A method for determining the three-dimensional crystal orientation of cast cubic single crystals

Through multiple directional cutting and grinding treatments, combined with dendrite direction and microcorrosion, the problems of expensive and limited application in the existing technology are solved, and the three-dimensional crystal orientation determination of arbitrary single crystals is realized, which improves efficiency and reduces cost.

CN114689405BActive Publication Date: 2024-11-12XIANGTAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210323362.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-29
Publication Date
2024-11-12
Estimated Expiration
2042-03-29

AI Technical Summary

Technical Problem

In the prior art, when determining the three-dimensional crystal orientation of cast single crystal high-temperature alloys, the equipment is expensive and complicated, and can only be used for block materials with central axis characteristics, and block materials with arbitrary geometric characteristics cannot be calibrated.

Method used

Through multiple directional cutting and grinding treatments, the orientation of the single crystal is determined using the dendrite direction, and the mixed corrosion agent of CuSO4, HCl and H2O is used for microcorrosion, and a macroscopic and crystal coordinate system is established to gradually determine the three-dimensional crystal orientation of any shape single crystal.

Benefits of technology

The three-dimensional crystal orientation determination of any shape nickel-based single-crystal high-temperature alloy is realized, which reduces equipment requirements and process complexity, significantly improves the efficiency of orientation determination and reduces costs, and extends the scope of application to parts of all geometric structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114689405B_ABST
    Figure CN114689405B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for determining the three-dimensional crystal orientation of a cast cubic single crystal. The present invention comprises the steps of cutting a single crystal, making a marking line 1 parallel to a primary dendrite on a section 1, cutting a calibration sample 1 perpendicular to the section 1, making a marking line 2 parallel to a primary dendrite on a section 2, cutting a calibration sample 2 perpendicular to the section 2, and calibrating the crystal orientation on the section 3. The present invention can determine the three-dimensional crystal orientation of a nickel-based single crystal high-temperature alloy of any shape, breaking through the limitation of the prior art that only the cast block material with central axis characteristics can be determined, and at the same time, the process is simple and the equipment requirements are low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of crystal orientation of cubic warp system single crystals, and in particular to a method for determining the three-dimensional crystal orientation of a cast cubic crystal system single crystal. Background Art

[0002] Single crystal high temperature alloys have excellent high temperature properties and are the preferred materials for turbine blades of advanced aircraft engines and ground gas turbines. The crystal lattice structure of nickel-based single crystal high temperature alloys belongs to the cubic system, and its mechanical properties have significant anisotropy, so orientation control is required during the preparation of single crystals. The seed crystal method is a method that can accurately control the crystal orientation of single crystal blades and has significant advantages in the field of single crystal preparation. Before using the seed crystal method to prepare single crystals, it is necessary to orientate and cut single crystals with specific orientations from large single crystals as seed crystals, so it is necessary to first determine the crystal orientation of the large single crystal.

[0003] Chinese invention CN104846441A discloses a method for cutting and preparing nickel-based single crystal alloy seed crystals for casting, and proposes an operational cutting scheme that can determine the crystal orientation of the single crystal and cut seed crystals of different orientations. However, this method requires the use of X-rays to measure the characteristic angles of the test block, and has the disadvantages of expensive equipment and complicated processes. Chinese invention CN109916693A discloses a method for determining the crystal orientation of a cast single crystal high-temperature alloy, and proposes that the crystal orientation of a cast single crystal high-temperature alloy can be determined by the dendrite direction. The equipment used in this method is simple, and the determination of the crystal orientation of a single crystal is relatively convenient, but this method is only applicable to cast block materials with central axis characteristics such as cylindrical and cubic shapes, and cannot calibrate the crystal orientation of a block cast single crystal high-temperature alloy with arbitrary geometric characteristics, and has application limitations. Summary of the invention

[0004] In order to overcome the shortcomings of the prior art in determining the three-dimensional crystal orientation of cast single crystal high-temperature alloys, such as expensive equipment and complicated processes, or only being able to determine the three-dimensional crystal orientation of cast block materials with central axis characteristics, the present invention proposes a method for determining the three-dimensional crystal orientation of cast cubic single crystals, which can determine the three-dimensional crystal orientation of nickel-based single crystal high-temperature alloys of any shape.

[0005] The technical solution of the present invention is:

[0006] A method for determining the three-dimensional crystal orientation of a cast cubic single crystal comprises the following steps:

[0007] (1) Cutting single crystal

[0008] For a single crystal of any shape, a cross section 1 is cut out in any direction to obtain a calibration sample 1, the cross section 1 is ground and polished, and micro-etched to obtain primary dendrites and secondary dendrites on the cross section 1;

[0009] (2) Make a marking line 1 on section 1 parallel to the primary dendrite

[0010] Draw a line on section 1 as marking line 1, and marking line 1 is parallel to the direction of any secondary dendrite in section 1;

[0011] (3) Vertical section 1 cutting calibration specimen 1

[0012] The calibration sample 1 is cut perpendicular to the cross section 1 and parallel to the marking line 1 to obtain the cross section 2 and the calibration sample 2, the cross section 2 is ground and polished, and micro-etched to obtain primary dendrites and secondary dendrites on the cross section 2;

[0013] (4) Make a marking line 2 on section 2 parallel to the primary dendrite

[0014] Draw a line on the cross section 2 as a marking line 2, and the marking line 2 is parallel to the direction of any primary dendrite in the cross section 2;

[0015] (5) Vertical section 2 cutting calibration sample 2

[0016] The calibration sample 2 is cut perpendicular to the cross section 2 and parallel to the calibration line 2 to obtain the cross section 3 and the calibration sample 3, the cross section 3 is ground and polished, and micro-etched to obtain primary dendrites and secondary dendrites on the cross section 3;

[0017] (6) Determine the crystal orientation on section 3

[0018] Draw a line on section 3 <001> Direction marking line, and make the <001> The direction marking line is parallel to the primary dendrite direction. <001> The direction of the direction marking line is the direction of the single crystal <001> Direction, continue to draw a line on section 3 to make a vertical line in the dendrite direction, the vertical line is <100> Direction marking line or <010> Direction marking line; <100> The direction of the direction marking line is the direction of the single crystal <100> Direction, <010> The direction of the direction marking line is the direction of the single crystal <010> direction.

[0019] Furthermore, the micro-corrosion uses a mixture of CuSO4, HCl and H2O as the etchant, and the corrosion time is 10-30 seconds.

[0020] Further, the ratio of CuSO4, HCl and H2O is 3-5 g:10-30 ml:10-30 H2O ml.

[0021] Mathematical principles are used to prove that the crystal orientation of a single crystal of a cubic system of any shape can be determined through a finite number of directional cuttings, such as Figure 1A macroscopic coordinate system OXYZ is established on section 1, where the OX direction is parallel to the primary dendrite direction. The coordinates of section 2 and the crystal orientation are as follows: Figure 2 As shown, the cross-section 3 coordinates and crystal orientation are as follows Figure 3 shown. Figure 4 Shown is the crystal orientation of a single crystal determined using the method of the present invention.

[0022] The beneficial effects of the present invention are:

[0023] The present invention can determine the three-dimensional crystal orientation of nickel-based single crystal high-temperature alloys of any shape, breaking through the limitation of the prior art that it can only determine the cast block materials with central axis characteristics, and can expand the types of parts for determining the single crystal orientation by metallographic observation combined with the directional cutting method to parts of all geometric structures. The process is simple, and the efficiency of crystal orientation determination can be significantly improved, saving time; at the same time, the equipment requirements are low, and the cost of crystal orientation determination is reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic diagram of the macroscopic coordinate system, crystal coordinate system and dendrite morphology in section 1;

[0025] Figure 2 It is a schematic diagram of the macroscopic coordinate system, crystal coordinate system and dendrite morphology in section 2;

[0026] Figure 3 It is a schematic diagram of the macro coordinate system, crystal coordinate system and dendrite morphology in section 3;

[0027] Figure 4 The crystal orientation of a single crystal is determined by the method of the present invention.

[0028] Among them, 1, marking line 1; 2, marking line 2; 3, marking line 3; 4, marking line 4; OXYZ, three coordinates of the macroscopic coordinate system; oxyz, coordinates of the crystal coordinate system. DETAILED DESCRIPTION

[0029] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited thereto.

[0030] Example 1

[0031] This embodiment is to determine the crystal orientation of a cylindrical cast cobalt-based single crystal high-temperature alloy with a diameter of 7.5 mm and a length of 15 mm.

[0032] The cobalt-based single crystal high-temperature alloy consists of Cr, Mo, Al, Co, W, Re, Ta, Hf, C and Co, wherein the mass percentage composition of the alloy is: Cr 3.2%, Mo 1.2%, Al 6%, Co 10%, W 6%, Re 4%, Ta 7.98%, Hf0.008%, C≤0.02%, and the rest is Co.

[0033] The specific process of this embodiment is:

[0034] Step 1: Cutting the single crystal

[0035] A cross section 1 is cut out in a direction parallel to an upper end face of the cylinder to obtain a calibration sample 1 , and the cross section 1 is ground and polished, and micro-etched to obtain primary dendrites and secondary dendrites on the cross section 1 .

[0036] Grinding and polishing conditions: 80#, 320#, 600#, 1000#, 1200# water-abrasive sandpaper was used to polish the section 1, and then polished on a polishing machine. The polished section 1 was etched; the etchant ratio was a mixture of 4gCuSO4, 20ml HCl and 20ml H2O; the etching time was 20s. After the etching treatment, the primary dendrite and secondary dendrite morphology were exposed.

[0037] Step 2: Make a marking line 1 on section 1 parallel to the primary dendrite

[0038] Draw a line on section 1 as marking line 1, which is parallel to the direction of any secondary dendrite in section 1.

[0039] Step 3: Cut the calibration sample 1 vertically through section 1

[0040] The calibration sample 1 is cut perpendicular to the cross section 1 and parallel to the marking line 1 to obtain the cross section 2 and the calibration sample 2. The cross section 2 is ground and polished, and micro-etched to obtain primary dendrites and secondary dendrites on the cross section 2.

[0041] The specific process of cutting the calibration sample 1 is:

[0042] A cutting line is made on the cross section 1 of the calibration sample 1 , the cutting line is parallel to the marking line 1 , and the cutting direction is perpendicular to the cross section 1 .

[0043] The distance from one edge to the other is 12 mm.

[0044] Step 4: Make a marking line 2 on section 2 parallel to the primary dendrite

[0045] A line is drawn on the cross section 2 as a marking line 2 , and the marking line 2 is parallel to the direction of any exposed longer primary dendrite in the cross section 2 .

[0046] Step 5: Cut the calibration sample 2 vertically

[0047] The calibration sample 2 is cut perpendicular to the cross section 2 and parallel to the calibration line 2 to obtain the cross section 3 and the calibration sample 3. The cross section 3 is ground and polished, and micro-etched to obtain primary dendrites and secondary dendrites on the cross section 3.

[0048] Step 6: Determine the crystal orientation on section 3

[0049] Draw a line on section 3 <001> Direction mark line 3, and make the <001> The direction marking line is parallel to the primary dendrite direction. <001> The direction of the direction marking line is the direction of the single crystal <001> Continue to draw a line on the cross section 3 to make a vertical line in the dendrite direction. <010> Direction marking line 4; <100> The direction of the direction mark line 3 is the single crystal <100> Direction, <010> The direction indicated by the direction mark line 4 is the single crystal <010> direction.

[0050] Example 2

[0051] This embodiment is to determine the crystal orientation of a spherical cast nickel-based single crystal high-temperature alloy with a diameter of 30 mm.

[0052] The nickel-based single crystal high-temperature alloy is composed of Cr, Mo, Al, Co, W, Re, Ta, Hf, C and Ni, wherein the mass percentage composition of the alloy is: Cr 3.2%, Mo 1.2%, Al 6%, Co 10%, W 6%, Re 4%, Ta 7.98%, Hf0.008%, C≤0.02%, and the rest is Ni.

[0053] The specific process of this embodiment is:

[0054] Step 1: Cutting the single crystal

[0055] A cross section 1 is cut out in any direction on the sphere to obtain a calibration sample 1 , and the cross section 1 is ground and polished, and micro-etched to obtain primary dendrites and secondary dendrites on the cross section 1 .

[0056] Grinding and polishing conditions: 80#, 320#, 600#, 1000#, 1200# water-abrasive sandpaper was used to polish the section 1, and then polished on a polishing machine. The polished section 1 was etched; the etchant ratio was a mixture of 4gCuSO4, 20ml HCl and 20ml H2O; the etching time was 20s. After the etching treatment, the primary dendrite and secondary dendrite morphology were exposed.

[0057] Step 2: Make a marking line 1 on section 1 parallel to the primary dendrite

[0058] Draw a line on section 1 as marking line 1, which is parallel to the direction of any secondary dendrite in section 1. Step 3: Cut the calibration sample 1 perpendicular to section 1.

[0059] The calibration sample 1 is cut perpendicular to the cross section 1 and parallel to the marking line 1 to obtain the cross section 2 and the calibration sample 2. The cross section 2 is ground and polished, and micro-etched to obtain primary dendrites and secondary dendrites on the cross section 2.

[0060] The specific process of cutting the calibration sample 1 is:

[0061] A cutting line is made on the cross section 1 of the calibration sample 1. The cutting line is parallel to the marking line 1, and the cutting direction is perpendicular to the cross section 1.

[0062] The distance from one edge to the other is 12 mm.

[0063] Step 4: Make a marking line 2 on section 2 parallel to the primary dendrite

[0064] A line is drawn on the cross section 2 as a marking line 2 , and the marking line 2 is parallel to the direction of any exposed longer primary dendrite in the cross section 2 .

[0065] Step 5: Cut the calibration sample 2 vertically

[0066] The calibration sample 2 is cut perpendicular to the cross section 2 and parallel to the calibration line 2 to obtain the cross section 3 and the calibration sample 3. The cross section 3 is ground and polished, and micro-etched to obtain primary and secondary dendrites on the cross section 3.

[0067] Step 6: Determine the crystal orientation on section 3

[0068] Draw a line on section 3 <001> Direction mark line 3, and make the <001> The direction marking line is parallel to the primary dendrite direction. <001> The direction of the direction marking line is the direction of the single crystal <001> Direction. Continue to draw a perpendicular line on section 3 to the dendrite direction. This perpendicular line is <010> Direction marking line 4; <100> The direction of the direction mark line 3 is the single crystal <100> Direction, <010> The direction indicated by the direction mark line 4 is the single crystal <010> direction.

[0069] Example 3

[0070] This embodiment is to determine the crystal orientation of an irregularly shaped cast nickel-based single crystal high-temperature alloy, whose maximum dimension length is 50 mm and minimum dimension length is 10 mm.

[0071] The nickel-based single crystal high-temperature alloy consists of Cr, Mo, Al, Co, W, Re, Ta, Hf, C and Ni, wherein the mass percentage composition of the alloy is: Cr 3%, Mo 1%, Al 6%, Co 12%, W 6%, Re 4%, Ta 7.95%, Hf 1%, C≤0.02%, and the rest is Ni.

[0072] The specific process of this embodiment is:

[0073] Step 1: Cutting the single crystal

[0074] A cross section 1 is cut out in any direction of an irregularly shaped single crystal to obtain a calibration sample 1 , the cross section 1 is ground and polished, and micro-etched to obtain primary dendrites and secondary dendrites on the cross section 1 .

[0075] Grinding and polishing conditions: 80#, 320#, 600#, 1000#, 1200# water-abrasive sandpaper was used to polish the section 1, and then polished on a polishing machine. The polished section 1 was etched; the etchant ratio was a mixture of 4gCuSO4, 20ml HCl and 20ml H2O; the etching time was 20s. After the etching treatment, the primary dendrite and secondary dendrite morphology were exposed.

[0076] Step 2: Make a marking line 1 on section 1 parallel to the primary dendrite

[0077] A line is drawn on the cross section 1 as a marking line 1 , and the marking line 1 is parallel to the direction of any secondary dendrite in the cross section 1 .

[0078] Step 3: Cut the calibration sample 1 vertically through section 1

[0079] The calibration sample 1 is cut perpendicular to the cross section 1 and parallel to the marking line 1 to obtain the cross section 2 and the calibration sample 2. The cross section 2 is ground and polished, and micro-etched to obtain primary dendrites and secondary dendrites on the cross section 2.

[0080] The specific process of cutting the calibration sample 1 is:

[0081] A cutting line is made on the cross section 1 of the calibration sample 1. The cutting line is parallel to the marking line 1, and the cutting direction is perpendicular to the cross section 1.

[0082] The distance from one edge to the other is 12 mm.

[0083] Step 4: Make a marking line 2 on section 2 parallel to the primary dendrite

[0084] A line is drawn on the cross section 2 as a marking line 2 , and the marking line is parallel to the direction of any exposed relatively long primary dendrite in the cross section 2 .

[0085] Step 5: Cut the calibration sample 2 vertically

[0086] The calibration sample 2 is cut perpendicular to the cross section 2 and parallel to the calibration line 2 to obtain the cross section 3 and the calibration sample 3. The cross section 3 is ground and polished, and micro-etched to obtain primary and secondary dendrites on the cross section 3.

[0087] Step 6: Determine the crystal orientation on section 3

[0088] Draw a line on section 3 <001> Direction mark line 3, and make the <001> The direction marking line is parallel to the primary dendrite direction. <001> The direction of the direction marking line is the direction of the single crystal <001> Continue to draw a line on section 3 to make a perpendicular line in the dendrite direction. <010> Direction marking line 4; <100> The direction of the direction mark line 3 is the single crystal <100> Direction, <010> The direction indicated by the direction mark line 4 is the single crystal <010> direction.

Claims

1. A method for determining the three-dimensional crystal orientation of a cast cubic single crystal, characterized in that: The steps include: (1) Cutting single crystal For a single crystal of any shape, a cross section 1 is cut out in any direction to obtain a calibration sample 1, the cross section 1 is ground and polished, and micro-etched to obtain primary dendrites and secondary dendrites on the cross section 1; (2) Make a marking line 1 on section 1 parallel to the primary dendrite Draw a line on section 1 as marking line 1, and marking line 1 is parallel to the direction of any secondary dendrite in section 1; (3) Vertical section 1 cutting calibration specimen 1 The calibration sample 1 is cut perpendicular to the cross section 1 and parallel to the marking line 1 to obtain the cross section 2 and the calibration sample 2, the cross section 2 is ground and polished, and micro-etched to obtain primary dendrites and secondary dendrites on the cross section 2; (4) Make a marking line 2 on section 2 parallel to the primary dendrite Draw a line on the cross section 2 as a marking line 2, and the marking line 2 is parallel to the direction of any primary dendrite in the cross section 2; (5) Vertical section 2 cutting calibration sample 2 The calibration sample 2 is cut perpendicular to the cross section 2 and parallel to the calibration line 2 to obtain the cross section 3 and the calibration sample 3, the cross section 3 is ground and polished, and micro-etched to obtain primary dendrites and secondary dendrites on the cross section 3; (6) Determine the crystal orientation on section 3 Draw a line on section 3 <001> Direction marking line, and make the <001> The direction marking line is parallel to the primary dendrite direction. <001> The direction of the direction marking line is the direction of the single crystal <001> Direction, continue to draw a line on section 3 to make a vertical line in the dendrite direction, the vertical line is <100> Direction marking line or <010> Direction marking line; <100> The direction of the direction marking line is the direction of the single crystal <100> Direction, <010> The direction of the direction marking line is the direction of the single crystal <010> direction.

2. The method for determining the three-dimensional crystal orientation of a cast cubic single crystal according to claim 1, characterized in that: Primary dendrites and secondary dendrites are fully interchangeable.

3. The method for determining the three-dimensional crystal orientation of a cast cubic single crystal according to claim 1, characterized in that: The micro-corrosion uses a mixture of CuSO4, HCl and H2O as the etchant, and the corrosion time is 10-30 seconds.

4. The method for determining the three-dimensional crystal orientation of a cast cubic single crystal according to claim 3, characterized in that: The ratio of CuSO4, HCl and H2O is 3-5 g:10-30 ml:10-30 H2O ml.