprising a feed chamber (31), the feed chamber (31) comprising an upper feed port (32) and a lower feed port (33), the lower feed port (33) being connected to one end of the drying cylinder (1), two rotatable screws (34) being arranged between the upper feed port (32) and the lower feed port (33), the two screws (34) being arranged in parallel at a certain interval and being capable of rotating in opposite directions, and the two screws (34) rotating in opposite directions; A rotating shaft (23) is respectively provided at both ends of the crushing rotor (21), the ends of the rotating shaft (23) respectively pass through both sides of the drying cylinder (1) and are fixed by a bracket (24), and a sealing disc assembly (4) is provided between the rotating shaft (23) and the drying cylinder (1); The rake teeth (22) are detachably mounted on the crushing rotor (21).

2. The electrolytic manganese dioxide powder crushing and drying device according to claim 1, characterized in that: The sealing disc assembly (4) comprises: a disc seat (41), one end of the disc seat (41) being fixedly arranged on both sides of the drying cylinder (1), a seat hole (42) being arranged in the disc seat (41), the rotating shaft (23) passing through the seat hole (42), and a packing (45) being arranged between the seat hole (42) and the rotating shaft (23); A sealing cover (43) is arranged at the other end of the packing seat (41) to press the packing (45) into the seat hole (42); A compressed gas pipe (44) is arranged on the disc seat (41) and is connected to the seat hole (42). The compressed gas pipe (44) is used to introduce compressed air.

3. The electrolytic manganese dioxide powder crushing and drying device according to claim 1, characterized in that: The crushing system (2) further comprises a first motor (25), wherein the first motor (25) is connected to the end of one of the rotating shafts (23) via a pulley set (26).

4. The electrolytic manganese dioxide powder crushing and drying device according to claim 1, characterized in that: The outside of the drying cylinder (1) is coated with a heat-insulating layer (13), and the heat-insulating layer (13) is made of aluminum silicate material.

5. The electrolytic manganese dioxide powder crushing and drying device according to claim 1, characterized in that: The feeder (3) further comprises a second motor (35), and the second motor (35) is connected to the ends of the two screws (34) via a reduction box (36).

6. A process for rinsing and drying electrolytic manganese dioxide powder, using the electrolytic manganese dioxide powder crushing and drying device according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Hot water acid washing: Place the coarse electrolytic manganese dioxide product fragments stripped from the anode of the electrolytic cell of the automatic stripping machine into a rinsing bucket, inject 65℃-75℃ hot water into the rinsing bucket, and continue to heat it to 95℃-100℃. After multiple rinses, until SO4 2- The content is less than 1%; S2, grinding: grinding the electrolytic manganese dioxide fragments rinsed in step S1, controlling the particle size to pass through a 325-mesh sieve of more than 95%, and adjusting the fan pressure and the classifier speed to control the particle size distribution of the electrolytic manganese dioxide to D10 of 3.5-4.5, D50 of 16-18, and D90 of 33-37; S3, powder alkali washing: pump 65℃-75℃ hot water into the powder washing barrel, add the manganese dioxide powder ground in step S2 into the powder washing barrel, continue to heat up to 95℃-100℃, add sodium hydroxide solution, stir, and neutralize. Stop the reaction when the pH value reaches 7-8; let it stand to allow the manganese dioxide powder to precipitate, discharge the upper clarified liquid, and recycle the discharged liquid for reuse; S4, powder pickling: add the prepared 3% acetic acid solution into the powder washing bucket, stir with the manganese dioxide powder slurry obtained in step S3, react for 1 hour, and control the temperature at 90°C-100°C to dissolve the calcium and magnesium substances remaining in the manganese dioxide powder; S5, filter pressing: performing solid-liquid separation on the manganese dioxide slurry obtained in step S4; S6, washing with water, washing the filter cake obtained in S5 with water, controlling the temperature at 70°C-80°C and stirring for 30 minutes, after 2-3 washings with water, adjusting the pH value to 6.5-7; S7, filter pressing and drying: the rinsed electrolytic manganese dioxide slurry is pumped into the filter press for solid-liquid separation, so that the moisture content of the filter cake is 15%-19%, the filtrate is used for recycling, and the filter cake is transported to the horizontal crushing type air flow dryer by a belt conveyor for crushing and drying; S8, iron removal: the electrolytic manganese dioxide powder after crushing and drying is transported to the iron remover through the dense phase conveying system for magnetic iron removal; S9. Discharging: After the products are mixed evenly by gravity mixing bin, pure electrolytic manganese dioxide finished products are finally obtained.

7. The electrolytic manganese dioxide powder rinsing and drying process according to claim 6, characterized in that: The crude electrolytic manganese dioxide product fragments in step S1 need to be rinsed twice, the first rinsing time is 1 hour, and the second rinsing time is 2 hours.

8. The electrolytic manganese dioxide powder rinsing and drying process according to claim 6, characterized in that: In step S3, the neutralization reaction time is 0.5 h.

Citation Information

Cited By

  • Rinsing process for improving product recovery rate

    CN121696157A