Preparation and inspection methods of test samples for microstructure inspection of polycrystalline tungsten or single crystal tungsten materials
Through electrochemical processing devices and methods, the problem of single crystal tungsten or polycrystalline tungsten material sample preparation and inspection is solved, efficient sample polishing and selective corrosion are achieved, and microstructure information is clearly displayed, meeting the needs of engineering applications. Inspection requirements.
Patent Information
- Application Number
- CN202210260075.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-16
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-03-16
AI Technical Summary
It is difficult to effectively prepare and inspect low-magnification and microstructural samples of single crystal tungsten or polycrystalline tungsten materials with existing technology, resulting in the inability to meet the needs of structural defects and microstructural inspection in engineering applications, and common methods are complicated to operate and time consuming. long, residual scratches on the surface and other problems.
Use electrochemical treatment devices and methods to perform surface treatment on single crystal tungsten or polycrystalline tungsten material samples through electrolytic polishing and selective etching, using electrochemical treatment liquids and specific process parameters to achieve polishing and selective etching of the samples to display crystals Microstructure information such as orientation, large-angle grain boundaries, small-angle grain boundaries, sub-grain boundaries, etc.
It achieves a scratch-free mirror effect on the surface of the sample, simplifies the operation, reduces the requirements for operators, and can clearly and intuitively display the microstructure structure. It is suitable for low-magnification and microstructure inspection of single crystal tungsten or polycrystalline tungsten materials. , improving the accuracy and safety of inspection.
Smart Images

Figure CN114737190B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a device and method for preparing and inspecting low-magnification and microstructure test samples of single-crystal tungsten or polycrystalline tungsten materials. The method can intuitively display the low-magnification organization and microstructure and microstructure (crystal orientation, large-angle grain boundaries, small-angle grain boundaries, subgrain boundaries) information of single-crystal tungsten or polycrystalline tungsten materials in a macroscopic and large-size range. Specifically, it relates to the preparation and inspection of low-magnification and microstructure test samples of single-crystal tungsten or polycrystalline tungsten materials. Specifically, it is a method for electrolytically polishing and selectively corroding the surface to be tested of a single-crystal tungsten or polycrystalline tungsten material sample by using an electrochemical treatment device, an electrochemical treatment liquid and specific process parameters, and using the difference in corrosion resistance of crystal planes with different orientations to display microstructures and microstructures such as crystal orientation, large-angle grain boundaries, small-angle grain boundaries, subgrain boundaries, etc., which can be used to achieve rapid characterization of low-magnification and microstructure of single-crystal tungsten or polycrystalline tungsten materials. Background Art
[0002] Tungsten is the metal material with the highest melting point. It is often used to manufacture parts used in oxygen-free and extremely high temperature environments. It has a wide range of uses in special application fields such as the aerospace field. Tungsten has very high strength and hardness, strong wear resistance, and mechanical processing, especially mechanical polishing, is very difficult. In addition, tungsten has strong corrosion resistance. When not heated, any concentration of hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid and aqua regia have no effect on tungsten. When the temperature rises to 80℃ to 100℃, among the various acids mentioned above, except hydrofluoric acid, other acids have a weak effect on tungsten. At room temperature, a high concentration of hydrofluoric acid and nitric acid mixed acid can dissolve tungsten, but tungsten does not react in alkaline solution.
[0003] At present, the low-magnification and microstructure sample preparation and inspection methods used for conventional metal materials are very difficult to use for polycrystalline tungsten. The main reason is that the mixed acid (a high-concentration mixed acid of hydrofluoric acid and nitric acid) etching solution or Murakami etching solution (an aqueous solution of KOH or NaOH and potassium ferrocyanide) has a weak corrosion ability on tungsten and a small amount of material removal. However, ordinary mechanical processing, metallographic sample preparation sandpaper grinding, and diamond polishing paste polishing have weak ability to remove tungsten surface materials. It is difficult to obtain surface processing quality suitable for mixed acid corrosion. The sample preparation process has extremely high requirements on the operator and the sample preparation time is very long. In addition, scratches left over from the sample preparation process often remain on the sample surface, which seriously affects the low-magnification and microstructure inspection.
[0004] Compared with polycrystalline tungsten, single-crystal tungsten has strong anisotropy, and its strength, hardness and corrosion resistance of specific crystal planes are higher than those of polycrystalline tungsten. The preparation and analysis of low-magnification and microstructure samples are more difficult. To date, there is still a lack of suitable sample preparation methods and inspection methods for low-magnification inspection and microstructure inspection. It is impossible to meet the low-magnification structural defect and microstructure inspection requirements required for single-crystal tungsten or polycrystalline tungsten in engineering applications. Summary of the invention
[0005] The technical problem solved by the present invention is: to overcome the deficiencies of the prior art and to provide a device and method for preparing and inspecting a test sample of single crystal tungsten or polycrystalline tungsten material, which can realize surface polishing and selective corrosion of the test sample.
[0006] The technical solution of the present invention is: a method for preparing a test sample for the microstructure inspection of polycrystalline tungsten or single crystal tungsten material, comprising:
[0007] Cut samples from polycrystalline tungsten or single crystal tungsten materials, and perform surface treatment on the surface to be tested. The surface roughness is equal to or better than Ra6.4;
[0008] After the insulation layers at both ends of the head and tail are stripped, the multiple strands of wires with current carrying capacity are unwound and evenly dispersed into a radial shape; a conductive metal foil having a diameter not less than the diameter of the outer envelope circle of the radial shape is selected, and a hole is punched in the middle of the conductive metal;
[0009] After the above-mentioned multiple strands of wire pass through the through hole in the middle of the conductive metal foil, the conductive metal foil is pushed to the ends of the multiple strands of wire dispersed in a radial shape;
[0010] Polishing the back of the sample to be tested to remove the oxide layer and the contamination layer until the polished area shows a bright metallic color;
[0011] By applying glue to the polishing area, the conductive metal foil is pressed and fixed to the polishing area;
[0012] Detect the resistance between the surface of the sample to be tested and the end of the wire. If the resistance is greater than 1Ω, remove the bonded wire and conductive metal foil and reprocess until the resistance does not exceed 1Ω;
[0013] Use acrylic resin and mold without conductive fillers to embed the sample with bonded wires, ensure that the sample surface to be tested can be exposed after embedding, and the rest of the sample is tightly wrapped in the resin, and remove the mold after curing;
[0014] Detect the resistance between the sample surface to be tested and the end of the wire. If the resistance is greater than 1Ω, remove the embedding resin, the bonded wires and the conductive metal foil, and then start processing again from the wires and conductive metal foils dispersed in a radial shape until the resistance does not exceed 1Ω;
[0015] Polish the test surface of the sample that meets the resistance requirements to obtain a test sample that can be used for tissue inspection.
[0016] Preferably, the grinding of the test surface of the sample whose resistance meets the requirements is completed by the following method:
[0017] Use a turntable grinder and polisher, and use 200#~280#, 500#, 1000#, 2000# diamond grinding discs or silicon carbide water-resistant sandpaper to grind the test surface of the test sample until it is smooth. For each number of sandpaper, first use a grinding disc speed of 150~250 rpm and a positive pressure of 5~20N to obtain the maximum cutting speed. After grinding until the wear marks on the test surface are uniform, rotate the sample 30~90°, continue grinding until uniform scratches are obtained again, then increase the speed to 450~500 rpm, and gradually reduce the positive pressure to 1~5N to obtain a polishing effect.
[0018] Preferably, the insulation layer of the head and tail ends of the multi-strand silver-plated copper wire with a water-resistant and alkali-resistant insulation layer not less than the outer envelope diameter of the sample plus 30 cm is stripped by 5 to 10 mm, and the stripped multi-strand wire heads are unwound and evenly dispersed into a radial shape; the current carrying capacity of the wire is related to the surface area of the sample to be processed, and the current carrying capacity is not less than the surface area of the sample to be processed multiplied by 2A / cm 2 .
[0019] Preferably, the conductive metal foil is aluminum foil or nickel foil with a thickness of 5 to 20 μm.
[0020] Preferably, the acrylic resin without conductive filler is a resin that can be rapidly cured at room temperature within 15 minutes.
[0021] An electrochemical treatment device for tissue inspection of polycrystalline tungsten or single crystal tungsten material, comprising:
[0022] DC regulated power supply: voltage upper limit is not less than 15V, current monitoring accuracy is equal to or better than 0.001A, current output capacity is greater than the surface area of the sample to be processed multiplied by 2A / cm 2 ;
[0023] Test sample: a test sample prepared according to the above method; connected to the positive electrode of a DC regulated power supply and used as an anode in the electrochemical treatment process;
[0024] Stainless steel cathode plate: 304 or 316 stainless steel plate with an area not less than 4 times the area of the test sample to be tested, thickness 2mm~4mm, surface roughness should be equal to or better than Ra1.6; a wire with insulation skin fixed on one edge of the stainless steel plate
[0025] Cathode connecting wire: a wire with insulation used to connect the stainless steel plate; the current carrying capacity of the wire used is greater than the surface area of the sample to be treated multiplied by 2A / cm 2 ;
[0026] Container: used to accommodate the test sample and the stainless steel cathode plate; with fixing measures to ensure that the angle between the test sample surface to be tested and the surface of the stainless steel cathode plate does not exceed 15°, and the distance is 20mm to 80mm; after filling with electrochemical treatment liquid, it can ensure that the test sample surface to be tested is completely immersed below the liquid level.
[0027] A surface polishing method for low-power and microstructure inspection of polycrystalline tungsten or single-crystalline tungsten materials, comprising:
[0028] Filling the electrochemical treatment liquid into the container of the electrochemical treatment device;
[0029] Remove bubbles from the surface of the test sample to be tested, and let it stand until the electrochemical treatment solution in the container of the electrochemical treatment device is stable and free of bubbles;
[0030] Set the DC regulated power supply voltage to 5V~15V, turn on the power supply, and keep it on for 5~10 minutes; check the surface of the sample to be tested. If a bright mirror effect has been formed, the polishing is completed. If there are still traces of mechanical damage, start again from removing the bubbles on the surface of the test sample to be tested until there are no traces of mechanical damage;
[0031] Rinse the test surface of the test sample and blow dry the water stains on the test sample and the test surface.
[0032] Preferably, the filling amount of the electrochemical treatment liquid satisfies that: the minimum distance between the test sample surface to be tested and the liquid surface is greater than 30 mm.
[0033] Preferably, the electrochemical treatment solution comprises analytical grade NaOH and deionized water. The preparation method is to use analytical grade NaOH and deionized water to prepare a 5% to 10% NaOH aqueous solution. After the preparation is completed, the solution is allowed to stand until it returns to room temperature and has no bubbles before use.
[0034] A surface selective etching method for microstructure inspection of polycrystalline tungsten or single crystal tungsten material, comprising:
[0035] S1) using the prepared surface-polished test sample as an anode to replace the test sample in the electrochemical treatment device, and completing the assembly of the electrochemical treatment device;
[0036] S2) adding the electrochemical treatment solution into the container of the electrochemical treatment device;
[0037] S3) removing bubbles from the surface of the test sample to be tested, and allowing the sample to stand until the electrochemical treatment solution in the container of the electrochemical treatment device is stable and free of bubbles;
[0038] S4) Set the DC regulated power supply voltage to 5V to 15V, turn on the power supply, and keep it on for 2 to 3 minutes;
[0039] S5) without turning off the DC regulated power supply, directly adjust the voltage of the DC regulated power supply to 1V-3V, and keep it powered on for 1-3 minutes;
[0040] S6) Check the test surface of the test sample. If the test surface has formed a preset grayscale contrast, go to S7). If the grayscale contrast is insufficient, re-polish the test sample and install it on the electrochemical treatment device, re-execute from S2), and extend the power-on time in S5) or increase the voltage of the DC regulated power supply; if the edge is corroded too heavily to form a depression, re-grind the test surface of the test sample, then re-polish the surface and go to S1) to re-execute.
[0041] S7) Rinse the surface of the test sample to be inspected and blow dry any water stains on the surface of the test sample and the surface to be inspected.
[0042] A low-magnification microstructure inspection method for polycrystalline tungsten or single-crystalline tungsten material, comprising:
[0043] Obtain a test sample after surface selective corrosion according to the method;
[0044] Use a visual inspection method under natural light, supplemented by using a stereo microscope under a 45° oblique illumination light source to inspect the surface of the sample to be inspected. If there is a continuous linear feature and there is a difference in grayscale contrast on both sides of the linear feature, it indicates that the linear feature is a grain boundary. If it is a closed surface feature, it indicates that it is an independent grain, segregation or inclusion.
[0045] A method for testing the microstructure and fine structure of polycrystalline tungsten or single crystal tungsten material, comprising:
[0046] Use a field emission scanning electron microscope to magnify and observe the surface of the test sample after inspection;
[0047] Single crystal tungsten or polycrystalline tungsten <111> The crystal orientation is in the form of a right-angled triangular pyramid, which can be calculated by measuring the length of the three sides. <111> The angle between the crystal plane orientation and the detection plane or the angle is detected by using EBSD or micro-area XRD method;
[0048] When the inspection result is a grain boundary, the specific grain boundary type is determined by combining the observation result of field emission scanning electron microscope with the angle calculated above;
[0049] When the inspection result is segregation or inclusion, the specific type of segregation or inclusion is confirmed by EDS quantification or micro-area XRD.
[0050] Preferably, the field emission scanning electron microscope is set to: 5-15KV, observation at 200-400PA, and magnification of at least 5000 times.
[0051] Preferably, if the field emission scanning electron microscope shows that the etching morphology on both sides of the interface is consistent, but there is a difference in secondary electron symmetry, and the angle between the crystal plane orientations on both sides of the interface does not exceed 2°, then the grain boundary type is a subgrain boundary; if the etching morphology on both sides of the interface is consistent, and the crystal plane orientations on both sides of the interface have an angle of 2° to 10°, then the grain boundary type is a small-angle grain boundary; if the etching morphology characteristics on both sides of the interface are inconsistent, and the angle between the crystal plane orientations on both sides of the interface is greater than 10°, then the grain boundary type is a large-angle grain boundary.
[0052] The beneficial effects of the present invention compared with the prior art are:
[0053] The existing mechanical polishing, mixed acid or Murakami etching solution used in low-power and microstructure inspection of single crystal tungsten and polycrystalline tungsten are not effective, which seriously affects the low-power and microstructure inspection. In addition, high-concentration mixed acid (high-concentration mixed acid of hydrofluoric acid and nitric acid) is dangerous in configuration and use due to its strong corrosiveness. Murakami etching solution (aqueous solution of KOH or NaOH and potassium ferrocyanide) needs to be used in a short period of time at low temperature away from light, otherwise there is a safety risk of highly toxic substances produced by the decomposition of potassium ferrocyanide. The raw materials and waste liquid of the above chemical etching solution are difficult to recycle and the safety is poor.
[0054] The present invention utilizes electrochemical reaction, builds a simple electrochemical treatment device, configures an electrochemical treatment solution (aqueous solution of low-concentration alkali) with simple components and relatively safe, and uses easily controllable voltage parameters to realize electrolytic polishing and selective corrosion as needed. Compared with mechanical polishing, during electrolytic corrosion, the sample undergoes an oxidation reaction at the anode, and the reaction product is directly dissolved in the alkali solution. The amount of surface material removed is large, and surface damage such as scratches can be effectively removed. The operation is simple, the sample size range is large, and the requirements for operators are not high. Electrolytic polishing can obtain a completely scratch-free mirror surface effect. In combination with selective corrosion, segregation, inclusion defects, and microscopic fine structures such as large-angle grain boundaries, small-angle grain boundaries, and even subgrain boundaries can be clearly and intuitively detected. It is particularly suitable for low-magnification and microscopic structural inspection of single-crystal tungsten or polycrystalline tungsten materials. In combination with visual inspection, stereomicroscope inspection, SEM, EDS, EBSD, and micro-area XRD analysis methods, low-magnification structural defects and fine structures of microstructures can be effectively distinguished. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 It is a schematic diagram of the device of the present invention;
[0056] Figure 2 Subgrain boundary display; (a) shows the macroscopic subgrain boundary of polycrystalline tungsten; (b) shows the microscopic subgrain boundary of single crystal tungsten
[0057] Figure 3 (a) and (b) show the macroscopic and microscopic grain boundaries of polycrystalline tungsten respectively;
[0058] Figure 4 (a) and (b) show the macro and micro subgrain boundaries or small-angle grain boundaries of single crystal tungsten respectively. DETAILED DESCRIPTION
[0059] 1. Preparation of test samples:
[0060] (1) Cut samples from polycrystalline tungsten or single crystal tungsten materials using electric spark machining or mechanical machining methods. Grind the sample surface with silicon carbide sandpaper or diamond grinding disc or use a milling machine, lathe or grinder for mechanical processing until the sample surface is flat and smooth with a surface roughness equal to or better than Ra6.4.
[0061] (2) Strip off 5 to 10 mm of insulation from both ends (head and tail) of a multi-strand silver-plated copper wire with a water-resistant and alkali-resistant insulation layer of an appropriate length (usually not less than the diameter of the outer envelope of the sample plus 30 cm), unwind the heads of the stripped multi-strand wires and evenly disperse them in a radial shape. The wire used should have an appropriate current carrying capacity, which is related to the surface area of the sample to be processed and can be calculated by multiplying the surface area of the sample to be processed by 2A / cm 2 Estimate.
[0062] (3) Cut a sheet of conductive metal foil (usually 5-20 μm thick aluminum foil or nickel foil) with a diameter equivalent to the outer envelope circle diameter of the multiple strands of wires uniformly dispersed in a radial shape after unwinding the ends of the multiple strands of wires described in (2), and punch a hole in the middle, the diameter of the hole being equivalent to the outer diameter of the wire described in (2).
[0063] (4) After the wire described in (2) passes through the middle through hole of the conductive metal foil described in (3), the conductive metal foil is pushed to the ends of the multiple wires dispersed in a radial shape described in (2).
[0064] (5) Place the sample described in (1) with the surface to be tested facing downward on a clean flat surface (may be supported by a pad), and polish the exposed back surface with silicon carbide sandpaper to remove the oxide layer and contamination layer until the polished area shows a bright metallic color.
[0065] (6) Apply an appropriate amount of 502 glue to the polished area mentioned in (5).
[0066] (7) Immediately press the heads of the multiple wires with the conductive metal foils dispersed radially in (4) through the conductive metal foils to the area with the 502 glue applied in (6), and press until it solidifies. If any wires leak out of the bonding area, they can be cut off and removed.
[0067] (8) Use a multimeter to test the resistance between the surface of the sample to be tested and the end of the wire mentioned in (2). It should not exceed 1Ω. If the resistance is higher than 1Ω, remove the bonded wire and conductive metal foil and repeat (2) to (7).
[0068] (9) Use an acrylic resin without conductive fillers that cures quickly at room temperature (generally within 15 minutes) and an appropriate mold to embed the sample with the wires bonded in (8). Ensure that the sample surface to be tested can be exposed after embedding, and the rest of the sample should be tightly covered in the resin. Remove the mold after curing.
[0069] (10) Use a multimeter to test the resistance between the sample surface to be tested and the end of the wire. It should not exceed 1Ω. If the resistance is greater than 1Ω, mechanical methods should be used to remove the embedding resin, the bonded wire and the conductive metal foil, and then repeat (2) to (9).
[0070] (11) Use a turntable grinder and polisher to grind the test surface of the test sample with qualified resistance in (10) to a smooth surface using 200#~280#, 500#, 1000#, 2000# diamond grinding discs or silicon carbide water-resistant sandpaper in sequence. For each sandpaper number, first use a grinding disc speed of 150~250 rpm and a positive pressure of 5~20N to obtain the maximum cutting speed. After grinding until the grinding marks on the test surface are uniform, rotate the sample 30~90°, continue grinding until uniform scratches are obtained again, increase the speed to 450~500 rpm, and gradually reduce the positive pressure to 1~5N to obtain a polishing effect. During the process, a continuous stream of water should be used to rinse the surface of the diamond grinding disc or sandpaper to fully remove the grinding products.
[0071] 2. Electrochemical treatment device assembly:
[0072] (1) DC regulated power supply: The upper voltage limit is not less than 15V, and the current monitoring accuracy is equal to or better than 0.001A. The DC regulated power supply should have an appropriate current output capacity. The current output capacity requirement is related to the surface area of the sample to be processed, which can be calculated by multiplying the surface area of the sample to be processed by 2A / cm 2 Estimate.
[0073] (2) Test samples: Test samples prepared according to the method in 1.
[0074] (3) Stainless steel cathode plate: A 304 or 316 stainless steel plate with an area not less than 4 times the area of the test sample in method 1, with a thickness of 2 mm to 4 mm. The surface of the stainless steel plate should be flat, and the surface roughness should be equal to or better than Ra1.6. A hole is punched on one edge of the stainless steel plate and stainless steel screws and nuts are installed to fix the wires described in (4).
[0075] (4) Cathode connecting wire: A wire with insulation used to connect the stainless steel plate mentioned in (3). The wire used should have an appropriate current carrying capacity, which is related to the surface area of the sample to be processed and can be calculated by multiplying the surface area of the sample to be processed by 2A / cm 2 Estimate.
[0076] (5) Container: A water-resistant and alkali-resistant container (usually a glass or quartz beaker can be used). Its volume should ensure that: it can accommodate the test sample described in (2) and the stainless steel cathode plate described in (3); it has fixing measures to ensure that the test surface of the test sample described in (2) is approximately parallel to the surface of the stainless steel cathode plate described in (3) (the angle does not exceed 15°, and the distance is 20mm to 80mm); after filling with electrochemical treatment liquid, it can ensure that the test surface of the test sample described in (2) can be completely immersed below the liquid surface (the minimum distance between the test surface and the liquid surface is recommended to be greater than 30mm).
[0077] (6) Attachment Figure 1 The tail end of the wire of the test sample prepared according to the method in 1 is connected to the positive electrode of the DC regulated power supply, and one end of the sample to be tested is placed in a container; one end of the cathode connecting wire is connected to the negative electrode of the DC regulated power supply, and the other end is fixedly connected to the punched position on one side of the edge of the stainless steel cathode plate with screws and nuts; the screw nut on one side of the stainless steel cathode plate is connected to one end of the cathode connecting wire, and the connection with the cathode connecting wire is used as the upper end, and is vertically inserted into the container; the angle between the test sample to be tested and the surface of the stainless steel cathode plate fixed in the container does not exceed 15°, and the distance is 20mm to 80mm, and electrochemical treatment liquid is added to ensure that the test sample to be tested is completely immersed below the liquid level.
[0078] 3. Preparation of electrochemical treatment solution:
[0079] (1) The electrochemical treatment solution includes analytical grade NaOH and deionized water.
[0080] (2) Use the analytical grade NaOH and deionized water described in (1) to prepare a 5% to 10% NaOH aqueous solution. The total volume of the electrolyte depends on the container used in 2(5) and the sample fixing position. After the electrolyte is filled, it should be ensured that the surface of the sample to be treated is not less than 30 mm from the liquid surface.
[0081] (3) After the electrolyte is prepared, let it stand until the solution returns to room temperature, becomes transparent and free of bubbles before use.
[0082] 4. Electrochemical surface polishing:
[0083] (1) Prepare the test sample as described in 1.
[0084] (2) Assemble the electrochemical treatment device as described in 2.
[0085] (3) Prepare the electrochemical treatment solution as described in 3.
[0086] (4) Add the electrochemical treatment solution described in (3) into the container of the electrochemical treatment device described in (2), and the amount of the solution added should comply with the requirements of 2(5).
[0087] (5) Observe the test surface of the test sample. If there are bubbles, tap the test sample with a glass rod or stir the electrochemical treatment solution near the test surface to remove them.
[0088] (6) Allow the electrochemical treatment solution in the electrochemical treatment device container to stand until it is stable and free of bubbles.
[0089] (7) Set the DC regulated power supply voltage to 5V to 15V, turn on the power, and keep it on for 5 to 10 minutes.
[0090] (8) During the power-on process, the electrochemical treatment liquid must not be disturbed or stirred to avoid sudden changes in current.
[0091] (9) After the power-on time described in (7) is reached, check the surface of the sample to be tested. If a bright mirror effect has been formed, polishing is completed. If there are still signs of mechanical damage, repeat (5) to (9).
[0092] (10) Rinse the test surface of the test sample that has passed the inspection in (9) under running tap water, and then use compressed air to blow dry the water stains on the test sample and the test surface.
[0093] 5. Electrochemical surface selective corrosion:
[0094] (1) Prepare the test specimen with the test surface polished as described in 4.
[0095] (2) Assemble the electrochemical treatment device as described in 2.
[0096] (3) Prepare the electrochemical treatment solution as described in 3.
[0097] (4) Add the electrochemical treatment solution described in (3) into the container of the electrochemical treatment device described in (2), and the amount of the solution added should comply with the requirements of 2(5).
[0098] (5) Observe the test surface of the test sample. If there are bubbles, tap the test sample with a glass rod or stir the electrochemical treatment solution near the test surface to remove them.
[0099] (6) Allow the electrochemical treatment solution in the electrochemical treatment device container to stand until it is stable and free of bubbles.
[0100] (7) Set the DC regulated power supply voltage to 5V to 15V, turn on the power, and keep it on for 2 to 3 minutes.
[0101] (8) Without turning off the power supply, directly adjust the DC regulated power supply voltage to 1V~3V and keep the power on for 1~3 minutes.
[0102] (9) During the power-on process, the electrochemical treatment liquid must not be disturbed or stirred to avoid sudden changes in current.
[0103] (10) After reaching the power-on time described in (7), check the surface of the sample to be tested. If the surface to be tested has formed an appropriate grayscale contrast, the selective etching is completed. If the contrast is insufficient, repeat the surface polishing described in 4 and (1) to (10) and appropriately extend the power-on time in (8) or increase the voltage in (8) until the surface to be tested obtains an appropriate grayscale contrast. If the edge is corroded too heavily to form a depression, the surface of the sample to be tested can be reprocessed using the method described in 1 (11) and then selectively etched according to the surface polishing described in 4 and (1) to (10).
[0104] (11) Rinse the test surface of the test sample that has passed the inspection in (10) under running tap water, and then use compressed air to blow dry the water stains on the test sample and the test surface.
[0105] 6. Low-magnification tissue inspection:
[0106] (1) Obtain test samples as described in 1.
[0107] (2) Assemble the electrochemical treatment device as described in 2.
[0108] (3) Prepare the electrochemical treatment solution as described in 3.
[0109] (4) Polish the surface to be inspected as described in 4.
[0110] (5) Selectively etch the surface to be inspected after polishing as described in 5 to obtain a sample having an appropriate grayscale contrast formed on the surface to be inspected.
[0111] (6) Visual inspection method is used under natural light, supplemented by using a stereo microscope to inspect the surface of the sample described in (5) under a 45° oblique illumination light source. Continuous linear features and differences in grayscale contrast on both sides of the linear features indicate that the linear features are grain boundaries. The specific grain boundary types (large-angle grain boundaries, small-angle grain boundaries, subgrain boundaries) need to be further confirmed by micro-area XRD, EBSD, SEM, and EDS. Closed surface features indicate segregation or inclusions, and the specific types need to be further confirmed by SEM and EDS.
[0112] 7. Microstructure and fine structure inspection:
[0113] (1) Obtain test samples as described in 1.
[0114] (2) Assemble the electrochemical treatment device as described in 2.
[0115] (3) Prepare the electrochemical treatment solution as described in 3.
[0116] (4) Polish the surface to be inspected as described in 4.
[0117] (5) Selectively etch the surface to be inspected after polishing as described in 5 to obtain a sample having an appropriate grayscale contrast formed on the surface to be inspected.
[0118] (6) Use a field emission scanning electron microscope to magnify and observe (generally more than 5000 times) the surface to be inspected.
[0119] (7) Single crystal tungsten or polycrystalline tungsten <111> The crystal orientation is in the form of a right-angled triangular pyramid, which can be calculated by measuring the length of the three sides. <111> The angle between the crystal plane orientation and the detection plane.
[0120] (8) The two sides of the subgrain boundary are observed in a scanning electron microscope at 15KV and 400PA (usually at least 5000 times magnification is required). The etching morphology on both sides of the interface should be consistent, but there is a difference in secondary electron dimensionality. The angle between the crystal plane orientations on both sides of the interface does not exceed 2°. The crystal plane angle can be detected by method (7) or by using EBSD or micro-area XRD methods.
[0121] (9) When observing the two sides of the small-angle grain boundary in a scanning electron microscope at 15KV and 400PA (usually at least 5000 times magnification is required), the etching morphology on both sides of the interface should be basically consistent. The crystal plane orientation on both sides of the interface is allowed to have an angle of 2° to 10°. It can be detected by method (7) or using EBSD or micro-area XRD method.
[0122] (10) When observing the two sides of the large-angle grain boundary in a scanning electron microscope at 15KV and 400PA (usually at least 2000 times magnification is required), the etching morphology on both sides of the interface should be significantly different, and the angle between the crystal plane orientations on both sides of the interface should be greater than 10°. This can be detected by method (7) or using EBSD or micro-area XRD methods.
[0123] (11)6(6) is preliminarily judged as segregation or inclusion: SEM and EDS detection show that the morphology or composition is significantly different from that of the normal matrix. The specific segregation type or inclusion type can be further confirmed by EDS quantification or micro-area XRD.
[0124] Embodiment 1:
[0125] A certain type of tungsten single crystal sample with a circular cross section (about 12 mm in diameter) and a thickness of about 2 mm was obtained by wire cutting.
[0126] Strip off the insulation layer of one end (head) of a 55# tetrafluoroethylene-bonded multi-strand silver-plated copper wire with a length of about 40cm, unwind the stripped multi-strand wire and evenly disperse it into a radial shape, prepare a sheet of conductive nickel foil, cut it into a circle with a diameter of about 12mm, punch a hole in the center, and the hole diameter is equivalent to the outer diameter of the wire. After the wire passes through the center hole, push the metal foil to the head of the multi-strand wire dispersed into a radial shape, apply 502 glue along the annular direction on the back of the surface to be tested of the tungsten single crystal sample, press the head of the radial multi-strand wire to the glue application surface through the metal foil, and cut off the wire that leaks out of the bonding area. Press until the 502 glue is solidified, and use a multimeter to detect the resistance between the surface to be tested of the tungsten single crystal and the tail end of the wire, which is 0.7Ω.
[0127] Use acrylic resin without conductive fillers and a round mold to embed the sample with bonded wires, so that the surface to be tested can be exposed after embedding, and the rest of the sample is tightly wrapped in the resin. After curing, remove the mold and use a multimeter to detect the resistance between the surface to be tested and the tail end of the wire, which is 0.7Ω.
[0128] Use a turntable grinder and polisher to grind the surface of the tungsten single crystal sample to be tested smooth using 240#, 500#, 1000#, and 2000# silicon carbide water-resistant sandpaper in turn. Each sandpaper number is first used with a grinding disc speed of 200 rpm and a positive pressure of 10N to obtain the maximum cutting speed. After grinding until the scratches on the surface to be tested are uniform, rotate the sample 60°, continue grinding until uniform scratches are obtained again, increase the speed to 500 rpm, and gradually reduce the positive pressure to 5N to obtain a polishing effect. During the process, use a continuous stream of water to rinse the surface of the diamond grinding disc or sandpaper to remove the grinding products.
[0129] Use deionized water to prepare a 5% NaOH aqueous solution. Use a DC regulated power supply, a stainless steel plate, an insulated wire, and a 500mL beaker to build an electrolytic corrosion device. The stainless steel plate is connected to the negative pole of the DC regulated power supply with a wire. The tail end of the wire on the polished sample is connected to the positive pole of the DC regulated power supply. The stainless steel plate and the sample are placed in the beaker. Fix the sample so that the surface to be tested is approximately parallel to the stainless steel plate, with an angle of no more than 15 degrees and a distance of about 30 to 35 mm. Pour the prepared 5% NaOH aqueous solution into the beaker so that the test surface of the sample is completely immersed about 35 mm below the liquid surface. Use a glass rod to tap the sample to remove surface bubbles.
[0130] After the solution is stable, set the voltage regulator to 6V, start the power supply, and continue electrolytic polishing for 5 minutes. After the power is turned on, check the test surface of the sample to form a bright mirror effect.
[0131] Continue to put the sample into the beaker to the same installation position as the above polishing, use a glass rod to tap the sample to remove surface bubbles, after the solution stabilizes, set the voltage regulator to 6V, start the power supply, and continue electrolytic polishing for 2 minutes. After that, do not turn off the power, set the voltage regulator to 1V, and continue electrolytic selective corrosion for 1.5 minutes. Take it out and check. The surface to be inspected has formed appropriate grayscale contrast and the interface characteristics are visible.
[0132] Further observation using SEM showed that the cross-sectional interface features were subgrain boundaries and the crystal planes were <111> Crystal surface, see attached Figure 2 .
[0133] Embodiment 2:
[0134] A square sample (about 10 mm × 10 mm in side length) of a certain type of polycrystalline tungsten plate with a thickness of about 4 mm was obtained by wire cutting.
[0135] Strip off the insulation layer of one end (head) of a 55# tetrafluoroethylene-bonded multi-strand silver-plated copper wire with a length of about 40cm, unwind the stripped multi-strand wire and evenly disperse it into a radial shape, prepare a sheet of conductive nickel foil, cut it into a circle with a diameter of about 12mm, punch a hole in the center, and the hole diameter is equivalent to the outer diameter of the wire. After the wire passes through the center hole, push the metal foil to the head of the multi-strand wire dispersed into a radial shape, apply 502 glue along the annular direction on the back of the surface to be tested of the tungsten single crystal sample, press the head of the radial multi-strand wire to the glue application surface through the metal foil, and cut off the wire that leaks out of the bonding area. Press until the 502 glue is solidified, and use a multimeter to detect the resistance between the surface to be tested of the tungsten single crystal and the tail end of the wire, which is 0.6Ω.
[0136] Use acrylic resin without conductive fillers and a round mold to embed the sample with bonded wires, so that the surface to be tested can be exposed after embedding, and the rest of the sample is tightly wrapped in the resin. After curing, remove the mold and use a multimeter to detect the resistance between the surface to be tested and the tail end of the wire, which is 0.6Ω.
[0137] Use a turntable grinder and polisher to grind the surface of the tungsten single crystal sample to be tested smooth using 240#, 500#, 1000#, and 2000# silicon carbide water-resistant sandpaper in turn. Each sandpaper number is first used with a grinding disc speed of 200 rpm and a positive pressure of 10N to obtain the maximum cutting speed. After grinding until the scratches on the surface to be tested are uniform, rotate the sample 60°, continue grinding until uniform scratches are obtained again, increase the speed to 500 rpm, and gradually reduce the positive pressure to 5N to obtain a polishing effect. During the process, use a continuous stream of water to rinse the surface of the diamond grinding disc or sandpaper to remove the grinding products.
[0138] Use deionized water to prepare a 5% NaOH aqueous solution. Use a DC regulated power supply, a stainless steel plate, an insulated wire, and a 500mL beaker to build an electrolytic corrosion device. The stainless steel plate is connected to the negative pole of the DC regulated power supply with a wire. The tail end of the wire on the polished sample is connected to the positive pole of the DC regulated power supply. The stainless steel plate and the sample are placed in the beaker. Fix the sample so that the surface to be tested is approximately parallel to the stainless steel plate, with an angle of no more than 15 degrees and a distance of about 30 to 35 mm. Pour the prepared 5% NaOH aqueous solution into the beaker so that the test surface of the sample is completely immersed about 35 mm below the liquid surface. Use a glass rod to tap the sample to remove surface bubbles.
[0139] After the solution is stable, set the voltage regulator to 5V, start the power supply, and continue electrolytic polishing for 8 minutes. After the power is turned on, check the test surface of the sample to form a bright mirror effect.
[0140] Continue to put the sample into the beaker to the same installation position as the above polishing, use a glass rod to tap the sample to remove surface bubbles, after the solution stabilizes, set the voltage regulator to 5V, start the power supply, and continue electrolytic polishing for 2 minutes. After that, do not turn off the power, set the voltage regulator to 1.5V, and continue electrolytic selective etching for 1 minute. After taking it out for inspection, the surface to be inspected has formed appropriate grayscale contrast, and significant grain boundaries and polycrystalline characteristics can be seen, without obvious segregation and inclusions.
[0141] Further observation using SEM revealed the characteristics of large-angle grain boundaries, see attached Figure 3 .
[0142] Embodiment 3:
[0143] A certain type of single crystal tungsten sample with a rectangular axial longitudinal section (side length of about 12mm×20mm) and a thickness of about 4mm was obtained by wire cutting.
[0144] Strip off the insulation layer of one end (head) of a 55# tetrafluoroethylene-bonded multi-strand silver-plated copper wire with a length of about 40cm, unwind the stripped multi-strand wire and evenly disperse it into a radial shape, prepare a sheet of conductive nickel foil, cut it into a circle with a diameter of about 10mm, punch a hole in the center, and the hole diameter is equivalent to the outer diameter of the wire. After the wire passes through the center hole, push the metal foil to the head of the multi-strand wire dispersed into a radial shape, apply 502 glue along the annular direction on the back of the surface to be tested of the tungsten single crystal sample, press the head of the radial multi-strand wire to the glue application surface through the metal foil, and cut off the wire that leaks out of the bonding area. Press until the 502 glue is solidified, and use a multimeter to detect the resistance between the surface to be tested of the tungsten single crystal and the tail end of the wire, which is 0.8Ω.
[0145] Use acrylic resin without conductive fillers and a round mold to embed the sample with bonded wires, so that the surface to be tested can be exposed after embedding, and the rest of the sample is tightly wrapped in the resin. After curing, remove the mold and use a multimeter to detect the resistance between the surface to be tested and the tail end of the wire, which is 0.8Ω.
[0146] Use a turntable grinder and polisher to grind the surface of the tungsten single crystal sample to be tested smooth using 240#, 500#, 1000#, and 2000# silicon carbide water-resistant sandpaper in turn. Each sandpaper number is first used with a grinding disc speed of 200 rpm and a positive pressure of 10N to obtain the maximum cutting speed. After grinding until the scratches on the surface to be tested are uniform, rotate the sample 60°, continue grinding until uniform scratches are obtained again, increase the speed to 500 rpm, and gradually reduce the positive pressure to 5N to obtain a polishing effect. During the process, use a continuous stream of water to rinse the surface of the diamond grinding disc or sandpaper to remove the grinding products.
[0147] Use deionized water to prepare a 5% NaOH aqueous solution. Use a DC regulated power supply, a stainless steel plate, an insulated wire, and a 500mL beaker to build an electrolytic corrosion device. The stainless steel plate is connected to the negative pole of the DC regulated power supply with a wire. The tail end of the wire on the polished sample is connected to the positive pole of the DC regulated power supply. The stainless steel plate and the sample are placed in the beaker. Fix the sample so that the surface to be tested is approximately parallel to the stainless steel plate, with an angle of no more than 15 degrees and a distance of about 30 to 35 mm. Pour the prepared 5% NaOH aqueous solution into the beaker so that the test surface of the sample is completely immersed about 35 mm below the liquid surface. Use a glass rod to tap the sample to remove surface bubbles.
[0148] After the solution is stable, set the voltage regulator to 6V, start the power supply, and continue electrolytic polishing for 5 minutes. After the power is turned on, check the test surface of the sample to form a bright mirror effect.
[0149] Continue to put the sample into the beaker to the same installation position as the above polishing, use a glass rod to tap the sample to remove the surface bubbles, and after the solution stabilizes, set the voltage regulator to 6V, start the power supply, and continue electrolytic polishing for 2 minutes. Then, do not turn off the power supply, set the voltage regulator to 1V, and continue electrolytic selective corrosion for 1.5 minutes. After taking it out, check that no appropriate grayscale contrast is formed on the surface to be inspected. Perform electrolytic polishing again at 6V and 8 minutes, then set the voltage regulator to 6V, start the power supply, and continue electrolytic polishing for 2 minutes. Then, do not turn off the power supply, set the voltage regulator to 1V, and continue electrolytic selective corrosion for 3 minutes. After taking it out, check that significant interface features can be seen, and no obvious segregation and inclusions are found.
[0150] Further SEM observation revealed small-angle grain boundaries and subgrain boundaries. Figure 4 .
[0151] Parts not described in detail in the present invention belong to common knowledge of those skilled in the art.
Claims
1. A surface selective etching method for the microstructure inspection of polycrystalline tungsten or single crystal tungsten materials, characterized in that include: S1) using the prepared surface-polished test sample as an anode to replace the test sample in the electrochemical treatment device, and completing the assembly of the electrochemical treatment device; The surface-polished test specimens were prepared by the following steps: Filling the electrochemical treatment solution into the container of the electrochemical treatment device; Remove bubbles from the surface of the test sample to be tested, and let it stand until the electrochemical treatment solution in the container of the electrochemical treatment device is stable and free of bubbles; Set the DC regulated power supply voltage to 5V~15V, turn on the power supply, and keep it on for 5~10 minutes; check the surface of the sample to be tested. If a bright mirror effect has been formed, the polishing is completed. If there are still traces of mechanical damage, start again from removing the bubbles on the surface of the test sample to be tested until there are no traces of mechanical damage; Rinse the test sample surface to be inspected and blow dry the water stains on the test sample and the surface to be inspected; The electrochemical treatment device comprises: DC regulated power supply: voltage upper limit is not less than 15V, current monitoring accuracy is equal to or better than 0.001A, current output capacity is greater than the surface area of the sample to be processed multiplied by 2A / cm 2 ; Test sample: Connect to the positive electrode of the DC regulated power supply and serve as the anode during the electrochemical treatment process; Stainless steel cathode plate: 304 or 316 stainless steel plate with an area not less than 4 times the area of the test sample to be tested, thickness 2mm~4mm, surface roughness should be equal to or better than Ra1.6; a wire with insulation skin is fixed on one edge of the stainless steel plate; Cathode connecting wire: a wire with insulation used to connect the stainless steel plate; the current carrying capacity of the wire used is greater than the surface area of the sample to be treated multiplied by 2A / cm 2 ; Container: used to contain the test sample and the stainless steel cathode plate; with fixing measures to ensure that the angle between the test sample surface to be tested and the surface of the stainless steel cathode plate does not exceed 15°, and the distance is 20mm to 80mm; after filling with electrochemical treatment liquid, it can ensure that the test sample surface to be tested is completely immersed below the liquid surface; S2) adding the electrochemical treatment solution into the container of the electrochemical treatment device; S3) removing bubbles from the surface of the test sample to be tested, and allowing the sample to stand until the electrochemical treatment solution in the container of the electrochemical treatment device is stable and free of bubbles; S4) Set the DC regulated power supply voltage to 5V to 15V, turn on the power supply, and keep it on for 2 to 3 minutes; S5) without turning off the DC regulated power supply, directly adjust the voltage of the DC regulated power supply to 1V-3V, and keep it powered on for 1-3 minutes; S6) Check the surface of the sample to be tested. If the surface to be tested has formed a preset grayscale contrast, go to S7). If the grayscale contrast is insufficient, re-polish the surface of the test sample and then install it on the electrochemical treatment device, re-execute from S2), and extend the power-on time in S5) or increase the voltage of the DC regulated power supply; If the edge corrosion is too severe to form a depression, the surface to be tested of the test sample is re-grinded, and then the surface is re-polished and the process is executed again in step S1); S7) Rinse the surface of the test sample to be inspected and blow dry any water stains on the surface of the test sample and the surface to be inspected.
2. The surface selective corrosion method according to claim 1, characterized in that: The filling amount of electrochemical treatment liquid meets the requirement that the minimum distance between the test sample surface to be tested and the liquid surface is greater than 30mm.
3. The surface selective corrosion method according to claim 1, characterized in that: The electrochemical treatment solution comprises analytical pure NaOH and deionized water. The preparation method is to use analytical pure NaOH and deionized water to prepare a 5% to 10% NaOH aqueous solution. After the preparation is completed, the solution is allowed to stand until it returns to room temperature and has no bubbles before use.
4. The surface selective corrosion method according to claim 1, characterized in that: The test samples were prepared in the following manner: Cut samples from polycrystalline tungsten or single crystal tungsten materials, and perform surface treatment on the surface to be tested. The surface roughness is equal to or better than Ra6.4; After the insulation layers at both ends of the head and tail are stripped, the multiple strands of wires with current carrying capacity are unwound and evenly dispersed into a radial shape; a conductive metal foil having a diameter not less than the diameter of the outer envelope circle of the radial shape is selected, and a hole is punched in the middle of the conductive metal; After the above-mentioned multiple strands of wire pass through the through hole in the middle of the conductive metal foil, the conductive metal foil is pushed to the ends of the multiple strands of wire dispersed in a radial shape; Polishing the back of the sample to be tested to remove the oxide layer and the contamination layer until the polished area shows a bright metallic color; By applying glue to the polishing area, the conductive metal foil is pressed and fixed to the polishing area; Detect the resistance between the surface of the sample to be tested and the end of the wire. If the resistance is greater than 1Ω, remove the bonded wire and conductive metal foil and reprocess until the resistance does not exceed 1Ω; Use acrylic resin and mold without conductive fillers to embed the sample with bonded wires, ensure that the sample surface to be tested can be exposed after embedding, and the rest of the sample is tightly wrapped in the resin, and remove the mold after curing; Detect the resistance between the sample surface to be tested and the end of the wire. If the resistance is greater than 1Ω, remove the embedding resin, the bonded wires and the conductive metal foil, and then start processing again from the wires and conductive metal foils dispersed in a radial shape until the resistance does not exceed 1Ω; The test surface of the sample to be tested is polished to meet the resistance requirements to obtain the test sample before surface polishing.
5. The surface selective corrosion method according to claim 4, characterized in that: The grinding of the test surface of the sample whose resistance meets the requirements is completed by the following method: Use a turntable grinder and polisher, and use 200#~280#, 500#, 1000#, 2000# diamond grinding discs or silicon carbide water-resistant sandpaper to grind the test surface of the test sample until it is smooth. For each number of sandpaper, first use a grinding disc speed of 150~250 rpm and a positive pressure of 5~20N to obtain the maximum cutting speed. After grinding until the wear marks on the test surface are uniform, rotate the sample 30~90°, continue grinding until uniform scratches are obtained again, then increase the speed to 450~500 rpm, and gradually reduce the positive pressure to 1~5N to obtain a polishing effect.
6. The surface selective corrosion method according to claim 4, characterized in that: Strip off 5 to 10 mm of the insulation layer at both ends of the head and tail of a multi-strand silver-plated copper wire with a water-resistant and alkali-resistant insulation layer that is not less than the outer envelope diameter of the sample plus 30 cm, unwind the stripped heads of the multi-strand wires and evenly disperse them into a radial shape; the current carrying capacity of the wire is related to the surface area of the sample to be processed, and the current carrying capacity is not less than the surface area of the sample to be processed multiplied by 2A / cm 2 .
7. The surface selective corrosion method according to claim 4, characterized in that: The conductive metal foil is selected from aluminum foil or nickel foil with a thickness of 5 to 20 μm.
8. The surface selective corrosion method according to claim 4, characterized in that: The acrylic resin without conductive filler is selected to be a resin that can be quickly cured at room temperature within 15 minutes.
9. A method for low-magnification microstructure inspection of polycrystalline tungsten or single-crystalline tungsten material, characterized in that include: Obtain a test sample after surface selective corrosion according to the method of claim 1; Use a visual inspection method under natural light, supplemented by using a stereo microscope under a 45° oblique illumination light source to inspect the surface of the sample to be inspected. If there is a continuous linear feature and there is a difference in grayscale contrast on both sides of the linear feature, it indicates that the linear feature is a grain boundary. If it is a closed surface feature, it indicates that it is an independent grain, segregation or inclusion.
10. A method for testing the microstructure and fine structure of polycrystalline tungsten or single crystal tungsten material, characterized in that include: Using a field emission scanning electron microscope to magnify and observe the surface to be inspected of the test sample after the inspection of claim 9; Single crystal tungsten or polycrystalline tungsten <111> The crystal orientation is in the form of a right-angled triangular pyramid, which can be calculated by measuring the length of the three sides. <111> The angle between the crystal plane orientation and the detection plane or the angle is detected by using EBSD or micro-area XRD method; When the inspection result of claim 9 is a grain boundary, the specific grain boundary type is determined by combining the observation result of the field emission scanning electron microscope with the above calculated angle; When the result of the inspection in claim 9 is segregation or inclusion, the specific type of segregation or inclusion is confirmed by EDS quantification or micro-area XRD.
11. The inspection method according to claim 10, characterized in that: The settings of the field emission scanning electron microscope are: 5-15KV, observation at 200-400PA, and magnification of at least 5000 times.
12. The inspection method according to claim 10, characterized in that: If the field emission scanning electron microscope shows that the etching morphology on both sides of the interface is consistent, but there is a difference in secondary electron symmetry, and the angle between the crystal plane orientations on both sides of the interface does not exceed 2°, then the grain boundary type is a subgrain boundary; if the etching morphology on both sides of the interface is consistent, and the crystal plane orientations on both sides of the interface have an angle of 2° to 10°, then the grain boundary type is a small-angle grain boundary; if the etching morphology characteristics on both sides of the interface are inconsistent, and the angle between the crystal plane orientations on both sides of the interface is greater than 10°, then the grain boundary type is a large-angle grain boundary.
Citation Information
Patent Citations
Metallographic corrosive, corrosion method for tungsten and display method for metallographic structure of tungsten
CN102519776A
Electropolishing preparation method of sample for EBSD (Electron Back-Scattered Diffraction) analysis of titanium-aluminum alloy
CN107402150A
Electrolytic polishing method of metal part
CN108396368A
Method for preparing metal material EBSD (electron backscatter diffraction) sample on basis of ultra-low temperature weak current control