Application of a chitosan Schiff base loaded divalent copper material in the preparation of β-boryl ester

By using chitosan Schiff base-supported divalent copper material to catalyze the reaction of α-propenyl ester compound and pennasol biborate at room temperature, the problem of using expensive transition metals and strong alkalis in the prior art is solved, and the problem of using expensive transition metals and strong alkalis is achieved. The efficient and environmentally friendly β-boron-based ester compound synthesis meets the needs of green environmental protection and industrial applications.

CN114702517BActive Publication Date: 2024-11-08HUBEI ENG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210454738.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-27
Publication Date
2024-11-08
Estimated Expiration
2042-04-27

AI Technical Summary

Technical Problem

The prior art requires the use of expensive transition metal catalysts and strong bases when synthesizing β-boron-based ester compounds, and the reaction conditions are harsh and cannot meet the needs of green environmental protection and industrial applications.

Method used

Using chitosan Schiff base-supported divalent copper material as a catalyst, the β-boronyl ester compound was generated by reacting with α-propenyl ester compound and pennadol biborate in pure water at room temperature, thereby avoiding other The use of added alkali and the material is recyclable and low cost.

Benefits of technology

The synthesis of β-boron-based ester compounds with high activity, high selectivity and low catalytic dosage has the advantages of low cost, low pollution, easy operation and wide substrate range, and has expanded the synthesis method of constructing C-B bonds, which has industrial value. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114702517B_ABST
    Figure CN114702517B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a chitosan Schiff base-loaded divalent copper material and its application in the synthesis of β-boryl ester compounds. The material uses chitosan Schiff base as a carrier, and the immobilized divalent copper ions are catalytically active components. The specific contents are: chitosan Schiff base-loaded divalent copper material (CX@Cu) is a catalyst, biboric acid pinacol ester is a boron reagent, and pure water is a solvent, and α-propenyl ester compounds containing different substituent groups are subjected to boron addition reaction to obtain β-boryl ester compounds. The chitosan Schiff base-loaded divalent copper material of the invention meets the core requirements of "saving resources, less pollution, reducing costs, and being recyclable" in green chemistry. And the method can synthesize organic boron compounds in the aqueous phase without any addition, provides a new method for the preparation of drug molecules and active intermediates, broadens the substrate range for preparing organic boron compounds, and has important theoretical and practical significance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of organic synthesis, and in particular to a specific application of a chitosan Schiff base loaded divalent copper material in the preparation of beta-boryl ester. Background Art

[0002] As an important class of synthetic intermediates, the CB bond of organoboron compounds can undergo a series of transformations through oxidation reactions, Suzuki-Miyaura coupling reactions, Petasis reactions, etc. to obtain CO bonds, CN bonds, and CC bonds; at the same time, organoboron compounds have a series of advantages in organic synthesis, such as good stability, easy preparation, low toxicity, wide functional group tolerance, and strong synthetic versatility. These excellent properties make organoboron compounds widely used in organic synthesis, materials, biomedicine and other fields. Organoboron compounds can be widely used as organic functional polymers. In the past few years, many strategies for synthesizing and constructing organoboron compounds have been successfully established. However, these methods have their own limitations and cannot meet the needs of diversified synthesis, so it is worth further exploring the development of new methods and new approaches for synthesizing organoboron compounds.

[0003] In 2020, in the literature (Angew. Chem. Int. Ed. 2020, 59 (26)), Wu's group used copper as a catalyst to catalyze the regioselective borocarbonylation coupling reaction of unactivated olefins with halogenated alkyl compounds to synthesize β-boryl ketone compounds; this reaction requires the addition of a strong base LiOMe, using dimethylacetamide as a solvent, and is carried out under heating conditions at 60°C. From the perspective of energy conservation and environmental protection, this method uses strong bases and organic solvents, which is environmentally unfriendly; from the perspective of substrate range, the substrate type is limited to benzene ring substituted substrates and cannot be extended to other groups such as alkyl chains. In the same year, the literature (Angew. Chem. Int. Ed. 2020, 59 (39)) used a Cu / Pd complex catalyst, with styrene, aromatic iodide, B2pin2 and CO as substrates, and successfully synthesized β-boryl ketone through a carbonylation reaction under the condition of adding base. Later, the authors expanded to methyl trifluorosulfonic acid as a substrate. The reaction required complex copper salts, palladium salts, toluene, a large amount of strong base and anhydrous and oxygen-free operation. Due to the limitations of the reaction itself, it cannot be expanded to substrates other than benzene ring substituents. The above shortcomings limit the application of this method.

[0004] In existing literature reports, various substrates used to construct different CB bond types mostly use expensive and toxic transition metals. When applied to homogeneous catalysis, although the activity of the reaction system is very high, most of them require strong base additives, high-priced ligands and transition metals, which cannot meet the concept of green sustainable development. Although there are reports of low-cost monovalent copper catalysis to prepare various organic borides, the reaction conditions are harsh, requiring a series of cumbersome operations such as strong base, anhydrous and oxygen-free, and low temperature, and its efficiency is not high, which cannot meet the application in actual production. In order to overcome these problems, it is of great significance to expand the preparation range of organic borides and explore high-efficiency and environmentally friendly catalytic reaction pathways for different types of organic borides. Summary of the invention

[0005] The purpose of the present invention is to solve the shortcomings of the above-mentioned background technology and provide a chitosan Schiff base loaded with divalent copper material as a catalyst for synthesizing a series of β-boryl ester compounds.

[0006] Chitosan has a single property. The main chain of the modified chitosan Schiff base polymer has amino groups, making it a natural cationic polymer, creating an alkaline environment for the organic reaction system and avoiding the use of other added bases. At the same time, chitosan Schiff base material is a stable multifunctional material with an open network, large pores, and a high specific surface area. It can be used as a large chelating ligand for active metal catalysts, as a carrier for dispersed nanoparticles, and as a direct heterogeneous organic catalyst. This heterogeneous catalyst material is easy to separate and recycle, and can be used repeatedly. At the same time, in terms of the selection of catalytic metal ions, compared with high-priced and highly polluting metals such as palladium, rhodium, and nickel, copper is a transition metal that is cheap, abundant in resources, and widely used. Therefore, this method is green, environmentally friendly, low-cost, and recyclable, providing an effective idea for constructing a new class of CB bond compounds and has potential industrial value.

[0007] The technical solution of the present invention is: application of a chitosan Schiff base loaded divalent copper material in catalytic preparation of β-boryl ester compounds, characterized in that the specific application steps include:

[0008] 1) adding an α-propylene ester compound I as a substrate, bipyraclostrobin as a boron source, and a chitosan Schiff base-loaded divalent copper material CX@Cu as a catalyst into pure water, mixing and stirring at room temperature for 8 to 16 hours, wherein the molar ratio of the α-propylene ester compound I, bipyraclostrobin, and CX@Cu-loaded copper is 1:(1 to 2):(0.01 to 0.05),

[0009] The chemical reaction equation is as follows:

[0010]

[0011] Wherein, R is phenyl, methyl, n-butyl, dodecyl, tert-butyl, 2-methoxyethyl;

[0012] 2) After the reaction is completed, the reaction is filtered, and the solid phase is washed, centrifuged, and dried to obtain the recovered chitosan Schiff base-loaded divalent copper material CX@Cu, which is recycled for the next reaction; the obtained liquid phase is separated and purified to obtain the β-boryl ester compound II.

[0013] Preferably, the copper content in the material CX@Cu in step a is 0.6 to 1.6 mmol / g.

[0014] Preferably, in step a, the molar ratio of the copper ion content of the α-propylene ester compound I, the bipyraclostrobin and the CX@Cu material is 1:2:0.0167-0.025.

[0015] Preferably, in step 1), the ratio of the amount of copper loaded to water in the chitosan Schiff base copper functional material CX@Cu is 0.005 mmol: 1-2 ml.

[0016] Preferably, in step 1), the mixture is stirred and reacted at room temperature for 16 hours.

[0017] Preferably, the filtrate obtained in step 2) is separated and purified to obtain the β-boryl ester compound II, specifically comprising: extracting the filtrate with ethyl acetate to obtain an organic phase containing the product, then drying over anhydrous Na2SO4, filtering, and rotary evaporation to remove excess organic solvent, and purifying the obtained crude product by column chromatography with a mixed solvent of ethyl acetate and petroleum ether to obtain the β-boryl ester compound II.

[0018] Preferably, in step 1), the chitosan Schiff base-loaded divalent copper material CX@Cu is prepared by a method comprising the following steps:

[0019] a. Mix glacial acetic acid and anhydrous ethanol in a volume ratio of 1:5-8 to obtain an acetic ethanol solution, add chitosan and an aldehyde compound to the acetic ethanol solution, and react at 25-50°C with stirring for 8-16 hours, wherein the aldehyde is one of 2-quinolinecarboxaldehyde, 5-bromosalicylaldehyde, and 3,5-di-tert-butylsalicylaldehyde, and the molar ratio of amino group -NH2 in chitosan to aldehyde group -CHO in the aldehyde compound is 1:3-4;

[0020] b. After the reaction is completed, the chitosan Schiff base material is separated, washed and dried to obtain a powder;

[0021] c . Place the chitosan Schiff base material in a copper sulfate solution and stir the reaction at 25-50°C for 8-16 hours to promote the adsorption of divalent copper ions;

[0022] d. After the adsorption is completed, the chitosan Schiff base loaded divalent copper material CX@Cu is obtained by separation, washing and drying.

[0023] The chemical equation for preparing chitosan Schiff base material from the above chitosan and aldehyde is:

[0024]

[0025] L is: One of them.

[0026] Further steps a The acetic acid and anhydrous ethanol are mixed in a volume ratio of 1:7.5 to obtain an acetic acid ethanol solution, and the molar ratio of amino group -NH2 in chitosan to aldehyde group -CHO in the aldehyde compound is 1:4.

[0027] Further, the copper sulfate solution in step c contains Cu 2+ The molar ratio of amino-NH2 in chitosan is at least 1:1, step c The copper ion concentration in copper sulfate solution is 0.16~0.24mol / L.

[0028] Furthermore, the separation, washing and drying in steps b and d both include: after filtering, washing the obtained solid phase with water and ethanol repeatedly and alternately, and drying in an oven at 50° C. for 12 hours.

[0029] During the preparation of chitosan Schiff base copper functional materials, copper sulfate solution provides sufficient copper ions to the chitosan Schiff base material, so that it can adsorb copper ions through its own adsorption capacity, which is a routine operation in the art.

[0030] In the present invention, the hydroxyl and amino groups in the molecular structure of chitosan can coordinate with transition metal ions and have strong chelating ability, which can coordinate with heavy metal ions Pb 2+ 、Zn 2+ , Hg + Forming chelates, such as with Hg + Forming a stable -N-Hg-O-inner salt structure, Cu 2+ With a tetra-coordinated metal ion, copper and chitosan are coordinated by heteroatoms to form a chelate with a special structure. Chitosan modified by aldehyde chemistry can further enhance stability and biocompatibility and change its weak mechanical properties. Under the catalysis of active copper in the CX@Cu catalytic material, B2(pin)2 breaks the BB bond and reacts with divalent copper to form a copper borane complex and a by-product Bpin-OH. Under the guidance of the carbonyl group, it undergoes a conjugate addition reaction of an unsaturated acceptor with α-propenyl ester to generate an intermediate. Through a polycyclic transition rearrangement, the proton source is provided by the solvent water, the target product is generated through a protonation process, and the regeneration of the catalytic material is achieved. In the Cu 2+ In a catalytic system, the rate-determining step is the protonation process.

[0031] The beneficial effects of the present invention are:

[0032] 1. The present invention provides a method for preparing a chitosan Schiff base-loaded divalent copper material, which has the advantages of high activity, high selectivity, recyclability, low catalytic dosage, etc.

[0033] 2. The catalytic material successfully realizes the boron addition reaction of α-propylene ester substrates. The synthesis method is carried out at room temperature with pure water as solvent and has the advantages of low cost, low pollution, simple components, easy operation and a wide range of substrates.

[0034] 3. This invention applies green and recyclable heterogeneous catalysts to organic boron addition reactions, expanding the synthetic method for constructing CB bonds. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 is the H NMR spectrum of the target product in Example 2;

[0036] Figure 2 It is the NMR carbon spectrum of the target product in Example 2. DETAILED DESCRIPTION

[0037] The following specific examples further illustrate the present invention in detail. The following specific examples further illustrate the present invention in detail. The drugs used in the examples are all commercially available products unless otherwise specified, and the methods used are all conventional methods in the art unless otherwise specified.

[0038] Example 1

[0039] The specific preparation method of the chitosan Schiff base loaded divalent copper material is as follows:

[0040] a. Mix glacial acetic acid and anhydrous ethanol in a volume ratio of 1:7.5 to obtain an acetic ethanol solution, add 1 g of chitosan and an aldehyde compound to the acetic ethanol solution, and stir the reaction at 50°C for 12 hours, wherein 1.0 g of chitosan contains about 6.2 mmol -NH2, and the molar ratio of amino -NH2 in chitosan to aldehyde group -CHO in the aldehyde compound is 1:4;

[0041] b. After the reaction is completed, the reaction solution is filtered, the resulting precipitate is repeatedly washed with water and ethanol alternately, and dried in an oven at 50° C. for 12 h to obtain a chitosan Schiff base material;

[0042] c. Add the chitosan Schiff base material obtained in step b to 30 mL of copper sulfate solution (prepared from 1.6 g of copper sulfate pentahydrate, containing about 6.4 mmol Cu 2+ ) and stirred at 50 °C for 12 h to promote the adsorption of divalent copper ions;

[0043] d. After the adsorption is completed, the reaction solution is filtered and the precipitate is repeatedly washed with water and ethanol alternately, and then dried in an oven at 50°C for 12 h to obtain the chitosan Schiff base-loaded divalent copper material CX@Cu.

[0044] When the aldehyde in step a of the above preparation method is 2-quinolinecarboxaldehyde, a chitosan Schiff base-loaded divalent copper material CX1@Cu is obtained (the divalent copper content is 0.9 mmol / g as determined by ICP);

[0045] When the aldehyde in step a of the above preparation method is 5-bromosalicylaldehyde, a chitosan Schiff base-loaded divalent copper material CX2@Cu (the divalent copper content determined by ICP is 0.6 mmol / g) is obtained;

[0046] When the aldehyde in step a of the above preparation method is 3,5-di-tert-butyl salicylaldehyde, a chitosan Schiff base-loaded divalent copper material CX3@Cu is obtained (the divalent copper content is 0.6 mmol / g as determined by ICP).

[0047] In step a of the above preparation method, no aldehyde is added, only chitosan is added to the acetic acid ethanol solution, and the other steps remain unchanged to obtain a comparative material CX0@Cu (the copper content is 1.6 mmol / g as determined by ICP).

[0048] Example 2

[0049] This embodiment provides a method for synthesizing β-boryl ester by catalysis of a chitosan Schiff base-loaded divalent copper material, comprising the following steps:

[0050] α-propenyl ester compound I, bipyraclostrobin reagent and different catalytic materials chitosan Schiff base loaded divalent copper materials CX1@Cu, CX2@Cu, CX3@Cu and blank control chitosan copper material CX0@Cu (prepared in Example 1) were added into 2 ml of water, wherein α-propenyl ester compound I was 0.3 mmol, bipyraclostrobin reagent was 0.6 mmol, and chitosan Schiff base loaded divalent copper material loaded copper was 0.005 mmol, and the mixture was stirred at room temperature for 16 h. In the α-propenyl ester compound I of this embodiment, R is phenyl;

[0051] After the reaction is completed, the precipitate is filtered, and the obtained precipitate is repeatedly washed and dried with water and ethanol alternately, and the chitosan Schiff base loaded divalent copper material is recycled, and the obtained filtrate is extracted with ethyl acetate three times to obtain an organic phase containing the product, and the water in the system is removed by drying with anhydrous Na2SO4, and the excess organic solvent is removed by filtration and rotary evaporation. The obtained crude product is used as a developing solvent with a volume ratio of petroleum ether / ethyl acetate mixed solvent = 5:1, and column chromatography purification is performed to obtain β-boryl ester compound II (R is phenyl).

[0052]

[0053] CX0@Cu, CX1@Cu, CX2@Cu, and CX3@Cu catalytic materials were used in the reaction, and the final yields were 30%, 80%, 70%, and 74%, respectively.

[0054] After the CX1@Cu catalytic material was used for 5 cycles, it was applied to the boron addition reaction of phenyl methacrylate for the sixth time, and the yield of the obtained product was 78%.

[0055] The NMR hydrogen spectrum and carbon spectrum of the target product are shown below. Figure 1 and Figure 2 :

[0056] 1 H NMR (400MHz, Chloroform-d); δ=7.39-7.22(m,2H),7.22-7.18(m,1H),7.09-7.07(m,2H), 2.96-2.90(m,1H),1.35-1.31(q,3H),1.29-1.27(m,1H),1.24(s,12H),1.11-1.05(m,1H).

[0057] 13 C NMR (100MHz, Chloroform-d); δ=175.80,151.02,129.33,126.58,121.62,83.37,36.59,24.87,24.84,19.40.

[0058] Example 3

[0059] This embodiment provides a method for preparing β-boryl ester by catalysis of a chitosan Schiff base-loaded divalent copper material, comprising the following steps:

[0060] 0.20 mmol of α-propenyl ester compound I, 0.4 mmol of biboric acid pinacol ester, and 0.005 mmol of copper-loaded chitosan Schiff base-loaded divalent copper material CX1@Cu were added into 2.0 ml of water, and the mixture was stirred and reacted at room temperature for 16 h. In this embodiment, the α-propenyl ester compound I is methyl methacrylate (R is methyl);

[0061] After the reaction was completed, the filtrate was filtered and extracted with ethyl acetate three times to obtain an organic phase containing the product, which was dried over anhydrous Na2SO4, filtered, and rotary evaporated to remove excess organic solvent. The crude product was used as a developing solvent with a volume ratio of petroleum ether / ethyl acetate mixed solvent = 6:1, and purified by column chromatography to obtain β-boryl ester compound II, with a product yield of 72%.

[0062]

[0063] The NMR hydrogen spectrum and carbon spectrum of the target product are shown below:

[0064] 1 H NMR (400MHz, Chloroform-d); δ = 3.65 (s, 3H), 2.71-2.66 (q, 1H), 1.22 (s, 6H), 1.20 (s, 6H), 1.19-1.14 (m, 3H), 1.13-1.10 (m, 1H), 0.98-0.90 (m, 1H).

[0065] 13 C NMR (100MHz, Chloroform-d); δ = 177.72, 83.18, 51.58, 25.34, 24.78, 24.71, 19.42.

[0066] The results of this example show that when the CX1@Cu catalytic material provided in Example 1 of the present invention participates in the boron addition reaction, the conversion rate of methyl methacrylate is high, and the yield of the boron addition product thereof reaches 72%.

[0067] Example 4

[0068] This embodiment provides a method for preparing β-boryl ester by catalysis of a chitosan Schiff base-loaded divalent copper material, comprising the following steps:

[0069] 0.20 mmol of α-propenyl ester compound I, 0.4 mmol of biboric acid pinacol ester, and 0.005 mmol of copper-loaded chitosan Schiff base-loaded divalent copper material CX1@Cu were added into 2.0 ml of water, and the mixture was stirred and reacted at room temperature for 16 h. In this embodiment, the α-propenyl ester compound I is butyl methacrylate (R is n-butyl);

[0070] After the reaction was completed, the filtrate was filtered and extracted with ethyl acetate three times to obtain an organic phase containing the product, which was dried over anhydrous Na2SO4, filtered, and rotary evaporated to remove excess organic solvent. The crude product was purified by column chromatography using a mixed solvent of petroleum ether / ethyl acetate in a volume ratio of 7:1 as a developing solvent to obtain β-boryl ester compound II, with a product yield of 81%.

[0071]

[0072] The NMR hydrogen spectrum and carbon spectrum of the target product are shown below:

[0073] 1H NMR (400MHz, Chloroform-d); δ=4.06-3.97(m,2H),2.66-2.60(m,2H),1.60-1.59(m,2H) ),1.39-1.30(m,2H),1.21(s,12H),1.20(s,3H),1.17-1.07(m,1H),0.92-0.86(m,4H).

[0074] 13 C NMR (100MHz, Chloroform-d); δ=177.35,83.11,64.08,35.44,30.72,24.77,24.75,19.39,19.13,13.74.

[0075] The results of this example show that when the CX1@Cu catalytic material provided in Example 1 of the present invention participates in the boron addition reaction, the conversion rate of butyl methacrylate is high, and the yield of the boron addition product thereof reaches 81%.

[0076] Example 5

[0077] This embodiment provides a method for preparing β-boryl ester by catalysis of a chitosan Schiff base-loaded divalent copper material, comprising the following steps:

[0078] 0.20 mmol of α-propenyl ester compound I, 0.4 mmol of biboric acid pinacol ester, and 0.005 mmol of copper-loaded chitosan Schiff base-loaded divalent copper material CX1@Cu were added into 2.0 ml of water, and the mixture was stirred and reacted at room temperature for 16 h. In this embodiment, the α-propenyl ester compound I is lauryl methacrylate (R is dodecyl);

[0079] After the reaction was completed, the filtrate was filtered and extracted with ethyl acetate three times to obtain an organic phase containing the product, which was dried over anhydrous Na2SO4, filtered, and the excess organic solvent was removed by rotary evaporation. The crude product was purified by column chromatography using a mixed solvent of petroleum ether / ethyl acetate in a volume ratio of 15:1 as a developing solvent to obtain a β-boryl ester compound II (R is dodecyl), and the product yield was 84%.

[0080]

[0081] The NMR hydrogen spectrum and carbon spectrum of the target product are shown below:

[0082] 1H NMR (400MHz, Chloroform-d); δ=4.04-4.00(m,1H),2.67-2.62(m,1H),1.61-1.57(m,2H),1.3 1-1.30(m,12H),1.29-1.26(m,8H),1.23-1.21(m,3H),1.18-1.10(m,1H),0.88-0.84(m,2H).

[0083] 13 C NMR (100MHz, Chloroform-d); δ=176.75,83.06,79.55,36.31,28.03,24.79,19.57.

[0084] The results of this example show that when the CX1@Cu catalytic material provided in Example 1 of the present invention participates in the boron addition reaction, the conversion rate of lauryl methacrylate is high, and the yield of its boron addition product reaches 84%.

[0085] Example 6

[0086] This embodiment provides a method for preparing β-boryl ester by catalysis of a chitosan Schiff base-loaded divalent copper material, comprising the following steps:

[0087] 0.20 mmol of α-propenyl ester compound I, 0.4 mmol of biboric acid pinacol ester, and 0.005 mmol of copper-loaded chitosan Schiff base-loaded divalent copper material CX1@Cu were added into 2.0 ml of water, and the mixture was stirred and reacted at room temperature for 16 h. In this embodiment, the α-propenyl ester compound I is tert-butyl methacrylate (R is tert-butyl);

[0088] After the reaction was completed, the filtrate was filtered and extracted with ethyl acetate three times to obtain an organic phase containing the product, which was dried over anhydrous Na2SO4, filtered, and rotary evaporated to remove excess organic solvent. The crude product was purified by column chromatography using a mixed solvent of petroleum ether / ethyl acetate in a volume ratio of 7:1 as a developing solvent to obtain β-boryl ester compound II, with a product yield of 75%.

[0089]

[0090] The NMR hydrogen spectrum and carbon spectrum of the target product are shown below:

[0091] 1 H NMR (400MHz, Chloroform-d); δ=2.55-2.49(m,1H),1.39(s,9H),1.21(s,6H),1.20(s,6H),1.14-1.13(m,3H),1.08-1.02(m,1H),0.87-0.82(m,1H).

[0092] 13 C NMR (100MHz, Chloroform-d); δ=176.75,83.06,79.55,36.31,28.03,24.79,19.57.

[0093] The results of this example show that when the CX1@Cu catalytic material provided in Example 1 of the present invention participates in the boron addition reaction, the conversion rate of tert-butyl methacrylate is high, and the yield of the boron addition product thereof reaches 75%.

[0094] Example 7

[0095] This embodiment provides a method for preparing β-boryl ester by catalysis of a chitosan Schiff base-loaded divalent copper material, comprising the following steps:

[0096] 0.20 mmol of α-propenyl ester compound I, 0.4 mmol of bipyraclostrobin, and 0.005 mmol of copper-loaded chitosan Schiff base-loaded divalent copper material CX1@Cu were added into 2.0 ml of water, and the mixture was stirred and reacted at room temperature for 16 h. In this embodiment, the α-propenyl ester compound I is 2-methoxyethyl methacrylate (R is 2-methoxyethyl);

[0097] After the reaction was completed, the filtrate was filtered and extracted with ethyl acetate three times to obtain an organic phase containing the product, which was dried over anhydrous Na2SO4, filtered, and rotary evaporated to remove excess organic solvent. The crude product was purified by column chromatography using a mixed solvent of petroleum ether / ethyl acetate in a volume ratio of 8:1 as a developing solvent to obtain β-boryl ester compound II, with a product yield of 74%.

[0098]

[0099] The NMR hydrogen spectrum and carbon spectrum of the target product are shown below:

[0100] 1 H NMR (400MHz, Chloroform-d); δ=4.23-4.14(m,2H),3.59-3.53(m,2H),3.36(s,3H),2.7 2-2.67(m,1H),1.21(s,12H),1.18-1.14(m,3H),1.11-1.10(m,1H),0.94-0.89(m,1H).

[0101] 13 C NMR (100MHz, Chloroform-d); δ=177.38,83.17,70.55,63.38,59.02,35.28,24.78,24.76,19.30.

[0102] The results of this example show that when the CX1@Cu catalytic material provided in Example 1 of the present invention participates in the boron addition reaction, the conversion rate of 2-methoxyethyl methacrylate is high, and the yield of its boron addition product reaches 74%.

Claims

1. Preparation of a chitosan Schiff base-loaded divalent copper material in catalysis β - application of a boryl ester compound, characterized in that The specific application steps include: 1) Use the substrate α -propylene ester compound I, biboric acid pinacol ester as a boron source, and chitosan Schiff base loaded divalent copper material CX@Cu as a catalyst were added into pure water, mixed and stirred at room temperature for 8-16 h, wherein α - The molar ratio of the propenyl ester compound I, the bipyraclostrobin and the copper loaded by CX@Cu is 1:(1-2):(0.01-0.05), The chemical reaction equation is as follows: , Wherein, R is phenyl, methyl, n-butyl, dodecyl, tert-butyl, 2-methoxyethyl; 2) After the reaction is completed, the reaction is filtered, and the solid phase is washed, centrifuged, and dried to obtain the recovered chitosan Schiff base-loaded divalent copper material CX@Cu, which is recycled for the next reaction; the obtained liquid phase is separated and purified to obtain β -boryl ester compound II; The chitosan Schiff base-loaded divalent copper material CX@Cu is prepared by a method comprising the following steps: a. Mix glacial acetic acid and anhydrous ethanol in a volume ratio of 1:5-8 to obtain an acetic acid ethanol solution, add chitosan and an aldehyde compound to the acetic acid ethanol solution, and react at 25-50°C with stirring for 8-16 hours, wherein the aldehyde is one of 2-quinolinecarboxaldehyde, 5-bromosalicylaldehyde, and 3,5-di-tert-butylsalicylaldehyde, and the molar ratio of amino group -NH2 in chitosan to aldehyde group -CHO in the aldehyde compound is 1:3-4; b. After the reaction is completed, the chitosan Schiff base material is separated, washed and dried to obtain a powder; c. Place the chitosan Schiff base material in a copper sulfate solution. The copper sulfate solution contains Cu 2+ The molar ratio of amino-NH2 in chitosan is at least 1:1, the concentration of copper ions in the copper sulfate solution is 0.16-0.24 mol / L, and the reaction is stirred at 25-50 °C for 8-16 h to promote the adsorption of divalent copper ions; d. After the adsorption is completed, the chitosan Schiff base loaded divalent copper material CX@Cu is obtained by separation, washing and drying.

2. The chitosan Schiff base-loaded divalent copper material as claimed in claim 1 is used in the catalytic preparation β - application of a boryl ester compound, characterized in that The copper content in the material CX@Cu in step 1) is 0.6~1.6 mmol / g.

3. The chitosan Schiff base-loaded divalent copper material as claimed in claim 1 is used in the catalytic preparation β - application of a boryl ester compound, characterized in that Step 1) α -The molar ratio of propenyl ester compound I, bipyraclostrobin and copper loaded by CX@Cu material is 1:2:0.0167~0.

025.

4. The chitosan Schiff base-loaded divalent copper material as claimed in claim 1 is used in the catalytic preparation β - application of a boryl ester compound, characterized in that Step 1) The ratio of copper loading to water in the chitosan Schiff base copper functional material CX@Cu is 0.005 mmol:1~2 ml.

5. The chitosan Schiff base-loaded divalent copper material as claimed in claim 1 is used in the catalytic preparation β - application of a boryl ester compound, characterized in that In step 1), the mixture was stirred and reacted at room temperature for 16 h.

6. The chitosan Schiff base-loaded divalent copper material according to claim 1 is used in the catalytic preparation β - application of a boryl ester compound, characterized in that The filtrate obtained in step 2) is separated and purified to obtain β -boryl ester compound II specifically comprises: extracting the filtrate with ethyl acetate to obtain an organic phase containing the product, then drying with anhydrous Na2SO4, filtering, and rotary evaporation to remove excess organic solvent, and purifying the obtained crude product with a mixed solvent column chromatography of ethyl acetate and petroleum ether to obtain β -Boryl ester compound II.

7. The chitosan Schiff base-loaded divalent copper material as claimed in claim 1 is used in the catalytic preparation β - application of a boryl ester compound, characterized in that In step a, glacial acetic acid and anhydrous ethanol are mixed in a volume ratio of 1:7.5 to obtain an acetic acid ethanol solution, and the molar ratio of amino group -NH2 in chitosan to aldehyde group -CHO in the aldehyde compound is 1:

4.

8. The chitosan Schiff base-loaded divalent copper material as claimed in claim 1 is used in the catalytic preparation β - application of a boryl ester compound, characterized in that The separation, washing and drying in steps b and d both include: after filtering, washing the obtained solid phase with water and ethanol repeatedly and alternately, and drying in an oven at 50° C. for 12 h.