Cutting tool and processing method thereof

By forming a self-lubricating layer of tungsten disulfide and carbon on the surface of the tool, combined with the film layer technology of sputter deposition, the problem of poor wear resistance of the tool is solved, achieving longer service life and better cutting performance.

CN114686824BActive Publication Date: 2024-10-22WUHAN SUPOR COOKWARE
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202011579186.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-28
Publication Date
2024-10-22
Estimated Expiration
2040-12-28

AI Technical Summary

Technical Problem

Knives used daily are prone to wear and scratches when cutting foods with different hardnesses, resulting in poor wear resistance and affecting service life and reliability.

Method used

A self-lubricating layer including tungsten disulfide and carbon is used to cover the surface of the cutter body. The first film layer and the second film layer are formed by sputtering deposition method to improve the bonding, extend the service life of the self-lubricating layer, and improve it through carbon Antioxidant properties and hardness.

Benefits of technology

Significantly improves the wear resistance and service life of the tool, maintains the integrity of the blade and cutting performance, reduces the friction coefficient, and prevents coating shedding and oxidation failure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114686824B_ABST
    Figure CN114686824B_ABST
Patent Text Reader

Abstract

The present application provides a tool and a processing method thereof, wherein the tool comprises a tool body, a transition layer and a self-lubricating layer; the transition layer covers the surface of the tool body; the self-lubricating layer covers the surface of the transition layer, and the components of the self-lubricating layer include tungsten disulfide and carbon. The present application can improve the wear resistance of the tool and extend the service life of the tool.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of kitchen utensils, and in particular to a knife and a processing method thereof. Background Art

[0002] The knives commonly used in daily life are mainly made of martensitic stainless steel, which has high strength, hardness and corrosion resistance, but slightly poor wear resistance. During long-term use in a home environment, the cutting edge frequently cuts various foods of different hardness, which is prone to wear, scratches and other adverse phenomena, thus affecting the service life of the knife and having a negative impact on the reliability and appearance of the knife. Summary of the invention

[0003] The present application provides a tool and a processing method thereof to improve the wear resistance of the tool and extend the service life of the tool.

[0004] A first aspect of the present application provides a tool, comprising:

[0005] Knife body;

[0006] A transition layer covering the surface of the blade body;

[0007] The self-lubricating layer covers the surface of the transition layer, and the components of the self-lubricating layer include tungsten disulfide and carbon.

[0008] The above-mentioned tool includes a tool body, a transition layer and a self-lubricating layer; the transition layer covers the surface of the tool body to improve the bonding of the tool body surface and prevent other coatings on the tool body surface from falling off; the self-lubricating layer covers the surface of the transition layer, and the components of the self-lubricating layer include tungsten disulfide and carbon. Both tungsten disulfide and carbon have low friction coefficients, especially tungsten disulfide, the dynamic friction coefficient of which is 0.030, and the static friction coefficient of which is 0.070. It has excellent lubricity and is easy to dissociate, and thus has good wear resistance and self-lubricating effects, thereby effectively improving the wear resistance of the tool surface and extending the service life of the tool. Among them, tungsten disulfide is a layered two-dimensional material with a hexagonal crystal system. Tungsten and sulfur are bonded by strong covalent bonds within the tungsten disulfide layer, and sulfur and sulfur molecular bonds are bonded by weak van der Waals forces between layers. The interlayer force is weak and the bond energy is low. It is very easy to displace during friction, so it has a low friction coefficient. In addition, tungsten disulfide can be adsorbed and filled on the uneven surface of the material in time, playing a certain self-repairing role, so that the blade can maintain lasting integrity; carbon has high stability and can improve the performance of metals. Adding carbon to the self-lubricating layer can improve the oxidation resistance of the self-lubricating layer, prevent the self-lubricating layer from absorbing moisture or oxidizing and failing in a humid environment, and can also increase the hardness of the self-lubricating layer, further improving the wear resistance of the tool.

[0009] Optionally, the transition layer includes a first film layer and a second film layer stacked on each other;

[0010] The first film layer covers the surface of the blade body, the first film layer is a single metal layer, the single metal is a component contained in the blade body, and the mass proportion of the single metal in the blade body is not less than 12%;

[0011] The second film layer covers the surface of the first film layer, and the second film layer is a carbon layer.

[0012] The transition layer of the above-mentioned tool includes a first film layer and a second film layer stacked on each other; the first film layer covers the surface of the tool body, the first film layer is a single metal layer, the single metal is a component contained in the tool body, and the mass proportion of the metal single substance in the tool body is not less than 12%, that is, a metal single substance with a higher content in the tool body is selected to form the first film layer on the surface of the tool body, so that the first film layer and the tool body form a reliable bond; the second film layer covers the surface of the first film layer, the second film layer is a carbon layer, that is, the carbon contained in the self-lubricating layer is selected to form the second film layer, so that the second film layer and the self-lubricating layer form a reliable bond; due to the high bonding between carbon and metal, the first film layer and the second film layer can form a reliable bond, thereby preventing the various coatings on the surface of the tool body from falling off during use.

[0013] Optionally, the knife body is made of martensitic stainless steel and the elemental metal is chromium, so as to ensure that the hardness of the knife meets the use requirements.

[0014] Optionally, the thickness of the first film layer is 1 μm to 1.5 μm to form a continuous and uniform coating, ensuring that the first film layer has high bonding properties and allowing the tool to maintain high toughness.

[0015] Optionally, the thickness of the second film layer is 0.8 μm to 1.2 μm, so as to form a continuous and uniform coating, ensure that the second film layer has high bonding properties, and ensure the structural strength of the second film layer itself.

[0016] Optionally, the thickness of the self-lubricating layer is 2 μm to 3 μm, so that the surface of the tool has a good self-lubricating effect and the tool maintains a high cutting performance.

[0017] Optionally, the friction coefficient of the self-lubricating layer is 0.1-0.2, so that the lubricity of the knife is consistent with the characteristics of the food, so that the knife can meet the cutting requirements of most food.

[0018] Optionally, in the self-lubricating layer, the mass proportion of the carbon is 30% to 40%, so that the friction coefficient of the tool is maintained within a reasonable range.

[0019] A second aspect of the present application provides a tool processing method, which comprises the following steps:

[0020] Step S1: preparing a blade body;

[0021] Step S2: using a sputtering deposition method to sequentially prepare a first film layer, a second film layer and a self-lubricating layer on the surface of the blade body, wherein the self-lubricating layer comprises tungsten disulfide and carbon.

[0022] The tool processing method includes steps S1 and S2, wherein step S1 includes preparing a tool body; step S2 includes using a sputtering deposition method to sequentially prepare a first film layer, a second film layer and a self-lubricating layer on the surface of the tool body, wherein the components of the self-lubricating layer include tungsten disulfide and carbon, so that the tool surface has both high self-lubricating performance and high hardness and stability, thereby preventing the self-lubricating layer from failing and extending the service life of the tool; the first film layer and the second film layer serve as a transition between the tool body and the self-lubricating layer, thereby improving the bonding between the self-lubricating layer and the tool body; and the first film layer, the second film layer and the self-lubricating layer are all formed sequentially by a sputtering deposition method, thereby simplifying the processing technology and reducing production costs, and adjacent film layers have high continuity, thereby improving the bonding between adjacent film layers.

[0023] Optionally, the first film layer is formed by sputtering a chromium target, and the second film layer is formed by sputtering a graphite target.

[0024] Optionally, in the last 3 to 5 minutes of preparing the first film layer, the chromium target is gradually closed and the graphite target is gradually opened, so that the second film layer can penetrate into the surface of the first film layer, forming a smooth transition between the second film layer and the first film layer, further improving the reliable bonding of the second film layer and the first film layer.

[0025] Optionally, the self-lubricating layer is formed by sputtering a graphite target and a tungsten disulfide target simultaneously;

[0026] In the last 3 to 5 minutes of preparing the second film layer, the power of the graphite target is gradually reduced to the set value, and the tungsten disulfide target is gradually turned on to form a smooth transition between the self-lubricating layer and the second film layer, further improving the reliable bonding between the self-lubricating layer and the second film layer.

[0027] It should be understood that the foregoing general description and the following detailed description are exemplary only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 A schematic diagram of the cross-sectional structure of a tool provided in an embodiment of the present application;

[0029] Figure 2 A flowchart of a tool processing method provided in an embodiment of the present application.

[0030] Reference numerals:

[0031] 1- knife body;

[0032] 2- Transition layer;

[0033] 20-first film layer;

[0034] 22- second film layer;

[0035] 3- Self-lubricating layer.

[0036] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0038] In the description of this application, unless otherwise clearly specified and limited, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance; unless otherwise specified or explained, the term "plurality" refers to two or more; the terms "connected" and "fixed" should be understood in a broad sense, for example, "connected" can be a fixed connection, a detachable connection, an integral connection, or an electrical connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0039] In the description of this specification, it should be understood that the directional words such as "upper" and "lower" described in the embodiments of the present application are described at the angles shown in the accompanying drawings and should not be understood as limiting the embodiments of the present application. In addition, in the context, it should also be understood that when it is mentioned that an element is connected to another element "upper" or "lower", it can not only be directly connected to another element "upper" or "lower", but also indirectly connected to another element "upper" or "lower" through an intermediate element.

[0040] like Figure 1As shown, the embodiment of the present application provides a knife, which can be a kitchen knife or a fruit knife, and includes a knife body 1, a transition layer 2 and a self-lubricating layer 3. The knife body 1 can be set into any appropriate shape as needed, and a knife handle can be set at one end of the knife body 1 to facilitate the user to hold the knife; the transition layer 2 covers the surface of the knife body 1 to improve the bonding of the surface of the knife body 1 and prevent other coatings on the surface of the knife body 1 from falling off; the self-lubricating layer 3 covers the surface of the transition layer 2, and the components of the self-lubricating layer 3 include tungsten disulfide (WS2) and carbon (C), that is, the self-lubricating layer 3 is a film layer formed by uniformly mixing tungsten disulfide and carbon, and both tungsten disulfide and carbon have low friction coefficients, especially the dynamic friction coefficient of tungsten disulfide is 0.030, the static friction coefficient is 0.070, the lubricity is excellent, and it is easy to dissociate, so it has good wear resistance and self-lubricating effects, so that the wear resistance of the tool surface can be effectively improved and the service life of the tool can be extended.

[0041] Among them, tungsten disulfide is a layered two-dimensional material with a hexagonal crystal system. Tungsten and sulfur are bonded by strong covalent bonds within the tungsten disulfide layer, and sulfur and sulfur molecular bonds are bonded by weak van der Waals forces between the layers. The interlayer force is weak and the bond energy is low. It is very easy to displace during the friction process, so it has a low friction coefficient. In addition, tungsten disulfide can be adsorbed and filled on the uneven surface of the material in time, playing a certain self-repairing role, so that the blade can maintain lasting integrity; carbon has high stability and can improve the performance of metals. Adding carbon to the self-lubricating layer 3 can improve the oxidation resistance of the self-lubricating layer 3, prevent the self-lubricating layer 3 from absorbing moisture or oxidizing and failing in a humid environment, and can also improve the hardness of the self-lubricating layer 3, further improve the wear resistance of the tool, and greatly improve the hardness, toughness, wear resistance and self-lubricating properties of the tool surface.

[0042] Specifically, pure tungsten disulfide easily absorbs moisture in a humid environment and undergoes oxidation and deterioration. Knives for cutting food (such as meat, vegetables or fruits, etc.) usually complete cutting in a humid environment. Therefore, after long-term use, the tungsten disulfide on the surface is easy to fail. Adding carbon to tungsten disulfide can improve the performance of tungsten disulfide and prevent tungsten disulfide from failing. The hardness of the pure tungsten disulfide film layer is 270HV~280HV, and the friction coefficient of the film layer (i.e., self-lubricating layer 3) formed after adding carbon to tungsten disulfide is improved, but it can still meet the lubrication requirements when cutting food, and the hardness can be significantly improved, which can reach 350HV~360HV, thereby reducing the wear on the tool surface.

[0043] Furthermore, the transition layer 2 includes a first film layer 20 and a second film layer 22 which are stacked on each other. The first film layer 20 covers the surface of the blade body 1, and the first film layer 20 is a single metal layer, and the single metal is a component contained in the blade body 1, that is, a metal single substance with a relatively high content in the blade body 1 is selected to form the first film layer 20 on the surface of the blade body 1, so that the first film layer 20 and the blade body 1 form a reliable bond; the second film layer 22 covers the surface of the first film layer 20, and the second film layer 22 is a carbon layer, that is, the carbon contained in the self-lubricating layer 3 is selected to form the second film layer 22, so that the second film layer 22 and the self-lubricating layer 3 form a reliable bond; due to the high bonding between carbon and metal, the first film layer 20 and the second film layer 22 can form a reliable bond, and the bonding of the three-layer structure formed by the first film layer 20, the second film layer 22 and the self-lubricating layer 3 arranged in sequence is very good, so that the surface of the blade body 1 can be prevented from delaminating or falling off during use.

[0044] Furthermore, a permeation structure is formed on the interface between the second film layer 22 and the first film layer 20, that is, a layer between the second film layer 22 and the first film layer 20 contains components of both the first film layer 20 and the second film layer 22, and acts as a transition between the second film layer 22 and the first film layer 20, so that the second film layer 22 and the first film layer 20 can fuse with each other, thereby improving the reliability of the bonding between the second film layer 22 and the first film layer 20.

[0045] Preferably, the mass proportion of the above-mentioned metal element in the blade body 1 is not less than 12%, so that the metal element is the element with the highest content in the blade body 1 except iron. For example, the mass proportion of the metal element in the blade body 1 can be 12% to 14%. Typically but not limitatively, the mass proportion of the metal element in the blade body 1 can be 12%, 12.2%, 12.4%, 12.6%, 12.8%, 13%, 13.2%, 13.4%, 13.6%, 13.8% or 14%, etc.

[0046] Furthermore, the material of the blade body 1 is martensitic stainless steel, such as 3Cr13, 5Cr15MoV, 9Cr18, Cr15MnMoCoV and the like. In a specific embodiment, the composition and corresponding mass proportion of the blade body 1 can be: C 0.26% to 0.35%; Si ≤ 1.00%; Mn ≤ 1.00%; S ≤ 0.030%; P ≤ 0.035%; Cr 12.00% to 14.00%; Ni ≤ 0.60%; the remainder is Fe. The single metal is chromium, and the content of chromium in martensitic stainless steel is relatively high, and the hardness of the film layer formed by chromium is high, about 380HV to 400HV, that is, the first film layer 20 can be made of a material with higher hardness, thereby ensuring that the hardness of the tool meets the use requirements.

[0047] Further, the thickness of the first film layer 20 is 1 μm to 1.5 μm. For example, the thickness of the first film layer 20 can be 1 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm or 1.5 μm, etc., to form a continuous and uniform coating, ensure that the first film layer 20 has a high bonding property, and keep the tool at a high toughness. When the thickness of the first film layer 20 is less than 1 μm, the thickness of the first film layer 20 is too thin, making it difficult for the first film layer 20 to evenly and completely cover the tool body 1, thereby affecting the bonding between the second film layer 22 and the first film layer 20; when the thickness of the first film layer 20 is greater than 1.5 μm, the thickness of the first film layer 20 is too thick. Since the first film layer 20 is usually made of a single metal with a high hardness, it will reduce the toughness of the tool and make the tool brittle.

[0048] Further, the thickness of the second film layer 22 is 0.8 μm to 1.2 μm, for example, the thickness of the second film layer 22 can be 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm or 1.2 μm, etc., to form a continuous and uniform coating, ensure that the second film layer 22 has a high bonding property, and ensure the structural strength of the second film layer 22 itself. When the thickness of the second film layer 22 is less than 0.8 μm, the thickness of the second film layer 22 is too thin, making it difficult for the second film layer 22 to evenly and completely cover the first film layer 22, thereby affecting the bonding between the self-lubricating layer 3 and the second film layer 22; when the thickness of the second film layer 22 is greater than 1.2 μm, the thickness of the second film layer 22 is too thick, resulting in a decrease in the strength of the second film layer 22 itself, causing interlayer fractures in the second film layer 22, thereby affecting the bonding force of the coating.

[0049] Further, the thickness of the self-lubricating layer 3 is 2 μm to 3 μm, for example, the thickness of the self-lubricating layer 3 can be 2 μm, 2.1 μm, 2.2 μm, 2.3 μm, 2.4 μm, 2.5 μm, 2.6 μm, 2.7 μm, 2.8 μm, 2.9 μm or 3 μm, so that the tool surface has a good self-lubricating effect and the tool maintains a high cutting performance. When the thickness of the self-lubricating layer 3 is less than 2 μm, the thickness of the self-lubricating layer 3 is too thin, and the self-lubricating layer 3 is difficult to form a uniform and complete coating, resulting in a reduction in the lubrication and wear reduction effect of the self-lubricating layer 3, thereby affecting the self-lubricating performance of the tool surface; when the thickness of the self-lubricating layer 3 is greater than 3 μm, the thickness of the self-lubricating layer 3 is too thick, affecting the sharpness of the tool.

[0050] Furthermore, the friction coefficient of the self-lubricating layer 3 is 0.1 to 0.2. For example, the friction coefficient of the self-lubricating layer 3 can be 0.1, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19 or 0.2, etc., so that the lubricity of the cutter is consistent with the characteristics of the food, so that the cutter can meet the cutting requirements of most food. When the friction coefficient of the self-lubricating layer 3 is less than 0.1, the surface of the cutter is too smooth, resulting in performance waste; when the friction coefficient of the self-lubricating layer 3 is greater than 0.2, the cutter is still prone to wear or scratches due to cutting food.

[0051] Further, in the self-lubricating layer 3, the mass proportion of carbon is 30% to 40%, for example, the mass proportion of carbon can be 30%, 30.1%, 30.2%, 30.3%, 30.4%, 30.5%, 30.6%, 30.7%, 30.8%, 30.9% or 40%, etc., so as to keep the friction coefficient of the tool within a reasonable range. When the mass proportion of carbon in the self-lubricating layer 3 is less than 30%, the carbon content is too low, resulting in excessive content of tungsten disulfide, thereby increasing the cost of the self-lubricating layer 3; when the mass proportion of carbon in the self-lubricating layer 3 is greater than 40%, the carbon content is too high, resulting in the friction coefficient of the self-lubricating layer 3 being greater than 0.2, thereby making it difficult to meet the lubrication requirements of the tool and affecting the service life of the tool.

[0052] like Figure 2 As shown, the embodiment of the present application also provides a tool processing method, which is used to process the tool provided by the embodiment of the present application, and the tool processing method includes steps S1 and S2. Step S1 includes preparing a tool body 1; step S2 includes using a sputtering deposition method to sequentially prepare a first film layer 20, a second film layer 22 and a self-lubricating layer 3 on the surface of the tool body 1, and the components of the self-lubricating layer 3 include tungsten disulfide and carbon, so that the tool surface has both high self-lubricating performance and high hardness and stability, preventing the self-lubricating layer 3 from failing and extending the service life of the tool; the first film layer 20 and the second film layer 22 play a transitional role between the tool body 1 and the self-lubricating layer 3, thereby improving the bonding between the self-lubricating layer 3 and the tool body 1; and the first film layer 20, the second film layer 22 and the self-lubricating layer 3 are all formed sequentially by a sputtering deposition method, which simplifies the processing technology, reduces the production cost, and has a high continuity between adjacent film layers, thereby improving the bonding between adjacent film layers.

[0053] Furthermore, in step S1, the blade body 1 may be made by conventional tool processing technology. For example, step S1 may include: stamping a blade blank, the blade blank is a strip of stainless steel having the same length as the blade body and a width of 18 mm to 40 mm, and then straightening, beveling and polishing in sequence to form a blade body 1 having a blade. After the blade body 1 is prepared, the blade body 1 needs to be cleaned and blown dry to keep the surface of the blade body 1 dry and clean, and to improve the adhesion of each film layer to the blade body 1.

[0054] Further, in step S2, the first film layer 20 is formed by sputtering a chromium target, and the second film layer 22 is formed by sputtering a graphite target, that is, the first film layer 20 is a chromium layer, and the second film layer 22 is a carbon layer.

[0055] Furthermore, in step S2, within the last 3 to 5 minutes of preparing the first film layer 20, the chromium target is gradually closed and the graphite target is gradually opened, so that the second film layer 22 can penetrate into the surface of the first film layer 20, forming a smooth transition between the second film layer 22 and the first film layer 20, further improving the reliable bonding between the second film layer 22 and the first film layer 20.

[0056] Furthermore, in step S2, the self-lubricating layer 3 is formed by sputtering a graphite target and a tungsten disulfide target simultaneously; in the last 3 to 5 minutes of preparing the second film layer 22, the power of the graphite target is gradually reduced to a set value, and the tungsten disulfide target is gradually turned on, forming a smooth transition between the self-lubricating layer 3 and the second film layer 22, thereby further improving the reliable bonding between the self-lubricating layer 3 and the second film layer 22.

[0057] Specifically, step S2 can be implemented using a multifunctional ion plating machine, which has two DC magnetron modules and two medium frequency magnetron modules. The specific steps are as follows:

[0058] Step S21: vertically hang the blade body 1 on the workbench in the multifunctional ion plating machine, turn on the mechanical pump, Roots pump, and molecular pump in sequence, and evacuate the vacuum to (3.0-5.0)×10 -3 Pa, and then turn on the ion source to use the glow discharge it generates to perform ion bombardment cleaning on the blade body 1. The ion source also has a promoting effect of ion-assisted deposition during the coating process.

[0059] Step S22: Deposit the first film layer 20, turn on the DC magnetron sputtering power supply, use DC magnetron sputtering to sputter a high-purity chromium target (chromium content is 99.99%), the sputtering power is 1200W~1300W, the bias voltage is 110V~130V, the ion source current is 1.2A~1.6A, the deposition time is 15min~20min, and the thickness of the first film layer 20 is 1μm~1.5μm.

[0060] Step S23: Deposit the second film layer 22. In the last 3 min to 5 min of the first film layer 20, adjust the sputtering current parameters of the chromium target and the graphite target, gradually turn off the power of the high-purity chromium target (i.e., slowly reduce the current bias), and at the same time gradually increase the power of the high-purity graphite target to deposit a carbon film as the second film layer 22. After stabilization, the target current of the graphite target is 3.0 A, the deposition gas pressure is 0.2 Pa to 0.5 Pa, and the working temperature is 50°C to 70°C, until the thickness of the second film layer is 0.8μm to 1.2μm.

[0061] Step S24: Deposit the self-lubricating layer 3. In the last 3 to 5 minutes of the second film layer 22, the working gas pressure is adjusted to 0.7 Pa to 0.8 Pa, the bias voltage is reduced to 50 V to 70 V, the current of the graphite target is gradually reduced (slowly adjusted from 3.0 A to 1.0 A) to 1.0 A, and at the same time, the current of the tungsten disulfide target is gradually started to 1.0 A to 1.2 A. Both targets are controlled by a medium frequency power supply. The deposition time is 180 min to 210 min, and the thickness of the self-lubricating layer is 2 μm to 3 μm.

[0062] It should be noted that during the process of depositing each film layer (including the first film layer 20, the second film layer 22 and the self-lubricating layer 3) in the coating machine, the workpiece rack and the tray on which the tool is suspended revolve in the coating machine at a speed of 1.5r / min to 2.0r / min; in order to improve the efficiency of depositing the film layer, the rotation of the workpiece rack can also be shut down during the process of coating the self-lubricating layer 3.

[0063] In order to illustrate the wear resistance of the above-mentioned cutting tools provided in the embodiments of the present application, the cutting tools provided in the embodiments of the present application were subjected to a wear resistance test by sampling, that is, at least 3 groups of sample cutting tools were selected, and GCr15 steel balls were used as friction pairs. The test was conducted under the friction conditions of 9.8N and 300r / min at room temperature. The longer the friction mileage, the better the wear resistance. The wear life of each group of sample cutting tools exceeded 3000m, and the friction coefficient of each group of sample cutting tools was between 0.1-0.2. Therefore, the cutting tools provided in the embodiments of the present application have good anti-wear and self-lubricating effects.

[0064] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A tool, characterized in that: include: Blade body (1); A transition layer (2) covering the surface of the blade body (1); A self-lubricating layer (3) covering the surface of the transition layer (2), wherein the components of the self-lubricating layer (3) include tungsten disulfide and carbon; The transition layer (2) comprises a first film layer (20) and a second film layer (22) which are stacked on top of each other; The first film layer (20) covers the surface of the blade body (1), the first film layer (20) is a single metal layer, the single metal is a component contained in the blade body (1), and the mass proportion of the single metal in the blade body (1) is not less than 12%; The second film layer (22) covers the surface of the first film layer (20), and the second film layer (22) is a carbon layer.

2. The tool according to claim 1, characterized in that The material of the knife body (1) is martensitic stainless steel, and the elemental metal is chromium.

3. The tool according to claim 1, characterized in that The thickness of the first film layer (20) is 1 μm to 1.5 μm.

4. The tool according to claim 1, characterized in that The thickness of the second film layer (22) is 0.8 μm to 1.2 μm.

5. The tool according to any one of claims 1 to 4, characterized in that: The thickness of the self-lubricating layer (3) is 2 μm to 3 μm.

6. The tool according to any one of claims 1 to 4, characterized in that: The friction coefficient of the self-lubricating layer (3) is 0.1-0.

2.

7. The tool according to any one of claims 1 to 4, characterized in that: In the self-lubricating layer (3), the mass proportion of carbon is 30% to 40%.

8. A tool processing method, characterized in that: The following steps are involved: Step S1: preparing a blade body (1); Step S2: using a sputtering deposition method to sequentially prepare a first film layer (20), a second film layer (22) and a self-lubricating layer (3) on the surface of the blade body (1), wherein the self-lubricating layer (3) comprises tungsten disulfide and carbon; The first film layer (20) is formed by sputtering a chromium target, and the second film layer (22) is formed by sputtering a graphite target.

9. The tool processing method according to claim 8, characterized in that: In the last 3 to 5 minutes of preparing the first film layer (20), the chromium target is gradually closed and the graphite target is gradually opened.

10. The tool processing method according to claim 8, characterized in that: The self-lubricating layer (3) is formed by sputtering a graphite target and a tungsten disulfide target simultaneously; In the last 3 to 5 minutes of preparing the second film layer (22), the power of the graphite target is gradually reduced to a set value, and the tungsten disulfide target is gradually turned on.

Citation Information

Patent Citations

  • coated TOOL

    AT504908A4

  • Amorphous-carbon-based hard multilayer film and hard surface member having the film on surface

    CN101062602A

  • Amorphous carbon coating and preparation method and application thereof

    CN101444985A

  • Tungsten disulfide (WS2) soft coating nano texture self-lubricating cutter and preparation method thereof

    CN102500778A

  • W-S-C-N self-lubricating gradient coating tool and manufacturing process thereof

    CN104862658A