Polyphenylene sulfide resin composition for automobile cooling parts and automobile cooling parts
By combining glass fiber and specific silane compounds in PPS resin, and performing thermal pressurization and thermal oxidation treatments, the problems of mechanical strength, antifreeze resistance, and mold scale inhibition in automotive cooling components are solved, achieving an efficient solution.
Patent Information
- Application Number
- CN202080078775.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-19
- Filing Date
- 2020-11-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-11-18
AI Technical Summary
It is difficult for existing PPS resins to simultaneously meet the requirements of high mechanical strength, antifreeze resistance and mold scale inhibition in automotive cooling parts, especially in complex shapes and multi-part combinations.
Using a combination of polyphenylene sulfide resin, glass fiber and silane compound with specific functional groups, through hot pressure filtration and thermal oxidation treatment, a PPS resin with high mechanical strength and antifreeze resistance is prepared, and through a specific process Conditions such as heat treatment and acid treatment inhibit the generation of mold scale.
It achieves significant improvements in high mechanical strength and antifreeze resistance, while effectively suppressing the generation of mold scale. It is suitable for automotive cooling components with complex shapes and multi-component combinations.
Smart Images

Figure GDA0003640251040000041 
Figure GDA0003640251040000051 
Figure GDA0003640251040000341
Abstract
Description
Technical Field
[0001] The present invention provides a PPS resin composition for automobile cooling parts which has extremely excellent antifreeze resistance while maintaining high mechanical strength and suppresses the generation of mold scale (deposits attached to the mold surface), and an automobile cooling part obtained by injection molding. Background Art
[0002] Polyphenylene sulfide resin (hereinafter, PPS resin) has well-balanced rigidity, heat resistance, hot water resistance, chemical resistance, and molding processability, and is therefore widely used in electrical / electronic parts, water supply parts, and automobile parts.
[0003] In these applications, mechanical strength is required, and PPS resin compositions have been proposed in which PPS resin is reinforced with glass fiber and a silane compound having a functional group such as an epoxy group is blended.
[0004] As the number of components installed in recent years has increased, there is a strong demand for space saving in the engine compartment. As a result, each component has been miniaturized, and development has shifted to modules that combine multiple components instead of a single component to integrate multiple functions. As a result, high mechanical strength is required to achieve thinner walls and complex shapes.
[0005] In addition, in automobile cooling parts, liquids such as antifreeze flow in contact with the inner wall surface, so PPS resin compositions with excellent antifreeze resistance are used. However, as products become more high-performance, they are exposed to more severe environments, and thus higher antifreeze resistance than ever before is required.
[0006] On the other hand, PPS resin has a high melting point and is therefore excellent in heat resistance, but on the other hand, the processing temperature during injection molding is high, so there are problems such as mold deposits caused by PPS resin and additives, poor appearance of molded products, reduced dimensional accuracy, and reduced productivity due to disassembly and cleaning of the mold.
[0007] In particular, automobile cooling parts are mounted on a large number of automobiles from the viewpoint of improving the fuel efficiency of the engine and optimizing the battery performance, and improving the yield and productivity have become major issues.
[0008] Therefore, there is a demand for a PPS resin composition for automobile cooling parts which has hot water resistance and antifreeze resistance in addition to mechanical strength and suppresses the generation of mold deposits.
[0009] Prior art literature
[0010] Patent Literature
[0011] For example, Patent Documents 1 and 2 disclose PPS resin compositions in which a straight-chain PPS resin is reinforced with glass fibers and a silane compound is mixed. In addition, Patent Document 3 discloses a PPS resin composition in which glass fibers and a silane compound are mixed with a PPS resin obtained by polymerizing a low-water-containing alkali metal sulfide that has undergone a specific treatment in an organic polar solvent with a dihalogenated aromatic compound. In addition, Patent Document 4 discloses a PPS resin composition in which glass fibers and a silane compound are mixed with a PPS resin obtained by mixing a high-molecular-weight PPS resin having a cross-linked structure and a low-molecular-weight PPS resin that does not have a cross-linked structure.
[0012] Patent Document 1: Japanese Patent Application Publication No. 2011-153242
[0013] Patent Document 2: Japanese Patent Application Publication No. 2010-195874
[0014] Patent Document 3: Japanese Patent Application Publication No. 2006-219666
[0015] Patent Document 4: Japanese Patent Application Laid-Open No. 6-41425 Summary of the invention
[0016] Problems to be solved by the invention
[0017] However, in Patent Documents 1 and 2, although mechanical strength is described, no specific study on antifreeze resistance is conducted, and the generation of mold scale is not satisfactory. In Patent Document 3, although mechanical strength is described, no specific study on antifreeze resistance is conducted, and the antifreeze resistance is not satisfactory. In addition, in Patent Document 4, although mechanical strength is described, no specific study on antifreeze resistance is conducted, and the effects of antifreeze resistance and generation of mold scale are not satisfactory.
[0018] The present invention provides a PPS resin composition for automobile cooling parts which has extremely excellent antifreeze resistance while maintaining high mechanical strength and suppresses the generation of mold deposits, and an automobile cooling part obtained by injection molding.
[0019] Means for solving problems
[0020] The polyphenylene sulfide resin composition for automobile cooling parts of the present invention has the following structure in order to solve the above-mentioned problems. That is,
[0021] A polyphenylene sulfide resin composition for automobile cooling parts, comprising: (A) 100 parts by weight of a polyphenylene sulfide resin; (B) 30 to 110 parts by weight of a glass fiber; and (C) 0.1 to 3 parts by weight of a silane compound having any functional group selected from an amino group and an isocyanate group; wherein the polyphenylene sulfide resin (A) has a number average molecular weight of 7,000 to 14,000; and when the polyphenylene sulfide resin (A) is dissolved in 20 times the weight of 1-chloronaphthalene at 250° C. for 5 minutes and then hot-pressed filtered using a PTFE membrane filter having a pore size of 1 μm, the residual amount is 2.0 to 5.0% by weight.
[0022] The automobile cooling component of the present invention has the following structure. That is,
[0023] An automobile cooling component is made of the polyphenylene sulfide resin composition.
[0024] The polyphenylene sulfide resin composition for automobile cooling parts of the present invention preferably has a melting crystallization peak temperature of 230° C. or higher.
[0025] The polyphenylene sulfide resin composition for automobile cooling parts of the present invention preferably satisfies all of the following conditions (i) and (ii).
[0026] (i) A type A1 test piece specified in ISO 20753 (hereinafter referred to as an ISO test piece) obtained by injection molding the polyphenylene sulfide resin composition has a tensile strength of 190 MPa or more as measured in accordance with ISO 527-1 or 527-2 at a tensile speed of 5 mm / min and an ambient temperature of 23°C.
[0027] (ii) After the ISO test piece is immersed in an antifreeze solution at 150°C for 500 hours, the retention rate of tensile strength measured according to ISO 527-1 or 527-2 at a tensile speed of 5 mm / min and an ambient temperature of 23°C is 80% or more.
[0028] The automobile cooling component of the present invention is preferably a combination of a housing and at least two tubes, wherein the housing is formed by injection molding the polyphenylene sulfide resin composition.
[0029] The automotive cooling component of the present invention is preferably a combination of a housing, a valve, and at least three pipes, wherein the housing is formed by injection molding the polyphenylene sulfide resin composition.
[0030] Effects of the Invention
[0031] The inventors of the present invention have found that a polyphenylene sulfide resin composition has high mechanical strength and antifreeze resistance and also suppresses the generation of mold deposit, which is an unknown characteristic. The polyphenylene sulfide resin composition is a mixture of a PPS resin, a glass fiber, and a silane compound having a specific functional group, wherein the number average molecular weight of the PPS resin is 7,000 to 14,000, and the PPS resin has a residual amount of 2.0 to 5.0% by weight when dissolved in 20 times the weight of 1-chloronaphthalene at 250° C. for 5 minutes and hot-pressed filtered using a PTFE membrane filter having a pore size of 1 μm. The PPS resin composition of the present invention is useful for automotive cooling parts, and is particularly useful for automotive cooling parts having a small / complex shape in which a plurality of parts are combined. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The schematic diagrams of automobile cooling components are composed of a housing and at least two tubes. (a) is a diagram viewed from above, and (b) is a diagram viewed from the side.
[0033] Figure 2 A schematic diagram of an automotive cooling component that combines a housing, a valve, and at least three tubes.
[0034] Figure 3 The following are schematic diagrams of molded articles for evaluating mold contamination. (a) is a diagram observed from above, and (b) is a diagram observed from the side. DETAILED DESCRIPTION
[0035] Hereinafter, embodiments of the present invention will be described. In the present invention, "weight" means "mass".
[0036] Since the resin composition of the present invention needs to have heat resistance, it is a composition containing a polyphenylene sulfide resin (hereinafter referred to as a PPS resin).
[0037] The (A) PPS resin used in the present invention is a polymer having a repeating unit represented by the following structural formula:
[0038]
[0039] From the viewpoint of heat resistance, the polymer preferably contains 70 mol% or more, and further 90 mol% or more of the repeating unit represented by the above structural formula. In addition, the PPS resin may be composed of repeating units having the following structure in which less than about 30 mol% of its repeating units are composed.
[0040]
[0041] Hereinafter, the contents of the polyhalogenated aromatic compound, the sulfidizing agent, the polymerization solvent, the molecular weight modifier, the polymerization aid, and the polymerization stabilizer used in the production method of the present invention will be described.
[0042] [Polyhalogenated aromatic compounds]
[0043] The so-called polyhalogenated aromatic compound refers to a compound having two or more halogen atoms in one molecule. As a specific example, polyhalogenated aromatic compounds such as p-dichlorobenzene, m-dichlorobenzene, o-dichlorobenzene, 1,3,5-trichlorobenzene, 1,2,4-trichlorobenzene, 1,2,4,5-tetrachlorobenzene, hexachlorobenzene, 2,5-dichlorotoluene, 2,5-dichloro-p-xylene, 1,4-dibromobenzene, 1,4-diiodobenzene, 1-methoxy-2,5-dichlorobenzene can be cited, and p-dichlorobenzene is preferably used. In addition, two or more different polyhalogenated aromatic compounds can also be combined to form a copolymer, but it is preferred to use a p-dihalogenated aromatic compound as the main component.
[0044] From the viewpoint of obtaining a PPS resin having a viscosity suitable for processing, the amount of the polyhalogenated aromatic compound used is, for example, in the range of 0.9 to 2.0 mol, preferably 0.95 to 1.5 mol, and more preferably 1.005 to 1.2 mol per 1 mol of the vulcanizing agent.
[0045] [Vulcanizing agent]
[0046] Examples of the sulfidizing agent include alkali metal sulfides, alkali metal hydrosulfides, and hydrogen sulfide.
[0047] Specific examples of alkali metal sulfides include lithium sulfide, sodium sulfide, potassium sulfide, rubidium sulfide, cesium sulfide, and mixtures of two or more thereof, of which sodium sulfide is preferably used. These alkali metal sulfides may be used in the form of hydrates, aqueous mixtures, or anhydrides.
[0048] Specific examples of alkali metal hydrosulfides include sodium hydrosulfide, potassium hydrosulfide, lithium hydrosulfide, rubidium hydrosulfide, cesium hydrosulfide, and mixtures of two or more thereof, among which sodium hydrosulfide is preferably used. These alkali metal hydrosulfides may be used in the form of hydrates, aqueous mixtures, or anhydrides.
[0049] Alternatively, a sulfiding agent prepared in situ in the reaction system from an alkali metal hydrosulfide and an alkali metal hydroxide may be used. Alternatively, a sulfiding agent prepared from an alkali metal hydrosulfide and an alkali metal hydroxide may be used after being transferred to a polymerization tank.
[0050] Alternatively, a sulfiding agent prepared in situ in the reaction system from an alkali metal hydroxide such as lithium hydroxide or sodium hydroxide and hydrogen sulfide may be used. Alternatively, a sulfiding agent prepared from an alkali metal hydroxide such as lithium hydroxide or sodium hydroxide and hydrogen sulfide may be transferred to a polymerization tank for use.
[0051] When a part of the sulfiding agent is lost before the start of the polymerization reaction due to a dehydration operation or the like, the amount of the sulfiding agent added means the residual amount obtained by subtracting the lost part from the actual amount added.
[0052] It should be noted that, an alkali metal hydroxide and / or an alkaline earth metal hydroxide may also be used together with a sulfiding agent. As a specific example of the alkali metal hydroxide, for example, sodium hydroxide, potassium hydroxide, lithium hydroxide, rubidium hydroxide, cesium hydroxide and a mixture of two or more thereof may be cited as a preferred specific example, and as a specific example of the alkaline earth metal hydroxide, for example, calcium hydroxide, magnesium hydroxide, strontium hydroxide, barium hydroxide, etc. may be cited, wherein sodium hydroxide is preferably used.
[0053] When an alkali metal hydrosulfide is used as the sulfiding agent, it is particularly preferred to use an alkali metal hydroxide simultaneously. The amount used is, for example, in the range of 0.95 to 1.20 mol, preferably 1.00 to 1.15 mol, and more preferably 1.005 to 1.100 mol per 1 mol of the alkali metal hydrosulfide.
[0054] [Polymerization solvent]
[0055] As a polymerization solvent, an organic polar solvent is preferably used. As a specific example, N- methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone and other N- alkylpyrrolidones, N-methyl-ε-caprolactam and other caprolactams, 1,3-dimethyl-2-imidazolidinone, N,N- dimethylacetamide, N,N- dimethylformamide, hexamethylphosphoric triamide, dimethyl sulfone, tetramethylene sulfoxide and the like are represented by aprotic organic solvents and mixtures thereof, and they are all preferably used because of the high stability of the reaction. Among them, N- methyl-2-pyrrolidone (hereinafter, sometimes abbreviated as NMP) is particularly preferably used.
[0056] The amount of the organic polar solvent used is preferably selected within the range of 2.0 to 10 mol, more preferably 2.25 to 6.0 mol, and even more preferably 2.5 to 5.5 mol per 1 mol of the sulfiding agent.
[0057] [Molecular weight regulator]
[0058] In order to form the terminals of the produced PPS resin or to adjust the polymerization reaction, molecular weight, etc., a monohalogenated compound (which may not necessarily be an aromatic compound) may be used together with the above-mentioned polyhalogenated aromatic compound.
[0059] [Polymerization aid]
[0060] It is also one of the preferred schemes to use a polymerization aid in order to obtain a PPS resin with a relatively high degree of polymerization in a short time. Here, the so-called polymerization aid refers to a substance that has the effect of increasing the viscosity of the obtained PPS resin. As specific examples of such polymerization aids, for example, organic carboxylic acid metal salts, water, alkali metal chlorides, organic sulfonates, alkali metal sulfates, alkaline earth metal oxides, alkali metal phosphates and alkaline earth metal phosphates can be cited. They can be used alone, and more than two kinds can also be used simultaneously. Among them, organic carboxylic acid metal salts and / or water are preferably used.
[0061] The organic carboxylic acid metal salts are of the general formula R(COOM) n (wherein, R is an alkyl group, cycloalkyl group, aryl group, alkylaryl group or arylalkyl group having 1 to 20 carbon atoms. M is an alkali metal selected from lithium, sodium, potassium, rubidium and cesium. n is an integer of 1 to 3.) The organic carboxylic acid metal salt can also be used in the form of a hydrate, anhydride or an aqueous solution. Specific examples of the organic carboxylic acid metal salt include, for example, lithium acetate, sodium acetate, potassium acetate, sodium propionate, lithium valerate, sodium benzoate, sodium phenylacetate, potassium p-toluate, and mixtures thereof.
[0062] The organic carboxylic acid metal salt can also be formed by adding an organic acid and one or more compounds selected from alkali metal hydroxides, alkali metal carbonates and alkali metal hydrogen carbonates in substantially equal chemical equivalents and reacting them. Among the above-mentioned organic carboxylic acid metal salts, sodium acetate is most preferably used because it is inexpensive and has moderate solubility in the polymerization system.
[0063] When these polymerization aids are used, the amount used is usually in the range of 0.01 to 0.7 mol, preferably 0.1 to 0.6 mol, more preferably 0.2 to 0.5 mol, based on 1 mol of the alkali metal sulfide added, in order to obtain a higher degree of polymerization.
[0064] In addition, using water as a polymerization aid is one of the effective means for obtaining a resin composition with a high balance between fluidity and high toughness. In this case, the amount added is usually in the range of 0.5 mol to 15 mol per 1 mol of the added alkali metal sulfide, preferably in the range of 0.6 to 10 mol, and more preferably in the range of 1 to 5 mol in order to obtain a higher degree of polymerization.
[0065] The addition time of these polymerization aids is not particularly specified, and they can be added at any time during the pre-process described below, at the start of polymerization, or during the polymerization. In addition, they can be added in multiple times, but when an organic carboxylic acid metal salt is used as a polymerization aid, it is more preferable to add them simultaneously during the pre-process or at the start of polymerization from the perspective of ease of addition. In addition, when water is used as a polymerization aid, it is effective to add it during the polymerization reaction after adding a polyhalogenated aromatic compound.
[0066] [Polymerization stabilizer]
[0067] In order to stabilize the polymerization reaction system and prevent side reactions, a polymerization stabilizer can also be used. The polymerization stabilizer contributes to the stabilization of the polymerization reaction system and inhibits undesirable side reactions. As a criterion for side reactions, the generation of thiophenol can be cited, and the generation of thiophenol can be inhibited by the addition of a polymerization stabilizer. As specific examples of polymerization stabilizers, compounds such as alkali metal hydroxides, alkali metal carbonates, alkaline earth metal hydroxides, and alkaline earth metal carbonates can be cited. Among them, alkali metal hydroxides such as sodium hydroxide, potassium hydroxide, and lithium hydroxide are preferred. Since the above-mentioned organic carboxylic acid metal salt also acts as a polymerization stabilizer, it becomes a kind of polymerization stabilizer used in the present invention. In addition, when using alkali metal hydrosulfide as a sulfiding agent, it is described above that it is particularly preferred to use alkali metal hydroxide at the same time, and the alkali metal hydroxide that becomes excessive relative to the sulfiding agent can also become a polymerization stabilizer.
[0068] These polymerization stabilizers can be used alone or in combination of two or more. The polymerization stabilizer is preferably used in a ratio of usually 0.02 to 0.2 mol, preferably 0.03 to 0.1 mol, and more preferably 0.04 to 0.09 mol relative to 1 mol of the added alkali metal sulfide. If it is within the above preferred range, the stabilization effect is sufficient, and on the other hand, it is economically advantageous and can increase the polymer yield.
[0069] There is no particular restriction on the timing of adding the polymerization stabilizer. It can be added at any time during the pre-process described below, at the start of polymerization, or during polymerization. It can also be added in multiple times. However, it is more preferable to add it simultaneously during the pre-process or at the start of polymerization from the perspective of convenience.
[0070] Next, the pre-step, the polymerization reaction step, and the recovery step will be specifically described in order.
[0071] [Pre-process]
[0072] The sulfiding agent is usually used in the form of a hydrate, but it is preferred that the mixture containing the organic polar solvent and the sulfiding agent is heated before adding the polyhalogenated aromatic compound to remove excess water outside the system. It should be noted that, in the case where water is excessively removed by this operation, it is preferred to add water to supplement the insufficient amount.
[0073] In addition, as described above, as a sulfiding agent, an alkali metal sulfide prepared from an alkali metal hydrosulfide and an alkali metal hydroxide in situ in the reaction system or in a tank different from the polymerization tank can also be used. There is no particular limitation on the method, and examples include a method in which an alkali metal hydrosulfide and an alkali metal hydroxide are added to an organic polar solvent in an inert gas atmosphere at a temperature range of room temperature to 150°C, preferably room temperature to 100°C, and the temperature is raised to at least 150°C, preferably 180 to 260°C, under normal pressure or reduced pressure to distill off water. A polymerization aid can also be added at this stage. In addition, toluene or the like can be added to react in order to promote the distillation of water.
[0074] The amount of water in the polymerization system during the polymerization reaction is preferably 0.5 to 10.0 moles per 1 mole of the added sulfidizing agent. The amount of water in the polymerization system here is the amount obtained by subtracting the amount of water removed from the polymerization system from the amount of water added to the polymerization system. In addition, the water added can be in any form such as water, aqueous solution, crystal water, etc.
[0075] [Polymerization reaction step]
[0076] The PPS resin is preferably produced by reacting a vulcanizing agent with a polyhalogenated aromatic compound in an organic polar solvent at a temperature ranging from 200 to 290°C.
[0077] When starting the polymerization reaction step, it is desirable to add a sulfiding agent and a polyhalogenated aromatic compound to an organic polar solvent in an inert gas atmosphere at room temperature to 220° C., preferably in a temperature range of 100 to 220° C. A polymerization aid may also be added at this stage. The order of adding these raw materials is not particularly limited and they may be added simultaneously.
[0078] Such a mixture is usually heated to a temperature in the range of 200° C. to 290° C. The heating rate is not particularly limited, but is usually selected from a range of 0.01 to 5° C. / min, more preferably 0.1 to 3° C. / min.
[0079] Generally, the temperature is finally raised to 250 to 290° C. and the reaction is usually carried out at this temperature for 0.25 to 50 hours, preferably 0.5 to 20 hours.
[0080] In the stage before reaching the final temperature, for example, a method of reacting at 200° C. to 260° C. for a certain period of time and then raising the temperature to 270 to 290° C. is effective in obtaining a higher degree of polymerization. In this case, the reaction time at 200° C. to 260° C. is usually selected in the range of 0.25 to 20 hours, preferably in the range of 0.25 to 10 hours.
[0081] It should be noted that in order to obtain a polymer with a higher degree of polymerization, it is effective to perform polymerization in multiple stages. When performing polymerization in multiple stages, it is effective to transfer to the next stage when the conversion rate of the polyhalogenated aromatic compound in the system at 245° C. reaches 40 mol % or more, preferably 60 mol %.
[0082] [Recycling process]
[0083] After the polymerization is completed, a solid substance is recovered from the polymerization reaction product including the polymer, the solvent, and the like.
[0084] The preferred recovery method of PPS resin is to carry out under quenching conditions. As a preferred recovery method, the flash method can be cited. The so-called flash method is to condense the polymerized reactants under high temperature and high pressure (usually above 250°C and 8kg / cm 2 The flash evaporation is a method of flashing a polymer in a state of normal pressure or reduced pressure to recover the solvent and the polymer in a powdery state. Here, the flash evaporation means that the polymer reactant is ejected from a nozzle. Specifically, the atmosphere for flash evaporation can be nitrogen or water vapor at normal pressure, and the temperature is usually selected in the range of 150°C to 250°C.
[0085] Flash evaporation can recover solid matter while recovering solvent, and the recovery time can be relatively short, so it is an economically excellent recovery method. For this recovery method, there is a tendency that ionic compounds represented by Na and organic low-polymerization degree products (oligomers) are easily introduced into the polymer during the solidification process.
[0086] However, the recovery method of the PPS resin used in the manufacturing method of the present invention is not limited to the flash method, and as long as the method satisfies the requirements of the present invention, a method (quench method) of slowly cooling and recovering a polymer in a particulate state may also be used. However, in view of economic efficiency, it is more preferable to use a PPS resin recovered by the flash method.
[0087] [Post-processing process]
[0088] In the present invention, it is important to subject the PPS resin obtained through the above-mentioned polymerization reaction step and recovery step to acid treatment.
[0089] The acid used for the acid treatment in the present invention is not particularly limited as long as it does not decompose the PPS resin, and examples thereof include acetic acid, hydrochloric acid, sulfuric acid, phosphoric acid, silicic acid, carbonic acid, and propyl acid, among which acetic acid and hydrochloric acid are more preferably used.
[0090] The water used in preparing the acid aqueous solution is preferably distilled water or deionized water. The acid aqueous solution preferably has a pH of 1 to 7, more preferably a pH of 2 to 4. If the pH is in the above preferred range, the metal content of the PPS resin can be prevented from increasing, and on the other hand, the volatile components of the PPS resin can be prevented from increasing.
[0091] The method of acid treatment is preferably to immerse the PPS resin in an acid or an aqueous solution of an acid, and it may be stirred and heated appropriately as needed. The temperature during heating is preferably 80 to 250°C, more preferably 120 to 200°C, and further preferably 150 to 200°C. If the temperature during heating is within the above-mentioned preferred range, the acid treatment effect is sufficient to prevent the metal content from increasing. On the other hand, the pressure will not be too high, which is preferred in terms of safety. In addition, the pH when the PPS resin is treated by immersing it in an aqueous solution of an acid is preferably less than 8 by acid treatment, and more preferably pH 2 to 8. If the pH when the PPS resin is treated by immersing it in an aqueous solution of an acid is within the above-mentioned preferred range, the metal content of the resulting PPS resin can be prevented from increasing.
[0092] The acid treatment time is preferably a time period that allows the reaction between the PPS resin and the acid to reach a sufficient equilibrium, preferably 2 to 24 hours when the treatment is performed at 80° C., and preferably 0.01 to 5 hours when the treatment is performed at 200° C.
[0093] Regarding the ratio of the PPS resin to the acid or the acid aqueous solution in the acid treatment, it is preferred to perform the treatment while the PPS resin is fully immersed in the acid or the acid aqueous solution, and the acid or the acid aqueous solution is preferably 0.5 to 500 L, more preferably 1 to 100 L, and even more preferably 2.5 to 20 L relative to 500 g of the PPS resin. If the acid or the acid aqueous solution is within the above preferred range relative to 500 g of the PPS resin, the PPS resin can be fully immersed in the acid or the acid aqueous solution and washed well, and the metal content of the PPS resin can be prevented from increasing. On the other hand, the amount of the acid or the acid aqueous solution relative to the PPS resin is appropriate, and the production efficiency can be improved.
[0094] The above-mentioned acid treatment is carried out by a method of adding a specified amount of PPS resin to a specified amount of water and acid, heating / stirring in a pressure vessel, or continuously carrying out the acid treatment. In the method of separating the acid or the aqueous solution of the acid and the PPS resin from the treatment solution after the acid treatment, filtration using a sieve or a filter is simple, and examples thereof include natural filtration, pressure filtration, reduced pressure filtration, centrifugal filtration, and the like. In order to remove the acid and impurities remaining on the surface of the PPS resin separated from the treatment solution, it is preferably washed with water or warm water several times. The washing method can be exemplified by a method of filtering and washing while applying water to the PPS resin on the filter device, and a method of separating the aqueous solution from the PPS resin and washing by filtering again after adding the separated PPS resin to the pre-prepared water. The water used for washing is preferably distilled water or deionized water. It can be considered that the structure of the terminal of the PPS resin treated with acid in this way changes, but it is difficult to express the structure of the PPS resin obtained by acid treatment with a general formula, and it is also difficult to specify it by characteristics, so it can only be specified by the process (acid treatment) used to obtain the PPS resin.
[0095] In the present invention, it is preferred to perform hot water treatment before the step of acid treatment, and the method is as follows. The water used for the hot water treatment in the present invention is preferably distilled water or deionized water. The hot water treatment temperature is preferably 80 to 250°C, more preferably 120 to 200°C, and further preferably 150 to 200°C. If the hot water treatment temperature is within the above-mentioned preferred range, the hot water treatment effect is excellent, the amount of volatile gas generated can be reduced, and on the other hand, the pressure will not be too high, which is preferred in terms of safety.
[0096] The hot water treatment time is preferably a time sufficient for extraction of the PPS resin with hot water, preferably 2 to 24 hours when treated at 80° C., and preferably 0.01 to 5 hours when treated at 200° C.
[0097] Regarding the ratio of PPS resin to water in the hot water treatment, it is preferred to treat the PPS resin in a state where the PPS resin is fully immersed in water. The amount of water is preferably 0.5 to 500 L, more preferably 1 to 100 L, and even more preferably 2.5 to 20 L relative to 500 g of PPS resin. If the amount of water is less than 0.5 L relative to 500 g of PPS resin, the PPS resin will not be fully immersed in water, so washing will be poor, and the amount of volatile gas generated will increase, which is not preferred. In addition, if the amount of water exceeds 500 L relative to 500 g of PPS resin, the amount of water relative to the PPS resin will become greatly excessive, and the production efficiency will be significantly reduced, which is not preferred.
[0098] There are no particular restrictions on the operation of these hot water treatments, and they can be carried out by adding a specified amount of PPS resin to a specified amount of water, heating / stirring in a pressure vessel, continuously implementing hot water treatment, etc. There are no particular restrictions on the method of separating the aqueous solution and the PPS resin from the treatment solution after hot water treatment, but filtering using a sieve or a filter is simple, and examples include natural filtration, pressure filtration, reduced pressure filtration, centrifugal filtration, etc. In order to remove impurities remaining on the surface of the PPS resin separated from the treatment solution, it is preferably washed with water or warm water several times. There are no particular restrictions on the washing method, and examples include a method of washing by filtering while applying water to the PPS resin on the filter device, a method of filtering again after adding the separated PPS resin to pre-prepared water, and the like to separate the aqueous solution from the PPS resin and wash. The water used for washing is preferably distilled water or deionized water.
[0099] In addition, it is not preferred that the PPS terminal group decomposes during these acid treatments and hot water treatments, so it is desirable to implement the acid treatment and hot water treatment under an inert atmosphere. As the inert atmosphere, nitrogen, helium, argon, etc. can be cited, but from the viewpoint of economic efficiency, a nitrogen atmosphere is preferred.
[0100] In the present invention, the step of washing the PPS resin with an organic solvent may be included before the step of subjecting the PPS resin to an acid treatment or the step of subjecting the PPS resin to a hot water treatment, and the method is as follows. In the present invention, the organic solvent used for washing the PPS resin is not particularly limited as long as it does not have the effect of decomposing the PPS resin, and examples thereof include nitrogen-containing polar solvents such as N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, 1,3-dimethylimidazolidinone, hexamethylphosphoramide, and piperazinone, sulfoxide / sulfone solvents such as dimethyl sulfoxide, dimethyl sulfone, and cyclopentane, ketone solvents such as acetone, methyl ethyl ketone, diethyl ketone, and acetophenone, and dimethyl ether, dipropyl ether, and dimethicone. The organic solvents include ether solvents such as alkane and tetrahydrofuran, chloroform, dichloromethane, trichloroethylene, 1,2-dichloroethane, perchloroethylene, monochloroethane, dichloroethane, tetrachloroethane, perchloroethane, halogen solvents such as chlorobenzene, methanol, ethanol, propanol, butanol, amyl alcohol, ethylene glycol, propylene glycol, phenol, cresol, polyethylene glycol, polypropylene glycol and alcohol / phenol solvents and aromatic hydrocarbon solvents such as benzene, toluene and xylene. Among these organic solvents, N-methyl-2-pyrrolidone, acetone, dimethylformamide and chloroform are particularly preferably used. In addition, these organic solvents can be used alone or in combination of two or more.
[0101] As a method of washing with an organic solvent, there are methods such as immersing the PPS resin in an organic solvent, and stirring or heating can also be performed as needed. There is no particular restriction on the washing temperature when washing the PPS resin with an organic solvent, and any temperature between room temperature and about 300°C can be selected. There is a tendency that the higher the washing temperature, the higher the washing efficiency, but generally a sufficient effect can be obtained at a washing temperature of room temperature to 150°C. It is also possible to wash under pressure in a pressure vessel at a temperature above the boiling point of the organic solvent. In addition, there is no particular restriction on the washing time. It is related to the washing conditions. In the case of intermittent washing, a sufficient effect can usually be obtained by washing for more than 5 minutes. In addition, washing can also be performed continuously.
[0102] These acid treatments, hot water treatments, and washing with organic solvents may be performed in appropriate combination.
[0103] [Heat treatment process]
[0104] In the present invention, further heat treatment is performed on the PPS resin after the above-mentioned post-treatment step, so that a PPS resin having high mechanical strength and excellent antifreeze resistance can be obtained, which is preferred. The heat treatment step is specifically described below.
[0105] In the present invention, in order to obtain a PPS resin with high mechanical strength, it is preferred to perform a heat treatment, but excessive heat treatment is not preferred because it causes the decrease in melt fluidity and the increase in gelled products in the resin, which may lead to non-filling during molding. However, if the heat treatment is too mild, the effect of reducing the volatile components is small, the strength of the resin is reduced, and there is a tendency for the antifreeze resistance to be reduced. Through the heat treatment of the present invention, a PPS resin with improved mechanical strength can be obtained without damaging the melt fluidity, suppressing the generation of gelled products.
[0106] The heat treatment may be carried out in either a high oxygen concentration atmosphere or a low oxygen concentration atmosphere as long as the heat treatment temperature and the heat treatment time are within specific ranges, but heat treatment in a low oxygen concentration atmosphere is preferred.
[0107] As the condition of the high oxygen concentration atmosphere, it is preferred that the oxygen concentration exceeds 2% by volume, and it is desired to heat the treatment at a temperature of 160 to 270°C and a heating treatment time of 0.1 to 17 hours. However, although the reduction rate of volatile components is fast under the condition of high oxygen concentration, oxidative crosslinking proceeds rapidly at the same time, so it is easy to produce gelled products. Therefore, it is preferred to heat the treatment generally at low temperature / long time or high temperature / short time. As the specific conditions for low temperature / long time heating treatment, it is preferred to heat the treatment at 160°C or more and 210°C or less for 1 hour or more and 17 hours or less, and more preferably at 170°C or more and 200°C or less for 1 hour or more and 10 hours or less. If the heating treatment temperature during the low temperature / long time heating treatment is in the above-mentioned preferred range, the effect of reducing volatile components is excellent, and the effect of improving mechanical strength can be expected. On the other hand, even if the heating treatment time is long at a low temperature and an oxygen concentration of more than 2% by volume, oxidative crosslinking is not easy to proceed, and the generation of gelled products can be prevented. As specific conditions for the high temperature / short time heat treatment, it is preferably carried out at a temperature of more than 210° C. and less than 270° C. for 0.1 hour or more and less than 1 hour, and more preferably at a temperature of more than 220° C. and less than 260° C. for 0.2 to 0.8 hours. If the heat treatment temperature during the high temperature / short time heat treatment is within the above preferred range, oxidative crosslinking is unlikely to proceed rapidly, and the generation of gelled products can be prevented. On the other hand, even if the heat treatment time is short at a high temperature, the effect of reducing volatile components is sufficient, and an improvement effect of mechanical strength can be expected.
[0108] As the condition of the low oxygen concentration atmosphere, the oxygen concentration is preferably 2% by volume or less, and it is desirable to heat the treatment at a temperature of 210 to 270° C. and a time of 0.2 to 50 hours. If the oxygen concentration is low, the effect of reducing the volatile components tends to be reduced, so it is preferred to heat the treatment at a high temperature / long time, and more preferably at a heating temperature of 220° C. to 260° C. for 2 to 20 hours. If the heating treatment time is within the above-mentioned preferred range, the volatile components are sufficiently reduced, and the effect of improving the mechanical strength can be expected. On the other hand, the productivity is excellent.
[0109] The heating device for heat treatment of the present invention can be a common hot air dryer, or a rotary or stirring blade heating device, but in the case of high efficiency and more uniform treatment, it is more preferred to use a rotary or stirring blade heating device, and examples include paddle dryers, fluidized bed dryers, KID dryers, steam pipe dryers, further tilted disk dryers, bucket dryers, vertical stirring dryers, etc. Among them, paddle dryers, fluidized bed dryers, and KID dryers are preferred in terms of uniform and efficient heating. In order to adjust the oxygen concentration of the heat treatment, it is also possible to mix non-oxidizing inert gases such as nitrogen, argon, helium, and water vapor into oxidizing gases such as oxygen, air, and ozone. As long as the heat treatment can be carried out in the heating device, there is no particular restriction on which position of the upper, lower, or side of the heating device to introduce the oxidizing gas or inert gas, but as a simpler method, it can be cited to introduce the gas from the upper part of the heating device. Furthermore, the oxidizing gas and the inert gas may be mixed before being introduced into the heating device, or the oxidizing gas and the inert gas may be mixed into the heating device from different locations.
[0110] It should be noted that it is believed that the structure of the PPS resin changes by undergoing the heat treatment process, but the PPS resin obtained by the heat treatment has a complex and diverse structure, and there are cases where it is not practical to specify the structure of the PPS resin. By undergoing the heat treatment process, the volatile components and water contained in the PPS resin can be removed, and a PPS resin having excellent mechanical strength and welding strength and excellent antifreeze resistance can be obtained.
[0111] The melt flow rate (hereinafter, sometimes abbreviated as MFR) of the PPS resin obtained through the above-mentioned polymerization reaction step, recovery step, preferably post-treatment step, and heat treatment step is preferably 1,000 g / 10 minutes or less, more preferably 700 g / 10 minutes or less, and further preferably 500 g / 10 minutes or less. If the MFR is in the above-mentioned preferred range, the degree of polymerization is sufficiently high and the mechanical strength is excellent. As a lower limit, a range exceeding 80 g / 10 minutes is preferred from the perspective of moldability, preferably 100 g / 10 minutes or more. Here, MFR is a value measured in accordance with ASTM-D1238-70 with a measurement temperature of 315.5°C and a load of 5,000 g.
[0112] The number average molecular weight of the PPS resin used in the present invention is 7,000 to 14,000, and more preferably 8,000 to 14,000. By setting the number average molecular weight to 7,000 or more, high mechanical strength and antifreeze resistance can be obtained, and the generation of mold scale can be suppressed. By setting the number average molecular weight to 14,000 or less, high antifreeze resistance can be obtained while obtaining appropriate fluidity.
[0113] Among them, the PPS resin having the following feature (1) can reduce the volatile components of the PPS resin composition when it is melted and obtain high antifreeze resistance. Furthermore, it is preferred from the intention of suppressing the generation of mold deposits. In addition, the PPS resin having the following feature (2) is also preferred from the viewpoint of suppressing the generation of mold deposits and obtaining high welding strength and antifreeze resistance.
[0114] (1) The residual amount when dissolved in 20 times the weight of 1-chloronaphthalene at 250°C for 5 minutes and filtered under hot pressure using a PTFE membrane filter with a pore size of 1 μm is 2.0 to 5.0% by weight or less.
[0115] Regarding the residual amount of the PPS resin, it is expected that it is preferably 4.8% by weight or less, and more preferably 4.5% by weight or less. By making the residual amount the above preferred range, appropriate fluidity can be obtained, so it is preferred. Regarding the lower limit of the residual amount, it is 2.0% by weight or more, preferably 2.2% by weight or more, and more preferably 2.5% by weight or more. By making the residual amount more than 2.0% by weight, crosslinking by thermal oxidation treatment is carried out, and high antifreeze resistance can be obtained while reducing the volatile components during melting. PPS resin with such properties is obtained by appropriately applying the thermal oxidation treatment after the above post-treatment process.
[0116] It should be noted that the above-mentioned residual amount is measured by using a material obtained by pressing a PPS resin into a film with a thickness of about 80 μm as a sample, using a high-temperature filtration device and a SUS test tube with an air pressure cover and a collecting funnel. Specifically, first, a membrane filter with a pore size of 1 μm is placed in a SUS test tube, and then the PPS resin pressed into a film with a thickness of about 80 μm and 20 times the weight of 1-chloronaphthalene are weighed and sealed. It is placed in a high-temperature filtration device at 250°C and heated and shaken for 5 minutes. Then, a syringe containing air is connected to the air pressure cover and the piston of the syringe is pushed out, and hot filtration is performed by air pressure. As a specific quantitative method for the residual amount, the weight difference between the membrane filter before filtration and the membrane filter vacuum dried at 150°C for 1 hour after filtration is obtained.
[0117] (2) When heated and melted at 320°C for 2 hours under vacuum, the amount of volatilized gas generated is 0.35% by weight or less.
[0118] Regarding the gas generation amount of PPS resin, it is expected that it is preferably less than 0.30 weight %, and more preferably less than 0.28 weight %. PPS resin with such properties is obtained by appropriately applying the above-mentioned washing and thermal oxidation treatment. By making the gas generation amount less than 0.35 weight %, the volatile components are reduced, and the welding strength and antifreeze resistance are improved, so it is preferred. Regarding the lower limit of the gas generation amount after thermal oxidation treatment, it is preferably less, but the preferred lower limit is 0.01 weight %. By being more than 0.01 weight %, it is possible to prevent the time of thermal oxidation treatment from becoming too long, and prevent it from becoming disadvantageous economically. In addition, when the time of thermal oxidation treatment is prolonged, gelled products are easily produced, which becomes a cause of poor molding, so it is also preferred to prevent it.
[0119] It should be noted that the so-called gas generation amount refers to the amount of adhesive components obtained by cooling the volatilized gas when the PPS resin is heated and melted under vacuum and liquefying or solidifying, and is measured by heating the glass ampoule with the PPS resin vacuum sealed in a tube furnace. The shape of the glass ampoule is 100mm×25mm, the neck is 255mm×12mm, and the wall thickness is 1mm. As a specific measurement method, only the main body of the glass ampoule with the PPS resin vacuum sealed is inserted into a tube furnace at 320°C and heated for 2 hours, so that the volatile gas is cooled and attached to the neck of the ampoule that is not heated by the tube furnace. After cutting out the neck and weighing it, the attached gas is dissolved in chloroform and removed. Then, the neck is dried and weighed again. The gas generation amount is calculated from the weight difference of the ampoule neck before and after the gas is removed.
[0120] For example, by adopting the above-mentioned production method, a resin composition which not only has excellent high antifreeze resistance but also suppresses the generation of mold deposit can be obtained by using the obtained PPS resin. In the present invention, it is preferable to use such a heat-treated PPS resin.
[0121] The PPS resin to be blended in the PPS resin composition of the present invention needs to be a PPS resin (A) having a number average molecular weight of 7,000 to 14,000 and a residual amount of 2.0 to 5.0% by weight when hot-pressed filtration is performed by the above method. The PPS resin (A) may be only one type of PPS resin having the above characteristics, or may be a mixture of multiple PPS resins having different characteristics. When multiple PPS resins are mixed, as long as the PPS resin in a mixed state has the above characteristics, a PPS resin that does not have the above characteristics when viewed alone may be included.
[0122] The PPS resin composition of the present invention is compounded with (B) glass fiber.
[0123] The amount of the glass fiber (B) in the PPS resin composition of the present invention is 30 to 110 parts by weight based on 100 parts by weight of the PPS resin (A), which is necessary to obtain excellent mechanical strength, weld strength, and dimensional accuracy.
[0124] When the amount of (B) glass fiber is less than 30 parts by weight relative to 100 parts by weight of (A) PPS resin, the composition cannot have a suitable strength. When the amount of (B) glass fiber exceeds 110 parts by weight, the melt fluidity of the composition decreases, and suitable molding processability and mechanical strength cannot be obtained.
[0125] As such (B) glass fiber, specifically, glass fiber, profiled cross-section glass fiber, glass cut fiber, flat glass fiber, etc. can be cited, and they can also be used in combination of two or more. Glass fiber is preferred. In addition, it is preferred to pre-treat these glass fibers with coupling agents such as isocyanate compounds, organosilane compounds, organic titanate compounds, organic borane compounds and epoxy compounds and use them with the intention of obtaining better mechanical strength, wherein it is preferably treated with a bunching agent containing an epoxy group.
[0126] The PPS resin composition of the present invention is blended with (C) a silane compound having any functional group selected from an amino group and an isocyanate group (hereinafter, sometimes referred to as (C) silane compound).
[0127] The amount of the silane compound (C) in the PPS resin composition of the present invention is 0.1 to 3 parts by weight based on 100 parts by weight of the PPS resin (A). This amount can achieve both excellent fluidity and antifreeze resistance.
[0128] When the amount of the silane compound (C) is less than 0.1 parts by weight relative to 100 parts by weight of the PPS resin (A), the composition cannot have adequate strength or antifreeze resistance. When the amount of the silane compound (C) exceeds 3 parts by weight, the melt fluidity of the composition decreases, and adequate molding processability cannot be obtained, and mold deposits also increase.
[0129] Specific examples of such (C) silane compounds include alkoxysilane compounds containing an isocyanate group such as γ-isocyanatepropyltriethoxysilane, γ-isocyanatepropyltrimethoxysilane, γ-isocyanatepropylmethyldimethoxysilane, γ-isocyanatepropylmethyldiethoxysilane, γ-isocyanatepropylethyldimethoxysilane, γ-isocyanatepropylethyldiethoxysilane, and γ-isocyanatepropyltrichlorosilane, and alkoxysilane compounds containing an amino group such as γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, and γ-aminopropyltriethoxysilane. Among them, γ-aminopropyltriethoxysilane and γ-isocyanatepropyltriethoxysilane are suitable for obtaining excellent antifreeze resistance, and γ-isocyanatepropyltriethoxysilane is particularly suitable for suppressing the generation of mold deposits in addition to excellent antifreeze resistance.
[0130] The PPS resin composition of the present invention may be added with an elastomer for the purpose of improving the thermal shock resistance within the range that does not impair the effects of the present invention. Such elastomers include (co)polymers obtained by polymerizing α-olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-octene, 4-methyl-1-pentene, isobutylene, etc., either alone or in combination of two or more thereof, for example, ethylene / propylene copolymers (" / " indicates copolymerization, the same below), ethylene / 1-butene copolymers, ethylene / 1-hexene copolymers, and ethylene / 1-octene copolymers. In addition, it can be obtained by introducing a monomer component having an epoxy group (a component containing a functional group) into a copolymer of an α-olefin and an α,β-unsaturated acid and its alkyl ester such as acrylic acid, methyl acrylate, ethyl acrylate, butyl acrylate, methacrylic acid, methyl methacrylate, ethyl methacrylate, butyl methacrylate, etc., such as ethylene / methyl acrylate copolymer, ethylene / ethyl acrylate copolymer, ethylene / butyl acrylate copolymer, ethylene / methyl methacrylate copolymer, ethylene / ethyl methacrylate copolymer, ethylene / butyl methacrylate copolymer, etc. Examples of the component containing a functional group include monomers containing epoxy groups such as glycidyl acrylate, glycidyl methacrylate, glycidyl ethacrylate, glycidyl itaconate, glycidyl citrate, etc. There is no particular limitation on the method of introducing these components containing functional groups, and methods such as copolymerizing an olefin-based (co)polymer during (co)polymerization or grafting an olefin-based (co)polymer using a free radical initiator can be used. The amount of the component containing the functional group introduced is appropriately in the range of 0.001 to 40 mol%, preferably 0.01 to 35 mol%, relative to the total monomers constituting the modified olefin (co)polymer. As a specific example of an olefin copolymer having a glycidyl group obtained by introducing a monomer component having an epoxy group into an olefin polymer, it is suitable to use ethylene / propylene-g-glycidyl methacrylate copolymer ("g" means grafting, the same below), ethylene / 1-butene-g-glycidyl methacrylate copolymer, ethylene / glycidyl acrylate copolymer, ethylene / glycidyl methacrylate copolymer, ethylene / methyl acrylate / glycidyl methacrylate copolymer, ethylene / methyl methacrylate / glycidyl methacrylate copolymer, or an olefin copolymer containing an epoxy group having other monomers as essential components in addition to glycidyl esters of α-olefins such as ethylene and propylene and α,β-unsaturated acids.
[0131] Preferred examples include ethylene / glycidyl methacrylate copolymers, ethylene / methyl acrylate / glycidyl methacrylate copolymers, and ethylene / methyl methacrylate / glycidyl methacrylate copolymers. Particularly preferred examples include ethylene / methyl acrylate / glycidyl methacrylate copolymers.
[0132] The amount of such an elastomer blended is preferably 1 to 20 parts by weight, and more preferably 2 to 15 parts by weight, based on 100 parts by weight of the (A) PPS resin, in order to achieve excellent mechanical strength, thermal shock resistance, and moldability.
[0133] Furthermore, the PPS resin composition of the present invention may be further blended with other resins within a range that does not impair the effects of the present invention. Such blendable resins are not particularly limited, but specific examples thereof include polyamide resins such as nylon 6, nylon 66, nylon 610, nylon 11, nylon 12, aromatic nylons, polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polycyclohexyldimethylene terephthalate, and polynaphthalene terephthalate, polyamide-imide, polyacetal, polyimide, polyetherimide, polyethersulfone, modified polyphenylene ether resin, polysulfone resin, polyallyl sulfone resin, polyketone resin, polyarylate resin, liquid crystal polymer, polyetherketone resin, polysulfide ether ketone resin, polyether ether ketone resin, polyamide-imide resin, and tetrafluoroethylene resin.
[0134] It should be noted that the PPS resin composition of the present invention may contain other components such as antioxidants, heat stabilizers (hindered phenol, hydroquinone, phosphorus, phosphite, amine, sulfur and their substitutes), weathering agents (resorcinol, salicylate, benzotriazole, benzophenone, hindered amine, etc.), mold release agents and lubricants (montanic acid and its metal salts, esters, half esters, stearyl alcohol, stearamide, stearic acid esters, diureas and polyethylene wax, etc.), pigments (cadmium sulfide, phthalocyanine, carbon black for coloring, etc.), dyes (nigrosine, etc.), crystal nucleating agents (talc, silica, kaolin, clay and other inorganic crystal nucleating agents or organic crystal nucleating agents)), plasticizers (octyl p-hydroxybenzoate, N-butylbenzenesulfonate, etc.), and other additives. The present invention also includes general additives such as amides, antistatic agents (alkyl sulfate type anionic antistatic agents, quaternary ammonium salt type cationic antistatic agents, nonionic antistatic agents such as polyoxyethylene sorbitan monostearate, betaine type amphoteric antistatic agents, etc.), flame retardants (for example, hydroxides such as red phosphorus, phosphate esters, melamine cyanurate, magnesium hydroxide, aluminum hydroxide, ammonium polyphosphate, brominated polystyrene, brominated polyphenylene ether, brominated polycarbonate, brominated epoxy resin, or a combination of these brominated flame retardants and antimony trioxide, etc.), heat stabilizers, lubricants such as calcium stearate, aluminum stearate, lithium stearate, bisphenol A type bisphenol epoxy resins, novolac phenol type epoxy resins, cresol novolac type epoxy resins, etc., strength enhancing materials, ultraviolet light inhibitors, colorants, and foaming agents. Among them, polyethylene as a mold release agent is preferred from the viewpoint of antifreeze resistance, and amide compounds are particularly preferred from the viewpoint of suppressing the generation of mold deposits in addition to antifreeze resistance. The type of the crystal nucleating agent is not particularly limited, but examples thereof include inorganic crystal nucleating agents and organic crystal nucleating agents. In particular, organic crystal nucleating agents are preferred from the viewpoint of antifreeze resistance and weld strength.Examples of the organic crystal nucleating agent used in the present invention include sorbitol compounds and metal salts thereof; phosphoric acid ester metal salts; rosin compounds; oleic acid amide, acrylic acid amide, stearic acid amide, decane dicarboxylic acid dibenzohydrazide, hexane dicarboxylic acid dibenzohydrazide, 1,4-cyclohexane dicarboxylic acid dicyclohexylamide, trimesic acid amide, anilide compounds, 2,6-naphthalene dicarboxylic acid dicyclohexylamide, N,N'-dibenzoyl-1,4-diaminocyclohexane, N,N'-dicyclohexanecarbonyl-1,5-diaminonaphthalene, octane dicarboxylic acid dibenzohydrazide and other amide compounds; ethylenediamine / stearic acid / sebacic acid polycondensates; montanic acid waxes; aliphatic carboxylic acid Organic compounds and polymer compounds such as metal salts of aromatic acids, metal salts of aromatic carboxylates, aromatic phosphonic acids and metal salts, metal salts of aromatic phosphates, metal salts of aromatic sulfonic acids, metal salts of β-diketones, metal salts of carboxyl groups, organic phosphorus compounds, polyethylene, polypropylene, polybutadiene, polystyrene, AS resin, ABS resin, poly(acrylic acid), poly(acrylate), poly(methacrylic acid), poly(methacrylate), polyamide 6, polyamide 46, polyamide 66, polyamide 6T, polyamide 9T, polyamide 10T, polyetheretherketone, and polyetherketone, among which polymer compounds having a carbonyl group are preferred, and polyetheretherketone is more preferred. The amount of such an organic crystal nucleating agent to be blended is preferably 0.06 to 0.19 parts by weight relative to 100 parts by weight of the (A) PPS resin.
[0135] The PPS resin composition of the present invention can be further added except (B) glass fiber, other inorganic filling materials and used in the scope that does not damage the effect of the present invention. There is no particular restriction on such inorganic filling materials that can be added, but as the specific example of the fibrous filling materials as inorganic filling materials, stainless steel fiber, aluminum fiber, brass fiber, rock wool, PAN system, carbon fiber of asphalt system, carbon nanotube, carbon nanofiber, calcium carbonate whisker, wollastonite whisker, potassium titanate whisker, barium titanate whisker, aluminum borate whisker, silicon nitride whisker, aramid fiber, aluminum oxide fiber, silicon carbide fiber, asbestos fiber, gypsum fiber, ceramic fiber, zirconium oxide fiber, silicon dioxide fiber, titanium oxide fiber, silicon carbide fiber etc. can be enumerated, and they can also be used in combination with more than two kinds. In addition, it is preferred that these fibrous filling materials are pre-treated with coupling agents such as isocyanate compounds, organosilane compounds, organic titanate compounds, organic borane compounds and epoxy compounds and used in the intention of obtaining more excellent mechanical strength.
[0136] In addition, specific examples of non-fibrous fillers as inorganic fillers include talc, wollastonite, zeolite, sericite, mica, kaolin, clay, pyrophyllite, bentonite, asbestos, silicates such as aluminum silicate and hydrotalcite, silicon oxide, magnesium oxide, aluminum oxide (alumina), silicon dioxide (crushed / spherical), quartz, glass beads, glass flakes, crushed / indeterminate glass, glass microspheres, molybdenum disulfide, aluminum oxide (crushed), translucent aluminum oxide (fibrous / plate-like / scaly / granular / indeterminate / crushed), and titanium oxide (crushed). , oxides such as zinc oxide (fibrous / plate-like / scaly / granular / indeterminate / crushed products), carbonates such as calcium carbonate, magnesium carbonate, zinc carbonate, sulfates such as calcium sulfate, barium sulfate, hydroxides such as calcium hydroxide, magnesium hydroxide, aluminum hydroxide, silicon carbide, carbon black and silicon dioxide, graphite, aluminum nitride, translucent aluminum nitride (fibrous / plate-like / scaly / granular / indeterminate / crushed products), polyphosphate, metal powder, metal flakes, metal strips, metal oxides, etc., and specific examples of metal types of metal powder, metal flakes, and metal strips include silver, nickel, copper, zinc, aluminum, stainless steel, iron, brass, chromium, tin, etc. In addition, carbon powder, carbon flakes, scaly carbon, fullerene, graphene, etc. can be cited, and they can be hollow, and further, these filling materials can be used in combination of two or more. Furthermore, these inorganic fillers may be used after being pretreated with a coupling agent such as an isocyanate compound, an organic silane compound, an organic titanate compound, an organic borane compound, and an epoxy compound. Among them, calcium carbonate, carbon powder, and graphite are preferred.
[0137] There is no particular restriction on the method for preparing the PPS resin composition of the present invention, but a method of supplying each raw material to a commonly known melt mixer such as a single-screw or twin-screw extruder, a Banbury mixer, a kneader, and a mixing roll, and kneading at a temperature of 280 to 380°C can be cited as a representative example. There is no particular restriction on the order of mixing the raw materials, and any method can be used, such as a method of mixing all the raw materials and then melt-kneading them by the above method, a method of mixing a part of the raw materials and then melt-kneading them by the above method and then mixing the remaining raw materials and then melt-kneading them, or a method of mixing a part of the raw materials and then melting and kneading them by a single-screw or twin-screw extruder and then using a side feeder to mix the remaining raw materials, etc. In addition, with respect to a small amount of additive components, it is of course possible to mix and granulate the other components by the above method, etc., and then add them before molding and supply them for molding.
[0138] The PPS resin composition of the present invention obtained by such operation can be used for various moldings such as injection molding, extrusion molding, blow molding, transfer molding, etc., but is particularly suitable for injection molding purposes. The PPS resin composition of the present invention is suitable for automobile cooling parts, especially small and complex-shaped automobile cooling parts that combine multiple parts. The so-called complex-shaped automobile cooling parts here, for example, combine the shell with at least two tubes, the shape of the shell can be any shape such as quadrilateral, triangle, ellipse, or respective composite shapes, and ribs, protrusions, flanges can also be set on its shell, or it can be a shape close to a plane. In addition, the shape of the tube combined with the above-mentioned shell can be straight or curved, and the cross-sectional shape of the tube can be any shape such as circular, elliptical, quadrilateral, etc. In addition, ribs, protrusions, and flanges can be set on the tube. In addition, at least two or more tubes can each be the same shape, or a combination of different shapes. In addition, the method of combining the tubes can be, for example, bolt fastening, in addition, it can also be welding such as hot plate welding, or it can be formed as a part of the shell by injection molding. In addition, the place of combining the tubes can be a wall surface or a bottom surface. Furthermore, the cover of the housing may be made of resin or metal, and the cover may be fastened by bolts or welded by hot plate welding or the like.
[0139] In addition, a shell, a valve and at least three tubes are combined, and the shape of the shell can be any shape such as a quadrilateral, a triangle, an ellipse, or a composite shape of each, and ribs, protrusions, and flanges can also be provided on the shell. In addition, the shape of the valve enclosed by the above-mentioned shell can be any shape such as a spherical shape, a cylindrical shape, or a composite shape of each, and a hole can also be opened in the valve. In addition, the number of valves can be 1, and can be more than 2. In addition, the shape of the tube combined with the above-mentioned shell can be straight or curved, and the cross-sectional shape of the tube can be any shape such as a circle, an ellipse, a quadrilateral, etc. In addition, ribs, protrusions, and flanges can be provided on the tube. In addition, at least three tubes can each be the same shape, or a combination of different shapes. In addition, the method of combining the tubes can be, for example, bolt fastening, and can also be welding such as hot plate welding, or can be molded as a part of the shell by injection molding. In addition, the valve encapsulation method can be that the outer shell is divided into a shell and a cover, the valve is encapsulated in the shell, and the cover is fastened with bolts to form the outer shell. In addition, the cover can be welded by hot plate welding or the like to form the outer shell.
[0140] The liquid flowing inside the shell can be water, or an antifreeze solution containing alcohols, glycols, glycerol, etc., and its type and concentration are not particularly limited. In addition, it can be high temperature or low temperature, and they can flow repeatedly.
[0141] The valve contained in the housing may be opened and closed by the driving force of the engine or the driving force of the electric motor.
[0142] The melting crystallization peak temperature of the PPS resin composition of the present invention obtained by a differential scanning calorimeter is preferably above 230°C, and more preferably above 235°C. If the melting crystallization peak temperature is above 230°C, the cooling time during injection molding becomes shorter, and productivity is improved, so it is preferred. In addition, the antifreeze resistance is also improved, so it is preferred. In order to obtain a PPS resin composition with such characteristics, it is conceivable to mix an organic crystal nucleating agent, for example. It should be noted that the melting crystallization peak temperature in the present invention is a value measured by taking about 10 mg of the particles of the PPS resin composition as a sample, using a differential scanning calorimeter DSC-7 manufactured by PerkinElmer, heating at a heating rate of 20°C / min, keeping it at 340°C for 5 minutes, and then cooling it at a rate of 20°C / min.
[0143] The tensile strength of the ISO test piece formed by injection molding the PPS resin composition of the present invention is preferably 190 MPa or more. If the tensile strength of the ISO test piece is in the above-mentioned preferred range, sufficient strength as a molded product can be satisfied. It should be noted that, in this case, the tensile strength is evaluated by the tensile strength measured by ISO 527-1 and 527-2 methods under the conditions of a tensile speed of 5 mm / min and an atmospheric temperature of 23°C. In addition, after such an ISO test piece is immersed in an antifreeze solution at 150°C for 500 hours, the tensile strength is measured according to ISO 527-1 and 527-2 methods under the conditions of a tensile speed of 5 mm / min and an atmospheric temperature of 23°C. The strength retention rate of the tensile strength after antifreeze treatment is preferably 80% or more. If the strength retention rate of the tensile strength after antifreeze treatment is in the above-mentioned preferred range, the mechanical strength is not easily reduced by antifreeze treatment, and it will not become the starting point of cracks in the molded product. If the tensile strength is 190 MPa or more and the tensile strength retention rate after antifreeze treatment is 80% or more, it has both better mechanical strength and resistance to hot water and antifreeze, so it is particularly preferred. In order to obtain a PPS resin composition with such characteristics, for example, a PPS resin with a number average molecular weight of 7,000 to 14,000 that has been subjected to thermal oxidation treatment can be mixed with glass fibers.
[0144] It should be noted that there is no particular limitation on the type of antifreeze, and it may be Foulx Worken genuine LLC (G13), Toyota Motors genuine S-LLC, Zeneral Motors genuine LLC (Dex-cool), or Hyundai Motors genuine LLC (A-110).
[0145] As described above, the PPS resin composition of the present invention has excellent mechanical strength and antifreeze resistance, and can also suppress the generation of mold deposits. That is, the PPS resin composition of the present invention is useful in automobile cooling parts, especially in small / complex-shaped automobile cooling parts in which a plurality of parts are combined, because it has high mechanical strength and high antifreeze resistance and also suppresses the generation of mold deposits.
[0146] Other applicable uses of the PPS resin composition of the present invention include, for example, electrical / electronic parts represented by sensors, LED lamps, household connectors, sockets, resistors, relay housings, switches, bobbins, capacitors, variable capacitor housings, oscillators, various terminal boards, transformers, plugs, printed circuit boards, tuners, speakers, microphones, headphones, small motors, head mounts, semiconductors, liquid crystals, FDD brackets, FDD chassis, motor brush holders, parabolic antennas, computer-related parts, and the like; and household and office electrical appliance parts represented by VTR parts, television parts, irons, hair dryers, rice cooker parts, microwave oven parts, audio parts, audio / laser disc (registered trademark) / optical disc and other audio equipment parts, lighting parts, refrigerator parts, air conditioner parts, typewriter parts, word processor parts, and the like. In addition, examples include office computer related parts, telephone related parts, fax machine related parts, copier related parts, washing fixtures, motor parts, igniters, typewriters, etc. as representative of mechanical related parts: microscopes, binoculars, cameras, clocks, etc. as representative of optical equipment, precision machinery related parts; faucets, mixing faucets, pump parts, pipe joints, water volume regulating valves, safety valves, water temperature sensors, water volume sensors, water meter cases and other water supply parts; valve AC generator terminals, AC generator connectors, IC regulators, dimmer potentiometer bases, exhaust valves and other valves, fuel-related / exhaust / intake system pipes, intake nozzle ventilation pipes, intake manifolds, fuel pumps, engine cooling water joints, carburetor bodies, steam Various uses include carburetor spacers, exhaust gas sensors, cooling water sensors, oil temperature sensors, throttle position sensors, crankshaft position sensors, air flow meters, brake pad wear sensors, air conditioner thermostat bases, heater flow control valves, radiator motor brush holders, water pump impellers, turbine blades, wiper motor related parts, distributors, starter switches, starter relays, transmission wiring, window washer nozzles, air conditioner panel switch substrates, fuel-related solenoid valve coils, fuse connectors, speaker terminals, electrical component insulation boards, stepping motor rotors, lamp holders, headlight reflectors, lamp housings, brake pistons, solenoid bobbins, engine oil filters, ignition housings, vehicle speed sensors, cable bushings and other automobile / vehicle related parts.
[0147] Example
[0148] The present invention will be described in more detail below with reference to Examples, but the present invention is not limited to the description of these Examples.
[0149] [Measurement method of PPS resin]
[0150] (1) Residual amount
[0151] In a SUS test tube made by Senshiu Scientific with an air pressure cap and a collecting funnel, a pre-weighed PTFE membrane filter with a pore size of 1 μm is placed, and 100 mg of PPS resin and 2 g of 1-chloronaphthalene, which are pressed into a membrane with a thickness of about 80 μm, are added and sealed. Insert it into the high-temperature filtration device SSC-9300 made by Senshiu Scientific, and heat and oscillate at 250°C for 5 minutes to dissolve the PPS resin in 1-chloronaphthalene. After connecting a 20 mL syringe containing air to the air pressure cap, push out the piston and filter the solution with a membrane filter. Take out the membrane filter, vacuum dry it at 150°C for 1 hour, and then weigh it. The difference in the weight of the membrane filter after filtration relative to the weight of the membrane filter before filtration is set as the residual amount (weight %).
[0152] (2) Gas generation
[0153] 3 g of PPS resin was weighed into a glass ampoule with a belly of 100 mm × 25 mm, a neck of 255 mm × 12 mm, and a wall thickness of 1 mm, and then vacuum sealed. Only the main body of the glass ampoule was inserted into a ceramic electric heating tube furnace ARF-30K manufactured by Asahika Seisakusho Co., Ltd. and heated at 320°C for 2 hours. After taking out the ampoule, the neck of the ampoule that was not heated by the tube furnace and attached with volatile gas was cut out with a file and weighed. Then, the attached gas was dissolved and removed with 5 g of chloroform, and then dried in a glass dryer at 60°C for 1 hour and weighed again. The weight difference of the neck of the ampoule before and after the gas was removed was set as the gas generation amount (weight %).
[0154] (3) Melt flow rate (MFR)
[0155] The measurement was performed at a measurement temperature of 315.5° C. and a load of 5,000 g in accordance with ASTM-D1238-70.
[0156] (4) Number average molecular weight
[0157] Gel permeation chromatography measurement: using an apparatus manufactured by WATERS (GPC-244), using a column: Shodex K-806M (manufactured by Showa Denko K.K.), a solvent: 1-chloronaphthalene, a detector: a hydrogen flame ionization detector, and 6 types of monodisperse polystyrenes for calibration, the number average molecular weight was determined according to the method described in the February issue of Polymer Thesis Vol. 44 (1987), pp. 139-141.
[0158] [Reference Example 1] Polymerization of PPS (PPS-1)
[0159] In an autoclave equipped with a stirrer and a valve at the bottom, 8,267.4 g (70.0 mol) of 47.5% sodium hydrosulfide, 2,925.0 g (70.2 mol) of 96% sodium hydroxide, 13,860.0 g (140.0 mol) of N-methyl-2-pyrrolidone (NMP), 1894.2 g (23.1 mol) of sodium acetate, and 10,500.0 g of ion exchange water were added, and the mixture was slowly heated to 240° C. over about 3 hours while nitrogen was passed under normal pressure. After 14,772.1 g of water and 280.0 g of NMP were distilled off, the reaction vessel was cooled to 160° C. The amount of water remaining in the system per 1 mol of the alkali metal sulfide added was 1.08 mol, including the water consumed by the hydrolysis of NMP. In addition, the amount of hydrogen sulfide scattered was 0.023 mol per 1 mol of the alkali metal sulfide added.
[0160] Next, 10,646.7 g (72.4 mol) of p-dichlorobenzene (p-DCB) and 6,444.9 g (65.1 mol) of NMP were added, the reaction vessel was sealed under nitrogen, and the temperature was raised from 200° C. to 270° C. at a rate of 0.6° C. / min while stirring at 240 rpm, and maintained at 270° C. for 70 minutes. The take-out valve at the bottom of the autoclave was opened, and the contents were flashed into a container with a stirrer over 15 minutes while pressurizing with nitrogen, and most of the NMP was removed by stirring at 250° C. for a while.
[0161] The obtained solid matter and 53 L of ion exchange water were added to an autoclave equipped with a stirrer, washed at 70°C for 30 minutes, and then filtered with a glass filter having a pore size of 10 to 16 μm. Then, 60 L of ion exchange water heated to 70°C was injected into a glass filter having a pore size of 10 to 16 μm, and filtered with suction to obtain 18,000 g of a PPS resin cake (including 7,550 g of PPS resin).
[0162] 18,000 g of the above-mentioned PPS resin filter cake, 40 L of ion exchange water, and 43 g of acetic acid were added to an autoclave with a stirrer. After the interior of the autoclave was replaced with nitrogen, the temperature was raised to 192°C and maintained for 30 minutes to perform an acid treatment. The pH during the acid treatment was 7. After the autoclave was cooled, the contents were filtered with a glass filter with a pore size of 10 to 16 μm. Next, 60 L of ion exchange water heated to 70°C was injected into the glass filter, and the filter cake was obtained by suction filtration. The obtained filter cake was dried at 120°C for 4 hours under a nitrogen flow to obtain a powder of the acid-treated PPS resin. Next, the PPS resin powder was added to a heating device with a volume of 100 L and equipped with a stirrer, and a thermal oxidation treatment was performed at 220°C and an oxygen concentration of 2% for 2 hours to obtain a cross-linked PPS-1. The number average molecular weight of the obtained polymer was 8,500, the amount of gas generated was 0.16% by weight, the residual amount was 2.1% by weight, and the MFR was 420 g / 10 minutes.
[0163] [Reference Example 2] Polymerization of PPS (PPS-2)
[0164] In a 70L autoclave equipped with a stirrer and a bottom stopper, 8.27kg (70.00 mol) of 47.5% sodium hydrosulfide, 2.91kg (69.80 mol) of 96% sodium hydroxide, 11.45kg (115.50 mol) of N-methyl-2-pyrrolidone (NMP), and 10.5kg of ion exchange water were added, and the mixture was slowly heated to 245°C over about 3 hours while nitrogen was passed under normal pressure. After 14.78kg of water and 0.28kg of NMP were distilled off, the reaction vessel was cooled to 200°C. The amount of water remaining in the system per 1 mol of the alkali metal sulfide added was 1.06 mol, including the water consumed by the hydrolysis of NMP. In addition, the amount of hydrogen sulfide scattered was 0.02 mol per 1 mol of the alkali metal sulfide added.
[0165] Then, the mixture was cooled to 200° C., 10.48 kg (71.27 mol) of p-dichlorobenzene and 9.37 kg (94.50 mol) of NMP were added, and the reaction vessel was sealed under nitrogen. The temperature was raised from 200° C. to 270° C. at a rate of 0.6° C. / min while stirring at 240 rpm. After reacting at 270° C. for 100 minutes, the bottom stopper valve of the autoclave was opened, and the contents were flashed into a container with a stirrer over 15 minutes while pressurizing with nitrogen, and most of the NMP was removed by stirring at 250° C. for a while.
[0166] The obtained solid matter and 76 L of ion exchange water were added to an autoclave equipped with a stirrer, washed at 70° C. for 30 minutes, and then suction filtered through a glass filter. Next, 76 L of ion exchange water heated to 70° C. was poured into the glass filter, and suction filtered to obtain a filter cake.
[0167] The obtained filter cake and 90 L of ion exchange water were added to an autoclave equipped with a stirrer, and acetic acid was added to adjust the pH to 7. After the inside of the autoclave was replaced with nitrogen, the temperature was raised to 192° C. and maintained for 30 minutes. The autoclave was then cooled and the contents were taken out.
[0168] After the contents were filtered with a glass filter, 76 L of ion exchange water at 70° C. was injected therein and filtered to obtain a filter cake. The obtained filter cake was dried at 120° C. under a nitrogen gas stream to obtain dry PPS. It was heat treated at 200° C. under an oxygen gas stream until the MFR value reached 150 g / 10 minutes to obtain cross-linked PPS-2. The number average molecular weight of the obtained polymer was 11,500, the gas generation amount was 0.39% by weight, the residual amount was 5.9% by weight, and the MFR was 140 g / 10 minutes.
[0169] [Reference Example 3] Polymerization of PPS (PPS-3)
[0170] Linear PPS-3 was obtained in the same manner as in Reference Example 2 except that heat treatment at 200°C under oxygen gas flow was not performed. The number average molecular weight of the obtained polymer was 8,000, the gas generation amount was 0.44% by weight, the residual amount was 1.5% by weight, and the MFR was 720 g / 10 minutes.
[0171] [Reference Example 4] Polymerization of PPS (PPS-4)
[0172] 4.67 kg of 30% sodium hydrosulfide aqueous solution (25 mol of sodium hydrosulfide), 2.00 kg of 50% sodium hydroxide (25 mol of sodium hydroxide) and 8 kg of N-methyl-2-pyrrolidone (NMP) were added to the autoclave, and the temperature was slowly raised to 205°C while stirring, and 4.11 kg of distilled water including 3.8 kg of water was removed. 3.75 kg (25.5 mol) of 1,4-dichlorobenzene and 2 kg of NMP were added to the residual mixture and heated at 230°C for 1 hour, and further heated at 260°C for 30 minutes. The reaction product was washed with warm water 5 times and dried under reduced pressure at 80°C for 24 hours to obtain a linear PPS-4 powder with a number average molecular weight of 3,700. The number average molecular weight of the obtained polymer was 3,700, the gas generation amount was 0.54% by weight, the residual amount was 1.3% by weight, and the MFR was 9,570 g / 10 minutes.
[0173] [Reference Example 5] Polymerization of PPS (PPS-5)
[0174] In a 70L autoclave equipped with a stirrer, 8,267.37 g (70.0 mol) of 47.5% sodium hydrosulfide, 2,962.50 g (71.10 mol) of 96% sodium hydroxide, 11,434.50 g (115.50 mol) of N-methyl-2-pyrrolidone (NMP), 516.60 g (6.30 mol) of sodium acetate, and 10,500 g of ion exchange water were added, and the mixture was slowly heated to 230°C over about 3 hours while nitrogen was passed under normal pressure. After 14,780.1 g of water and 280 g of NMP were distilled off, the reaction vessel was cooled to 160°C. The amount of water remaining in the system per 1 mol of the alkali metal sulfide added was 1.06 mol, including the water consumed by the hydrolysis of NMP. In addition, the amount of hydrogen sulfide scattered was 0.017 mol per 1 mol of the alkali metal sulfide added.
[0175] Next, 10,363.50 g (70.5 mol) of p-dichlorobenzene and 9,078.30 g (91.7 mol) of NMP were added, and the reaction vessel was sealed under nitrogen. The temperature was raised to 270°C at a rate of 0.6°C / min while stirring at 240 rpm, and the temperature was maintained at 270°C for 140 minutes. Then, 2,520 g (140 mol) of ion exchange water was pressure-injected into the autoclave while cooling to 250°C at a rate of 1.3°C / min. Then, the temperature was cooled to 200°C at a rate of 1.0°C / min, and then quenched to near room temperature.
[0176] The contents were taken out, diluted with 26,300 g of NMP, and the solvent and solid matter were separated by filtration with a sieve (80 mesh), and the obtained particles were washed with 31,900 g of NMP and separated by filtration. It was washed several times with 56,000 g of ion exchange water, separated by filtration, and then washed with 70,000 g of 0.05 wt% acetic acid aqueous solution and separated by filtration. After washing and filtration with 70,000 g of ion exchange water, the obtained water-containing PPS particles were dried with hot air at 80°C and dried under reduced pressure at 120°C to obtain linear PPS-5. The number average molecular weight of the obtained polymer was 7,700, the gas generation was 0.11 wt%, the residual amount was 0.02 wt%, and the MFR was 580 g / 10 minutes.
[0177] [Reference Example 6] Polymerization of PPS (PPS-6)
[0178] Linear PPS-6 was obtained in the same manner as in Reference Example 5 except that 1,722.00 g (21.00 mol) of sodium acetate was added. The number average molecular weight of the obtained polymer was 8,900, the gas generation amount was 0.09 wt %, the residual amount was 0.02 wt %, and the MFR was 210 g / 10 min.
[0179] [Compounds used in Examples and Comparative Examples]
[0180] The compounding materials used in the present examples and comparative examples are as follows.
[0181] (A) PPS resin
[0182] PPS-1: PPS resin obtained by polymerization according to the method described in Reference Example 1
[0183] PPS-2: PPS resin obtained by polymerization according to the method described in Reference Example 2
[0184] PPS-3: PPS resin obtained by polymerization according to the method described in Reference Example 3
[0185] PPS-4: PPS resin obtained by polymerization according to the method described in Reference Example 4
[0186] PPS-5: PPS resin obtained by polymerization according to the method described in Reference Example 5
[0187] PPS-6: PPS resin obtained by polymerization according to the method described in Reference Example 6
[0188] (B) Glass fiber
[0189] B: Chopped strands (T-760H manufactured by Nippon Electric Glass Co., Ltd., 3 mm long, average fiber diameter 10.5 μm)
[0190] (C) Silane compound
[0191] C-1: 3-aminopropyltriethoxysilane (KBE-903 manufactured by Shin-Etsu Chemical Co., Ltd.)
[0192] C-2: 3-isocyanatepropyltriethoxysilane (KBE-9007 manufactured by Shin-Etsu Chemical Co., Ltd.)
[0193] (D) Additives
[0194] D-1: Polyethylene (Hydraulic 7000FP manufactured by Mitsui Chemicals Co., Ltd.)
[0195] D-2: Amide compound (Lite Amide WH500 manufactured by Kyoeisha Chemical Co., Ltd.)
[0196] D-3: an organic crystal nucleating agent (polyetheretherketone PEEK450-PF manufactured by Bictlex Emcee Co., Ltd.).
[0197] [Measurement and evaluation method]
[0198] The measurement and evaluation methods in the present examples and comparative examples are as follows.
[0199] (1) Tensile strength
[0200] It was measured in accordance with ISO 527-1, 2 (2012). Specifically, the measurement was carried out as follows. The PPS resin composition particles of the present invention were dried using a hot air dryer at 130 °C for 3 hours, and then supplied to a Sumitomo Heavy Industries, Ltd. injection molding machine (SE-50D) with a barrel temperature set at 310 °C and a mold temperature set at 145 °C. Using a mold of the A1 type test piece shape (4 mm thickness) specified in ISO20753 (2008), injection molding was carried out under the condition that the average velocity of the molten resin passing through the cross-sectional area of the central parallel part was 400 ± 50 mm / s, and test pieces were obtained. After conditioning the test pieces for 16 hours under the conditions of 23 °C and 50% relative humidity, the tensile strength was measured in accordance with ISO 527-1, 527-2 (2012) in an atmosphere of 23 °C and 50% relative humidity under the conditions of a grip distance of 115 mm and a test speed of 5 mm / min. If it is 185 MPa or more, it can be said that the product level is practically problem-free, and the higher this value, the more excellent the mechanical strength, which is preferable.
[0201] (2) Tensile strength retention rate
[0202] The antifreeze was prepared by diluting Volkswagen Genuine LLC (G13) with distilled water to a 50 wt% aqueous solution. At a temperature of 150 °C, a test piece of the A1 type test piece shape (4 mm thickness) specified in ISO 20753 was immersed in the antifreeze for 500 hours, then the attached liquid was wiped off, and after conditioning for 16 hours under the conditions of 23 °C and 50% relative humidity, the tensile strength was measured in accordance with ISO 527-1, 527-2 method in an atmosphere of 23 °C and 50% relative humidity under the conditions of a grip distance of 115 mm and a test speed of 5 mm / min. The value calculated by (tensile strength after antifreeze immersion treatment / tensile strength described in (1)) was expressed as a percentage, and this value was set as the tensile strength retention rate. If it is 75% or more, it can be said that the product level is practically problem-free, and the higher this value, the more excellent the antifreeze resistance, which is preferable.
[0203] (3) Mold contamination
[0204] With Figure 1The mold for gas evaluation of the molded product shown (molded product dimensions: length 55 mm, width 20 mm, thickness 2 mm, gate dimensions: width 2 mm, thickness 1 mm (side gate), vent maximum length 20 mm, width 10 mm, depth 5 μm) was continuously molded at a barrel temperature of 330°C, a mold temperature of 130°C, an injection speed of 100 mm / s, and an injection pressure of 50 to 80 MPa so that the filling time for each resin composition was 0.4 seconds. The mold contamination of the mold vent was visually observed every 10 injections (molding machine used: Sumitomo Heavy Industries "SE-30D"). If the number of injections until adhesion is 100 injections or more, it can be said that it is a level that can be used in practice, and the larger the number of injections, the better the mold fouling resistance, which is preferred.
[0205] (4) Welding strength
[0206] An ASTM 4 dumbbell piece (1.6 mmt) with gates at both ends and a weld line near the center of the test piece was molded using an injection molding machine at a barrel temperature of 320°C and a mold temperature of 135°C. Ten samples were obtained for measurement, and the weld strength was measured under the conditions of a test speed of 10 mm / min and a distance between fixtures of 64 mm. If it is 65 MPa or more, it can be said that it is a product level with no practical problems. The higher the value, the better the mechanical strength, which is preferred.
[0207] (5) Liquidity
[0208] The flow length was measured using a spiral flow mold with a thickness of 1 mm and a barrel temperature of 320°C, a mold temperature of 140°C, an injection speed of 230 mm / sec, an injection pressure of 98 MPa, an injection time of 5 seconds, and a cooling time of 15 seconds (using an injection molding machine: Sumitomo Heavy Industries "SE-30D"). The larger the value, the better the fluidity.
[0209] (6) Melting crystallization peak temperature
[0210] About 10 mg of the pellets of the PPS resin composition were taken as a sample, and the temperature was increased at a rate of 20°C / min using a differential scanning calorimeter DSC-7 manufactured by PerkinElmer. The sample was kept at 340°C for 5 minutes and then cooled at a rate of 20°C / min. The crystallization peak temperature at this time was measured and set as the melt crystallization peak temperature.
[0211] [Manufacturing of PPS resin composition] (Examples 1 to 5, Comparative Examples 1 to 10)
[0212] Using a twin screw extruder (TEM-26 manufactured by Toshiba Machine Co., Ltd.) with a 26 mm diameter intermediate addition port and a barrel temperature set to 320°C and a screw speed set to 400 rpm, 100 parts by weight of the PPS resin (A) obtained in Reference Examples 1 to 6 were added from the raw material supply port at a weight ratio shown in Table 1 to form a molten state, and (B) inorganic filler was supplied from the intermediate addition port at a weight ratio shown in Table 1, and melt kneading was performed at a discharge rate of 30 kg / hour to obtain pellets. The above-mentioned properties were evaluated using the pellets. The results are shown in Tables 1 and 2.
[0213] [Table 1]
[0214]
[0215] [Table 2]
[0216] Table 2
[0217]
[0218] Industrial Availability
[0219] The PPS resin composition obtained in this way has high mechanical strength and antifreeze resistance and also has unknown characteristics such as suppressing the generation of mold deposits. Therefore, it is useful for automobile cooling parts, especially small / complex-shaped automobile cooling parts combining multiple parts.
[0220] Explanation of symbols
[0221] 1. Shell
[0222] 2. Valve
[0223] 3. Axis
[0224] 4. Tube
[0225] 5. Hole
[0226] 6. Pad
[0227] 7. Cavity
[0228] 8. Gate part.
Claims
1. A polyphenylene sulfide resin composition for automobile cooling parts, comprising: (A) 100 parts by weight of a polyphenylene sulfide resin; (B) 30 to 110 parts by weight of a glass fiber; and (C) 0.1 to 3 parts by weight of a silane compound having an isocyanate group; wherein the polyphenylene sulfide resin (A) has a number average molecular weight of 7,000 to 14,000; and when the polyphenylene sulfide resin (A) is dissolved in 20 times the weight of 1-chloronaphthalene at 250° C. for 5 minutes and hot-pressed filtered using a PTFE membrane filter having a pore size of 1 μm, the residual amount is 2.0 to 5.0% by weight. 2 . The polyphenylene sulfide resin composition according to claim 1 , which has a melting crystallization peak temperature of 230° C. or higher.
3. The polyphenylene sulfide resin composition according to claim 1 or 2, which satisfies all of the following conditions (i) and (ii). (i) using an A1 type test piece specified in ISO 20753 obtained by injection molding the polyphenylene sulfide resin composition, the tensile strength measured according to ISO 527-1 or 527-2 under the conditions of a tensile speed of 5 mm / min and an ambient temperature of 23° C. is 190 MPa or more. Hereinafter, the A1 type test piece specified in ISO 20753 obtained by injection molding the polyphenylene sulfide resin composition is referred to as an ISO test piece. (ii) After the ISO test piece is immersed in an antifreeze solution at 150°C for 500 hours, the retention rate of tensile strength measured according to ISO 527-1 or 527-2 at a tensile speed of 5 mm / min and an ambient temperature of 23°C is 80% or more.
4. An automobile cooling component, which is made of the polyphenylene sulfide resin composition according to any one of claims 1 to 3.
5. An automobile cooling component, comprising a housing and at least two tubes, wherein the housing is formed by injection molding the polyphenylene sulfide resin composition according to any one of claims 1 to 3.
6. An automobile cooling component, which is composed of a housing, a valve, and at least three pipes, wherein the housing is formed by injection molding the polyphenylene sulfide resin composition according to any one of claims 1 to 3.