Electrode intermediate product, electrode powder, electrode using the same, electrode particles using the same, and preparation methods thereof

By preparing a negative electrode containing an electrode intermediate product of the first metal coating and a lithium compound powder state, and combining biomass to prepare a three-dimensional structure electrode powder, the deficiencies in charge and discharge efficiency, stability and lifespan of secondary battery electrode materials are solved. High-performance electrode material preparation was achieved.

CN114747046BActive Publication Date: 2024-10-29IND UNIV COOP FOUND HANYANG UNIV ERICA CAMPUS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202080083335.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-15
Publication Date
2024-10-29
Estimated Expiration
2040-10-15

AI Technical Summary

Technical Problem

Existing secondary battery electrode materials have deficiencies in charge and discharge efficiency, stability and lifespan, making it difficult to meet the high performance requirements of secondary batteries for vehicles.

Method used

By preparing an electrode intermediate product including basic particles of the first metal coating and a second metal melt source, forming an electrode film or particles with a uniform alloy composition, or using the powder state of a lithium compound and a conductive substance to form a negative electrode activity on the current collector Material layer, combined with biomass, prepares silicon oxide electrode powder with a three-dimensional structure to improve the charge and discharge characteristics and stability of the electrode material.

Benefits of technology

It achieves high charge and discharge characteristics, long life and stability of the secondary battery electrode material, simplifies the preparation process, reduces the cost, and is suitable for the high performance requirements of secondary batteries for vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114747046B_ABST
    Figure CN114747046B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing an electrode intermediate product. The method for preparing the electrode intermediate product may include: preparing elementary particles; mixing the elementary particles and a coating source containing a first metal to form a coating containing the first metal on the surface of the elementary particles; and heat treating the elementary particles formed with the coating and a second metal to form a molten source formed by melting the elementary particles formed with the coating and the second metal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to an electrode intermediate product, an electrode using the same, electrode particles using the same, and methods for preparing the same. More specifically, it relates to an electrode intermediate product comprising basic particles having a coating formed thereon comprising a first metal and a molten source of a molten second metal, an electrode using the same, electrode particles using the same, and methods for preparing the same.

[0002] Furthermore, the present application relates to electrode powder, an electrode using the same, and a method for preparing the same, and more particularly, to electrode powder for a secondary battery, an electrode using the same, and a method for preparing the same. Background Art

[0003] While the global secondary battery market was dominated by the initial growth of small information technology (IT) devices such as smartphones, the secondary battery market for vehicles has grown rapidly with the recent growth of the electric vehicle market.

[0004] Secondary batteries for vehicles are leading the growth of the electric vehicle market as they achieve low prices and stable performance through mass production and technological development based on product standardization. Their growth is rapidly expanding as the range problem, which has been blamed as a shortcoming of electric vehicles, is solved by improving battery performance.

[0005] With the explosive growth in demand for secondary batteries, the development of a new generation of secondary batteries is also being actively carried out to meet the demand for secondary battery safety and increased battery capacity.

[0006] For example, Korean Patent Gazette No. 10-1788232 discloses an electrode for a secondary battery, in which an electrode mixture comprising an electrode active material and a binder is applied to a collector, characterized in that it comprises: a first binder and an electrode active material having a glass transition temperature (Tg) lower than that of the second binder described below; a first electrode mixture layer applied on the collector and a second binder and an electrode active material having a glass transition temperature higher than that of the first binder; and a second electrode mixture applied on the first electrode mixture layer, wherein the glass transition temperature of the first binder is below 15°C, the glass transition temperature of the second binder is above 10°C within a range higher than the glass transition temperature of the first binder, the glass transition temperature of the second binder is a temperature greater than or equal to 10°C and less than 25°C within a range higher than the glass transition temperature of the first binder, the electrode for a secondary battery is a negative electrode, and the electrode active material comprises a Si-based substance. Summary of the invention

[0007] Technical issues

[0008] A technical problem to be solved by the present application is to provide an electrode intermediate product, an electrode using the same, electrode particles using the same, and a preparation method thereof.

[0009] Another technical problem to be solved by the present application is to provide an electrode intermediate product for a secondary battery capable of improving the charge and discharge efficiency, an electrode using the intermediate product, an electrode particle using the intermediate product, and a preparation method thereof.

[0010] Another technical problem to be solved by the present application is to provide an electrode intermediate product for secondary batteries with high stability and long life, an electrode using the intermediate product, an electrode particle using the intermediate product, and a preparation method thereof.

[0011] Another technical problem to be solved by the present application is an electrode intermediate product for an all-solid-state battery, an electrode using the intermediate, electrode particles using the intermediate, and a method for preparing the intermediate.

[0012] Another technical problem to be solved by the present application is to provide electrode powder, electrodes using the same, and methods for preparing the same.

[0013] Another technical problem to be solved by the present application is to provide an electrode powder for a secondary battery capable of improving the charge and discharge efficiency, an electrode using the same, and a method for preparing the same.

[0014] Another technical problem to be solved by the present application is to provide an electrode powder for a secondary battery with high stability and long life, an electrode using the same, and a method for preparing the same.

[0015] Another technical problem to be solved by the present application is to provide electrode powder for all-solid-state batteries, electrodes using the same, and methods for preparing the same.

[0016] The technical problems to be solved by this application are not limited to the above-mentioned technical problems.

[0017] Solutions to the problem

[0018] In order to solve the above technical problems, the present application provides a method for preparing an electrode intermediate product.

[0019] According to one embodiment, the preparation method of the above-mentioned electrode intermediate product may include: a step of preparing basic particles; a step of mixing the above-mentioned basic particles and a coating source containing the first metal to form a coating containing the above-mentioned first metal on the surface of the above-mentioned basic particles; and a step of heat-treating the above-mentioned basic particles and the second metal formed with the above-mentioned coating to form a molten source formed by melting the above-mentioned basic particles and the above-mentioned second metal.

[0020] According to one embodiment, the elementary particles may include metal, metal oxide, metal carbide or carbon structure.

[0021] According to one embodiment, the elementary particles may include a carbon structure, and the method for preparing the electrode intermediate product may further include a step of pretreating the elementary particles with a metal nitric acid solution before mixing the elementary particles with the coating source.

[0022] According to one embodiment, the first metal and the second metal may include lithium.

[0023] According to one embodiment, the coating source may include a compound of lithium, nitrogen, fluorine, sulfur, carbon, and oxygen.

[0024] According to one embodiment, after the elementary particles and the coating source are mixed, heat treatment may be performed at a temperature higher than room temperature.

[0025] In order to solve the above technical problems, the present application provides a method for preparing an electrode.

[0026] According to one embodiment, the method for preparing the electrode may include: a step of preparing the molten source of the above embodiment; and a step of applying the molten source to prepare an electrode film.

[0027] In order to solve the above technical problems, the present application provides a method for preparing electrode particles.

[0028] According to an embodiment, the method for preparing the electrode particles may include: preparing the molten source of the embodiment; and cooling and dividing the molten source to prepare the electrode particles.

[0029] In order to solve the above technical problems, the present application provides a method for preparing a coating source.

[0030] According to one embodiment, the method for preparing the coating source may include: preparing a first precursor comprising sulfur and chlorine, a second precursor comprising sulfur and chlorine, and a third precursor comprising sulfur and nitrogen; reacting the first precursor, the second precursor, and the third precursor to prepare a first compound comprising sulfur, chlorine, oxygen, nitrogen, and hydrogen; reacting the first compound with a fourth precursor comprising fluorine to prepare a second compound; and reacting the second compound with a metal salt comprising a first metal to prepare a third compound.

[0031] According to one embodiment, before reacting the second compound and the metal salt, the method for preparing the coating source may further include a step of reacting the second compound with deionized water at a temperature lower than normal temperature, and the step of preparing the third compound may include a step of reacting the second compound reacted with deionized water with the metal salt.

[0032] According to one embodiment, the first metal may include lithium, potassium, sodium, zinc, iron, magnesium, silicon or aluminum.

[0033] In order to solve the above problems, the present application provides a method for preparing an electrode intermediate product.

[0034] According to one embodiment, the preparation method of the above-mentioned electrode intermediate product may include: a step of preparing the above-mentioned coating source of the above-mentioned embodiment; a step of mixing the elementary particles and the above-mentioned coating source to form a coating containing the above-mentioned first metal on the surface of the above-mentioned elementary particles; and a step of heat-treating the above-mentioned elementary particles and the second metal formed with the above-mentioned coating to form a molten source formed by melting the above-mentioned elementary particles and the above-mentioned second metal.

[0035] In order to solve the above technical problems, the present application provides an electrode film or electrode particles.

[0036] According to one embodiment, the electrode film or the electrode particle may be formed by solidifying a molten source in which a primary particle and a coating layer provided on a surface of the primary particle and including a first metal are melted together with a second metal.

[0037] According to one embodiment, the elementary particles may include at least one of silicon oxide, aluminum, aluminum oxide, copper, copper oxide, titanium, titanium oxide, titanium carbide, magnesium, tin, tin oxide, germanium, bismuth, molybdenum or a carbon structure.

[0038] In order to solve the above technical problems, the present application provides a negative electrode.

[0039] According to one embodiment, the negative electrode may include: a current collector; and a negative electrode active material provided on the current collector, and the negative electrode active material layer may include: a lithium compound including lithium and negative ions combined with the lithium; a conductive material having a higher electrical conductivity than the lithium compound; and a binder.

[0040] According to one embodiment, in the negative electrode active material layer, the ratio of the lithium compound, the conductive material and the binder may be 6:2:2 to 8:1:1 based on weight percentage.

[0041] According to one embodiment, the negative ions may include NO3 - , Cl - Br - 、FSI - 、F - or I - At least one of .

[0042] In order to solve the above technical problems, the present application provides a method for preparing electrode powder.

[0043] According to one embodiment, the method for preparing the electrode powder may include: preparing silicon oxide; mixing the silicon oxide and a first metal to react to prepare an intermediate compound; and providing a cleaning solution to the intermediate compound to prepare silicon and an electrode powder containing at least the silicon in the first metal from the intermediate compound. The proportion of the first metal in the electrode powder may be controlled according to the molar concentration of the cleaning solution.

[0044] According to one embodiment, the higher the molar concentration of the cleaning solution is, the smaller the ratio of the first metal in the electrode powder can be.

[0045] According to one embodiment, when the molar concentration of the cleaning solution is higher than the reference concentration, the electrode powder may not contain the first metal but contain the silicon. When the molar concentration of the cleaning solution is lower than the reference concentration, the electrode powder may contain an alloy powder of the silicon and the first metal.

[0046] According to one embodiment, the electrode powder may have a three-dimensional structure.

[0047] According to one embodiment, the step of preparing the above-mentioned silicon oxide may include: preparing biomass including grains or grain leaves; heat-treating the above-mentioned biomass; and providing an acidic solution to the heat-treated biomass to prepare the above-mentioned silicon oxide with a three-dimensional structure.

[0048] According to one embodiment, the silicon oxide and the first metal may be heat-treated in an inert gas atmosphere to form the intermediate compound.

[0049] In order to solve the above problems, the present application provides a negative electrode.

[0050] According to one embodiment, the negative electrode may include: electrode powder prepared by the preparation method of the above embodiment; a conductive material having a higher conductivity than the electrode powder; and a binder.

[0051] According to one embodiment, the negative electrode may include silicon prepared from grains or leaves of grains and having a three-dimensional structure.

[0052] According to one embodiment, the negative electrode may further include magnesium alloyed with the silicon to have a three-dimensional structure.

[0053] Effects of the Invention

[0054] The preparation method of the electrode intermediate product of the embodiment of the present application may include: a step of mixing basic particles and a coating source containing the first metal to form a coating containing the first metal on the surface of the above-mentioned basic particles; and a step of heat-treating the above-mentioned basic particles with the above-mentioned coating and the second metal to form a molten source formed by melting the above-mentioned basic particles with the above-mentioned coating and the second metal.

[0055] The molten source is an intermediate product for preparing an electrode, and an electrode film or electrode particles can be prepared from the molten source. Accordingly, the elements contained in the elementary particles, the first metal, and the second metal have a substantially uniform alloy composition in the molten source, the electrode film, and the electrode particles, thereby improving the charge and discharge characteristics, life, and stability of a secondary battery containing the electrode film.

[0056] Furthermore, according to an embodiment of the present application, a negative electrode active material layer can be formed by coating a coating source containing a powdered lithium compound on a current collector. Accordingly, the proportion of the lithium compound in the negative electrode containing the current collector and the negative electrode active material layer can be easily controlled, and the negative electrode can be prepared by a simple process. Therefore, a negative electrode and a preparation method thereof that saves preparation cost and is easy to mass produce can be provided.

[0057] Furthermore, according to an embodiment of the present application, after the three-dimensional silicon oxide and the first metal react to prepare an intermediate compound, a cleaning solution is provided to the intermediate compound to prepare a three-dimensional electrode powder. Furthermore, the three-dimensional silicon oxide can be prepared using biomass. Therefore, the preparation process of the electrode powder capable of preparing an electrode for a secondary battery can be simplified, saving preparation cost and preparation time. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 It is a flow chart for illustrating a method for preparing an electrode intermediate product and an electrode film or electrode particles using the same according to the first embodiment of the present application.

[0059] Figure 2 It is a flow chart for illustrating a method for preparing a coating source used in the preparation process of an electrode intermediate product according to the first embodiment of the present application.

[0060] Figure 3 It is a diagram for explaining the basic particles and coatings prepared according to the method for preparing an electrode intermediate product according to the first embodiment of the present application.

[0061] Figure 4 It is a flow chart for explaining a method for preparing a negative electrode using the electrode powder of the second embodiment of the present application.

[0062] Figure 5It is a flow chart for explaining a method for preparing a negative electrode using the electrode powder of the third embodiment of the present application.

[0063] Figure 6 A diagram for explaining a secondary battery according to an embodiment of the present application.

[0064] Figure 7 The scanning electron microscope (SEM) images of the electrode films of Experimental Examples 1-1 to 1-6 of the present application were taken.

[0065] Figure 8 The scanning electron microscope images of the electrode films of Experimental Examples 1-7 to 1-12 of the present application were taken.

[0066] Figures 9 to 20 The graphs are used to illustrate the charge and discharge characteristics of secondary batteries including the electrode films of Experimental Examples 1-1 to 1-12 of the present application.

[0067] Fig.21 It is a diagram for explaining the charge and discharge characteristics of the secondary battery including the electrode thin films of Experimental Examples 1-1 to 1-3, 1-6, and 1-9 of the present application.

[0068] Fig. 22 It is a diagram for explaining the charge and discharge characteristics of the secondary battery including the electrodes of Experimental Examples 1 to 13 of the present application.

[0069] Fig.23 It is a diagram for explaining the charge and discharge characteristics of the secondary battery including the electrode of Experimental Example 1-14 of the present application.

[0070] Fig.24 It is a diagram for comparing and explaining the charge and discharge characteristics of secondary batteries including the electrodes of Experimental Examples 1-13 and 1-14 of the present application.

[0071] Fig.25 The scanning electron microscope images of the electrode powders of Experimental Examples 1-15 to 1-18 of the present application are taken.

[0072] Figure 26 to Figure 29 The graphs are used to illustrate the charge and discharge characteristics of secondary batteries including the electrodes of Experimental Examples 1-15 to 1-18 of the present application.

[0073] Fig.30 It is a graph for comparing and explaining the charge and discharge characteristics of secondary batteries including the electrodes of Experimental Examples 1-15 to 1-19 of the present application.

[0074] Fig.31 It is a curve chart of the compound of Experimental Example 2-1 and the solid electrolyte of Experimental Example 8-3 of the present application detected by differential scanning calorimetry (DSC).

[0075] Fig.32 This is a curve chart of the compounds of Experimental Example 7-1 and Experimental Example 7-2 of the present application detected by differential scanning calorimetry.

[0076] Fig.33 It is a diagram for explaining the crystal structure of the solid electrolyte of Experimental Examples 8-1 to 8-3 of the present application.

[0077] Fig.34 It is a graph showing the ionic conductivity of the compound of Experimental Example 2-1 and the solid electrolytes of Experimental Examples 8-1 to 8-3 of the present application versus temperature.

[0078] Fig.35 This is a picture taken of an electrolyte membrane coated with the solid electrolyte of Experimental Example 8-1 of the present application. DETAILED DESCRIPTION

[0079] The preferred embodiments of the present application are described in detail below with reference to the accompanying drawings. However, the technical concept of the present application is not limited to the embodiments described below, and can also be embodied in other forms. The embodiments described here are provided only to make the disclosed content more thorough and complete and to fully convey the concept of the present application to those of ordinary skill in the technical field to which the present invention belongs.

[0080] In this specification, when a structural element is mentioned to be located on other structural elements, it means that it can be directly formed on other structural elements or a third structural element can be interposed therebetween. In addition, in the drawings, the thickness of the film and the region is exaggerated for the purpose of effectively explaining the technical content.

[0081] Furthermore, in various embodiments of this specification, although the terms such as first, second, and third are used to describe various structural elements, these structural elements are not limited by these terms. These terms are used only to distinguish a certain structural element from other structural elements. Therefore, the first structural element mentioned in a certain embodiment can also be recorded as the second structural element in other embodiments. The various embodiments described and illustrated herein also include embodiments complementary thereto. Furthermore, "and / or" in this specification is used to include at least one meaning of the structural elements listed before and after.

[0082] In the specification, unless clearly defined in the context, singular expressions include plural expressions. Furthermore, the terms "including" or "having" are used to refer to the existence of features, numbers, steps, structural elements or their combinations recorded in the specification, and should not be understood as excluding the existence or additional possibility of one or more other features, numbers, steps, structural elements or their combinations in advance.

[0083] Furthermore, in the following description of the present application, when the detailed description of related well-known functions or structures is judged to be likely to unnecessarily obscure the gist of the present invention, its detailed description will be omitted.

[0084] Hereinafter, an electrode intermediate product, an electrode using the intermediate product, an electrode particle using the intermediate product, and a method for preparing the intermediate product and the electrode particle according to a first embodiment of the present application will be described.

[0085] Figure 1 1 is a flow chart for illustrating a method for preparing an electrode intermediate product and an electrode film or electrode particles using the same according to the first embodiment of the present application. Figure 2 Flowchart for explaining the method for preparing a coating source used in the preparation process of the electrode intermediate product of the first embodiment of the present application. Figure 3 It is a diagram for explaining the basic particles and coatings prepared according to the method for preparing an electrode intermediate product according to the first embodiment of the present application.

[0086] Reference Figure 1 and Figure 3 , prepare elementary particles 100 (step S110).

[0087] The elementary particles 100 may include metals, metal oxides, metal carbides or carbon structures. For example, the elementary particles 100 may include at least one of silicon oxide, aluminum, aluminum oxide, copper, copper oxide, titanium, titanium oxide, titanium carbide, magnesium, tin, tin oxide, germanium, bismuth or molybdenum. For example, the carbon structure may be carbon fiber, carbon fabric, carbon fiber paper, graphene, carbon nanotubes (CNTs), etc.

[0088] According to an embodiment, the elementary particle 100 may be provided in a powder state. The elementary particle 100 may be purified in a vacuum state at 60°C.

[0089] In the case where the elementary particle 100 includes the carbon structure, the elementary particle 100 may be pretreated with a metal nitric acid solution. For example, the elementary particle 100 may be pretreated with a zinc nitric acid solution or a copper nitric acid solution. Accordingly, the carbon structure may be easily coated with the coating source described later, and a coating may be easily formed on the surface of the carbon structure. If the carbon structure is not pretreated with a metal nitric acid solution as in the embodiment of the present application, it is not easy to be coated with the coating source described later, and the coating may not be formed.

[0090] Next, refer to Figure 1 and Figure 3 , the elementary particle 100 and a coating source including a first metal are mixed to form a coating layer 110 including the first metal on the surface of the elementary particle 100 (step S120 ).

[0091] Specifically, after mixing the elementary particle 100 and the coating source, a heat treatment may be performed to form the coating 110 on the surface of the elementary particle 100. For example, the elementary particle 100 and the coating source may be heat treated at a temperature of 200° C. to 300° C. for 5 to 15 minutes.

[0092] The coating source may be a compound of lithium, nitrogen, fluorine, sulfur, carbon and oxygen. For example, the coating source may be as shown in the following chemical formula 1.

[0093] Chemical formula 1

[0094]

[0095] Reference Figure 2 The preparation method of the above-mentioned coating source is described.

[0096] The steps of preparing the coating source may include: step S115, preparing a first precursor comprising sulfur and chlorine, a second precursor comprising sulfur and chlorine, and a third precursor comprising sulfur and nitrogen; step S125, reacting the first precursor, the second precursor, and the third precursor to prepare a first compound; step S135, reacting the first compound with a fourth precursor comprising fluorine to prepare a second compound; and step S145, reacting the second compound with a metal salt comprising the first metal to prepare a third compound (the coating source).

[0097] For example, the first precursor may include thionyl chloride, the second precursor may include chlorosulfonic acid, and the third precursor may include sulfamic acid. The first compound may be prepared by mixing the first precursor, the second precursor, and the third precursor and then heat treating them in an inert gas atmosphere (e.g., 150° C.). The first compound may include sulfur, chlorine, oxygen, nitrogen, and hydrogen. Specifically, the first compound may be as shown in the following chemical formula 2.

[0098] Chemical formula 2

[0099]

[0100] The fourth precursor containing fluorine may contain bismuth trifluoride. The second compound may be prepared by distilling the first compound and the fourth precursor under reduced pressure while stirring. The second compound may be as shown in the following chemical formula 3.

[0101] Chemical formula 3

[0102]

[0103] For example, the first metal is lithium, and the metal salt containing the first metal may contain lithium carbonate. Alternatively, as another example, the first metal may contain potassium, sodium, zinc, iron, magnesium, silicon or aluminum, and the metal salt may contain a carbonate of the first metal.

[0104] Before reacting the second compound and the metal salt, the second compound and deionized water may be reacted at a temperature lower than room temperature (e.g., -70°C). The second compound is easily vaporized at room temperature and changes into a toxic gas, and the reaction of the second compound and the metal salt may be an exothermic reaction. Thus, as described above, the second compound and the metal salt may react in a liquid state at a temperature lower than room temperature, thereby improving the reaction safety and reaction efficiency of the second compound and the metal salt.

[0105] Then, after the metal salt is titrated until the pH of the second compound reacted with deionized water is neutral, the third compound (the coating source) can be prepared by filtering, washing and drying.

[0106] As described above, according to the embodiments of the present application, the first compound can be prepared by reacting the first precursor, the second precursor, and the third precursor, and then the second compound can be reacted with the metal salt to prepare the coating source. Thus, the coating source can be prepared with a low cost and a simple process with a high yield, and thus the cost of preparing the electrode intermediate product, electrode film, and electrode particles described later using the coating source can be reduced and the preparation process can be simplified.

[0107] Next, refer to Figure 1 and Figure 3 The elementary particles 100 and the second metal forming the coating layer 110 may be heat treated to prepare an electrode intermediate product including the elementary particles 100 and the molten source of the second metal that are melted to form the coating layer 110 (step S130).

[0108] The second metal may be provided in the form of a foil. That is, the molten source may be prepared by mixing the elementary particle 100 formed with the coating 110 in a powder state and the second metal in a foil state. For example, the elementary particle 100 formed with the coating 110 and the second metal may be melted by heat treatment at a temperature of 250° C. to 350° C. for 5 to 10 minutes.

[0109] According to one embodiment, after the primary particle 100 formed with the coating layer 110 is provided in a container and subjected to heat treatment, the second metal may be provided to the heat-treated container.

[0110] According to one embodiment, the first metal and the second metal included in the coating 110 may be metals of the same element. For example, the first metal and the second metal may be lithium. That is, the coating 110 including lithium may be formed on the surface of the elementary particle 100 by the coating source including lithium, thereby improving the lithium affinity of the elementary particle 100. Therefore, the elementary particle 100 with improved lithium affinity is easy to react with lithium as the second metal, thereby preparing the molten source for melting the elementary particle 100 and lithium.

[0111] If the coating layer 110 is not formed on the surface of the primary particle 100 , the primary particle 100 and the second metal are not easily reacted, and thus the molten source cannot have a uniform composition.

[0112] The electrode film can be prepared from the molten source. Specifically, the electrode film can be prepared by coating the molten source on a current collector. For example, the molten source can be coated by a doctor blade method.

[0113] Furthermore, electrode particles can be prepared from the molten source. Specifically, the electrode particles can be prepared by cooling the molten source and then dividing the cooled molten source. The electrode particles can be circulated, stored, and delivered in this state, and the electrode film can be prepared by melting the electrode particles in a secondary battery and / or secondary battery electrode manufacturing company.

[0114] According to an embodiment of the present application, the elementary particle 100 and the coating source containing the first metal may be mixed to form the coating 110 containing the first metal on the surface of the elementary particle 100, and the elementary particle 100 formed with the coating 110 and the second metal may be heat-treated to prepare the molten source of the elementary particle 100 and the second metal formed with the coating 110. The molten source is an intermediate product for preparing an electrode, and the electrode film or the electrode particles may be prepared from the molten source. Thus, the elements contained in the elementary particle 100, the first metal and the second metal may substantially have a uniform alloy composition in the molten source, the electrode film and the electrode particles, thereby improving the charge and discharge characteristics, life and stability of the secondary battery containing the electrode film.

[0115] In reference Figures 1 to 3In the described embodiments of the present application, the third compound (the coating source) is used to coat the elementary particles 100 , but the use of the third compound is not limited thereto, and the third compound may also be used as an additive for electrolytes for secondary batteries or supercapacitors.

[0116] Specifically, the third compound may be used as a metal salt added to an electrolyte containing dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), or ethyl propyl carbonate (EPC).

[0117] Hereinafter, an electrode powder, an electrode using the same, and a method for preparing the same according to a second embodiment of the present application will be described.

[0118] Figure 4 It is a flow chart for explaining a method for preparing a negative electrode using the electrode powder of the second embodiment of the present application.

[0119] Reference Figure 4 , prepare a lithium compound (step S210).

[0120] The lithium compound may include lithium and negative ions combined with the lithium. For example, the negative ions may include NO3 - , Cl - Br - 、FSI - 、F - or I - Specifically, for example, the lithium compound may include at least one of LiNO3, LiCl, LiBr, LiFSI, LiF or LiI.

[0121] According to one embodiment, the lithium compound may be prepared in a powder state.

[0122] A source material may be prepared by mixing the lithium compound, a conductive material, a binder, and a solvent (step S220 ).

[0123] The conductive material may have a higher conductivity than the lithium compound. For example, the conductive material may include carbon black. Alternatively, as another example, the conductive material may include at least one of Super P, acetylene black, SUPER C65, graphene, or carbon nanotubes.

[0124] The above-mentioned binder can make the above-mentioned conductive material and the above-mentioned lithium compound adhere to the collector described later. For example, the above-mentioned binder can include polyvinylidene fluoride (PVDF, poly (vinylidene fluoride)). As another example, the above-mentioned binder can include at least one of carboxymethyl cellulose (Carboxymethyl Cellulose, CMC), styrene-Butadiene Rubber (Styrene-Butadiene Rubber, SBR), polytetrafluoroethylene (Polytetrafluoroethylene, PTFE), polyoxyethylene powder (Poly (ethylene oxide) Powder) or silver paste (Silver Paste).

[0125] The lithium compound, the conductive material and the binder may be dispersed and / or dissolved in the solvent. For example, the solvent may include N-methylpyrrolidone (NMP). As another example, the solvent may include at least one of N,N-dimethylformamide (DMF), toluene, dimethyl sulfoxide (DMSO), hexane or tetrahydrofuran (THF).

[0126] The source material may be coated on a current collector to prepare a negative electrode (step S230).

[0127] The negative electrode active material layer can be formed on the current collector by coating the source material on the current collector, thereby preparing the negative electrode comprising the current collector and the negative electrode active material. For example, the current collector can be a metal foil, and the negative electrode active material layer can be formed by heat treating the current collector at a temperature of 60° C. after coating the coating source on the current collector.

[0128] As described above, the negative electrode active material layer can be formed by mixing the powdered lithium compound and the powdered conductive material with the binder. Therefore, when observing the inside and cross section of the negative electrode active material layer, the powdered lithium compound can be observed.

[0129] The lithium compound may function as a negative electrode active material that absorbs and releases lithium during the charge and discharge process of a secondary battery including the negative electrode.

[0130] According to one embodiment, in the solvent, the ratio of the lithium compound, the conductive material and the binder can be 6:2:2 to 8:1:1 based on weight percentage. Thus, in the negative electrode active material layer, the ratio of the lithium compound, the conductive material and the binder can be 6:2:2 to 8:1:1 based on weight percentage. If the ratio of the lithium compound is lower than 60 weight percentage and the ratio of the conductive material and the binder is higher than 20 weight percentage, respectively, the charge and discharge characteristics of the secondary battery including the negative electrode may be reduced. In addition, if the ratio of the lithium compound is higher than 80 weight percentage and the ratio of the conductive material and the binder is lower than 10 weight percentage, respectively, the life characteristics may be reduced due to the volume expansion of the negative electrode active material layer of the negative electrode during the charge and discharge process of the secondary battery including the negative electrode.

[0131] However, as described above, according to the embodiments of the present application, based on weight percentage, the ratio of the lithium compound, the conductive material and the binder can be 6:2:2 to 8:1:1, thereby improving the charge and discharge characteristics and life characteristics of the secondary battery including the negative electrode.

[0132] According to an embodiment of the present application, the above-mentioned lithium compound in powder state and the above-mentioned conductive material in powder state can be used to form the above-mentioned negative electrode active material layer on the above-mentioned current collector. The proportion of the above-mentioned lithium compound in the above-mentioned negative electrode including the above-mentioned current collector and the above-mentioned negative electrode active material layer can be easily controlled, so that the above-mentioned negative electrode can be prepared in a simple process. Therefore, a negative electrode and a preparation method thereof that saves preparation costs and is easy to mass produce can be provided.

[0133] Hereinafter, an electrode powder, an electrode using the same, and a method for preparing the same according to a third embodiment of the present application will be described.

[0134] Figure 5 It is a flow chart for explaining a method for preparing a negative electrode using the electrode powder of the third embodiment of the present application.

[0135] Reference Figure 5 , prepare silicon oxide (step S310).

[0136] According to one embodiment, the silicon oxide may have a porous three-dimensional structure, and the silicon oxide may be prepared using biomass. Specifically, for example, the step of preparing the silicon oxide may include: preparing biomass including grains or grain leaves; heat treating the biomass; and providing an acidic solution to the heat treated biomass to prepare the silicon oxide having a three-dimensional structure.

[0137] For example, the biomass may be rice or rice leaves, the biomass may be heat-treated at a temperature of 300° C., and the acidic solution may be hydrochloric acid.

[0138] The silicon oxide and the first metal are mixed and reacted to prepare an intermediate compound (step S320 ).

[0139] The first metal may be provided in a powder state and may be mixed with the silicon oxide in a powder state. For example, the first metal may include magnesium.

[0140] The mixture of the silicon oxide and the first metal may be heat-treated in an inert gas atmosphere. For example, the mixture may be heat-treated in a nitrogen atmosphere at 600° C. for 3 hours. Thus, the intermediate compound may be prepared by reacting the silicon oxide and the first metal with each other.

[0141] A cleaning solution may be provided to the intermediate compound to prepare silicon and an electrode powder including at least the silicon in the first metal from the intermediate compound (step S330 ).

[0142] According to one embodiment, in the step of preparing the electrode powder, the proportion of the first metal in the electrode powder may be controlled according to the molar concentration of the cleaning solution. For example, the cleaning solution may contain hydrochloric acid.

[0143] Specifically, the higher the molar concentration of the cleaning solution, the higher the ratio of the first metal removed from the intermediate compound, thereby reducing the ratio of the first metal in the electrode powder. Conversely, the lower the molar concentration of the cleaning solution, the lower the ratio of the first metal removed from the intermediate compound, thereby increasing the ratio of the first metal in the electrode powder.

[0144] That is, when the molar concentration of the cleaning solution is higher than the reference concentration, the first metal can be substantially completely removed from the intermediate compound, and accordingly, the electrode powder can be substantially free of the first metal and formed of the silicon. Alternatively, when the molar concentration of the cleaning solution is lower than the reference concentration, the first metal can remain in the intermediate compound, and accordingly, the electrode powder can be formed of an alloy of the silicon and the first metal. The reference concentration can be adjusted according to the amount of the first metal and the time for providing the cleaning solution. Specifically, the greater the amount of the first metal and / or the longer the time for providing the cleaning solution, the higher the reference concentration can be.

[0145] As described above, the silicon oxide may have a three-dimensional structure. Accordingly, the electrode powder prepared using the silicon oxide may also have silicon with a three-dimensional structure. Furthermore, the silicon of the electrode powder may be activated by the cleaning solution. In other words, silicon with a three-dimensional structure may be formed by removing the first metal. Accordingly, the charge and discharge characteristics of a secondary battery including an electrode prepared using the electrode powder may be improved.

[0146] The electrode powder can be compared with the reference Figure 1 The conductive material, the binder, and the solvent described above are mixed together and then applied to a current collector to form an electrode for a secondary battery.

[0147] According to an embodiment of the present application, the electrode powder having a three-dimensional structure may be prepared by a simple process of reacting the silicon oxide having a three-dimensional structure with the first metal to prepare the intermediate compound and then providing the cleaning solution to the intermediate compound.

[0148] Furthermore, the above silicon oxide having a three-dimensional structure can be prepared using biomass.

[0149] Therefore, the production process of the electrode powder capable of producing an electrode for a secondary battery can be simplified, production costs can be reduced, and mass production can be facilitated.

[0150] By reference Figures 1 to 5 The electrode film and the negative electrode prepared by the method described above can be used as electrodes of a secondary battery together with a solid electrolyte. Figure 6 The secondary battery according to the embodiment of the present application is described.

[0151] Figure 6 A diagram for explaining a secondary battery according to an embodiment of the present application.

[0152] Reference Figure 6 The secondary battery of the embodiment of the present application may include a negative electrode 210 , a solid electrolyte 220 and a positive electrode 230 .

[0153] The negative electrode 210 may include a reference Figures 1 to 3 Alternatively, the negative electrode may include the electrode film prepared from the molten source or the electrode film prepared from the electrode particles. Figure 4 and Figure 5 The electrode prepared from the electrode powder is described.

[0154] For example, the positive electrode 230 may include lithium oxide, and the lithium oxide may include at least one of nickel, cobalt, manganese, or aluminum. Alternatively, as another example, the positive electrode 230 may include oxides of lithium, phosphorus, and iron.

[0155] The solid electrolyte 220 may be a compound of positive ions and negative ions.

[0156] Specifically, the positive ion may include at least one of thiophenium represented by Chemical Formula 4, thiazolium represented by Chemical Formula 5, phospholane represented by Chemical Formula 6, oxathiolanium represented by Chemical Formula 7 or Chemical Formula 8, and thiazolidinium represented by Chemical Formula 9. R1 in Chemical Formulas 4 to 9 may be an alkyl group.

[0157] Chemical formula 4

[0158]

[0159] Chemical formula 5

[0160]

[0161] Chemical formula 6

[0162]

[0163] Chemical formula 7

[0164]

[0165] Chemical formula 8

[0166]

[0167] Chemical formula 9

[0168]

[0169] Specifically, the negative ions may include hydrofluoric acid salt (Fluorohydrogenate) represented by Chemical Formula 10. Specifically, the negative ions may include hydrofluoric acid salt (Fluorohydrogenate) represented by Chemical Formula 10.

[0170] Chemical formula 10

[0171]

[0172] Alternatively, the negative ion may include cyano(nitroso)methanide or tetrazolidine.

[0173] According to other embodiments, different from the above, the solid electrolyte 220 may be an oxide, a sulfide or a polymer.

[0174] The following describes an electrode film prepared according to a specific experimental example based on the first embodiment of the present application and the results of evaluating its characteristics.

[0175] Preparation of coating source for experimental example

[0176] Sulfoxyl chloride is prepared as a first precursor, chlorosulfonic acid is prepared as a second precursor, and sulfamic acid is prepared as a third precursor. Sulfoxyl chloride, chlorosulfonic acid, and sulfamic acid are mixed and then heat-treated at 150° C. for 12 hours.

[0177] The generated gas was removed using a caustic solution, and the remaining solvent was removed by distillation to prepare a caustic as the first compound. Bismuth trifluoride was prepared as the fourth precursor, and after stirring and reacting with bis(chlorosulfonyl)imide in a glove box for 8 hours, bis(fluorosulfonyl)imide was prepared by distillation under reduced pressure as the second compound.

[0178] Then, the second compound was reacted with deionized water at -70°C and heated to room temperature, and then lithium carbonate was slowly added to neutralize the pH. Then, the coating source of the experimental example represented by the above chemical formula 1 was prepared by filtering, washing with ethyl acetate, and drying.

[0179] Preparation of the electrode film of Experimental Example 1-1

[0180] Silicon oxide was prepared as the elementary particles. Silicon oxide (SiO2) was pre-treated in a vacuum state at 60°C.

[0181] The coating source prepared according to the above-mentioned experimental example was prepared, and silicon oxide and the coating source were mixed and then heat-treated at 250° C. for 10 minutes to form a coating on the surface of the silicon oxide.

[0182] Then, the silicon oxide having the coating formed thereon was placed in a stainless steel container and heat-treated at 300° C., and then lithium was added for reaction to prepare a molten source.

[0183] The electrode thin film of Experimental Example 1-1 including the Li—SiO 2 alloy was prepared by applying a molten source onto a substrate using a doctor blade method.

[0184] Preparation of the electrode film of Experimental Example 1-2

[0185] The electrode thin film of Experimental Example 1-2 including a Li-TiO 2 alloy was prepared by the same method as that of Experimental Example 1-1, using titanium oxide (TiO 2 ) as a basic particle.

[0186] Preparation of electrode films of Experimental Examples 1-3

[0187] The electrode thin film of Experimental Example 1-3 including a Li—Mg—Si alloy was prepared by the same method as that of Experimental Example 1-1, except that titanium oxide (Mg—Si) was used as a primary particle.

[0188] Preparation of electrode films of Experimental Examples 1-4

[0189] The electrode thin film of Experimental Example 1-4 including the Li—Bi alloy was prepared by the same method as that of Experimental Example 1-1, using bismuth (Bi) as a basic particle.

[0190] Preparation of electrode films of Experimental Examples 1-5

[0191] The electrode thin film of Experimental Example 1-5 including the Li—Ge alloy was prepared by the same method as Experimental Example 1-1, using germanium (Ge) as a basic particle.

[0192] Preparation of electrode films of Experimental Examples 1-6

[0193] The electrode thin film of Experimental Example 1-6 including the Li-Ti3C2 alloy was prepared by the same method as Experimental Example 1-1, using titanium carbide (Ti3C2) as the primary particle.

[0194] Preparation of electrode films of Experimental Examples 1-7

[0195] The electrode film of Experimental Example 1-7 including a Li—Sn—SnO 2 alloy was prepared by the same method as Experimental Example 1-1, using tin and tin oxide (Sn and SnO 2 ) as basic particles.

[0196] Preparation of electrode films of Experimental Examples 1-8

[0197] The electrode thin film of Experimental Example 1-8 including a Li—Mo alloy was prepared by the same method as that of Experimental Example 1-1, using molybdenum (Mo) as a primary particle.

[0198] Preparation of electrode films of Experimental Examples 1-9

[0199] The electrode thin film of Experimental Example 1-9 including the Li—CuO alloy was prepared by the same method as that of Experimental Example 1-1, using copper oxide (CuO) as a basic particle.

[0200] Preparation of electrode films of Experimental Examples 1-10

[0201] The electrode thin film of Experimental Example 1-10 including the Li—Mg alloy was prepared by the same method as that of Experimental Example 1-1, using magnesium (Mg) as a primary particle.

[0202] Preparation of electrode films of Experimental Examples 1-11

[0203] The electrode film of Experimental Example 1-11 including a Li—Al—Al 2 O 3 alloy was prepared by the same method as Experimental Example 1-1, using aluminum and aluminum oxide (Al and Al 2 O 3 ) as basic particles.

[0204] Preparation of electrode films of Experimental Examples 1-12

[0205] The electrode thin film of Experimental Example 1-12 including the Li-graphene alloy was prepared by using graphene as a basic particle in the same manner as Experimental Example 1-1.

[0206] The structures of the electrode thin films of Experimental Examples 1-1 to 1-12 are summarized in Table 1 below.

[0207] Table 1

[0208] distinguish Electrode film composition Experimental Example 1-1 <![CDATA[Li-SiO2]]> Experimental Example 1-2 <![CDATA[Li-TiO2]]> Experimental Examples 1-3 Li-Mg-Si Experimental Examples 1-4 Li-Bi Experimental Examples 1-5 Li-Ge Experimental Examples 1-6 <![CDATA[Li-Ti3C2]]> Experimental Examples 1-7 <![CDATA[Li-Sn-SnO2]]> Experimental Examples 1-8 Li-Mo Experimental Example 1-9 Li-CuO Experimental Example 1-10 Li-Mg Experimental Example 1-11 <![CDATA[Li-Al-Al2O3]]> Experimental Example 1-12 Li-graphene

[0209] Figure 7 To take scanning electron microscope (SEM) images of the electrode films of Experimental Examples 1-1 to 1-6 of the present application, Figure 8 The scanning electron microscope images of the electrode films of Experimental Examples 1-7 to 1-12 of the present application were taken.

[0210] Reference Figure 7 and Figure 8 , Figure 7 Parts (a) to (f) of FIG. 1 are images of the electrode films of Experimental Examples 1-1 to 1-6 of the present application, respectively. Figure 8 Parts (a) to (f) are pictures of the electrode films of Experimental Examples 1-7 to 1-12 of the present application, respectively.

[0211] Reference Figure 7 and Figure 8 It can be confirmed that the elements contained in the elementary particles and lithium stably form a three-dimensional structure in an alloy state. In addition, it can be known that the structure of the electrode film finally prepared can be controlled according to the type of elements contained in the elementary particles. Specifically, it can be confirmed that the electrode film containing the Li-Ge alloy of Experimental Example 1-5 and the electrode film containing the Li-Mg alloy of Experimental Example 1-10 have a bed-shaped three-dimensional structure extending in one direction.

[0212] Figures 9 to 20 The graphs are used to illustrate the charge and discharge characteristics of secondary batteries including the electrode films of Experimental Examples 1-1 to 1-12 of the present application.

[0213] Reference Figures 9 to 20 The electrode films of Experimental Examples 1-1 to 1-12 were placed on both sides to prepare a battery. -2 The current density and 2mAhcm-2 The charge and discharge characteristics are evaluated and the coulombic efficiency is measured.

[0214] pass Figures 9 to 20 It was confirmed that the battery including the electrode thin films of Experimental Examples 1-1 to 1-12 can be driven stably for a long time. In particular, it was confirmed that the battery including the electrode thin film including the Li-SiO2 alloy of Experimental Example 1-1, the electrode thin film including the Li-TiO2 alloy of Experimental Example 1-2, the electrode thin film including the Li-Mg-Si alloy of Experimental Example 1-3, the electrode thin film including the Li-Ti3C2 alloy of Experimental Example 1-6, and the electrode thin film including the Li-CuO alloy of Experimental Example 1-9 can be driven stably for a long time.

[0215] Fig.21 It is a diagram for comparing and explaining the charge and discharge characteristics of secondary batteries including the electrode films of Experimental Examples 1-1 to 1-3, 1-6, and 1-9 of the present application.

[0216] Reference Fig.21 Batteries were prepared using the electrode films and tetrahydrofuran (ThF) electrolyte of Experimental Examples 1-1 to 1-3, 1-6 and 1-9, respectively, and were charged and discharged 120 times under 1C conditions.

[0217] pass Fig.21 It was confirmed that the secondary batteries including the electrode films of Experimental Examples 1-1 to 1-3, 1-6, and 1-9 had a capacity of 2700 mAhg -1 The high capacity above 98% is still retained after 120 charge and discharge cycles.

[0218] The results confirm that the secondary battery including the lithium alloy electrode film prepared according to the embodiment of the present application has high charge and discharge capacity and long life.

[0219] Hereinafter, electrodes using electrode powders prepared according to specific experimental examples based on the second embodiment and the third embodiment of the present application and evaluation of their characteristics will be described.

[0220] Electrode powder and electrode of Experimental Examples 1-13

[0221] LiNO3 was prepared as a lithium compound, carbon black was prepared as a conductive material, polyvinylidene fluoride (PVDF) was prepared as a binder, N-methylpyrrolidone (NMP) was prepared as a solvent, and copper foil was prepared as a current collector.

[0222] The source material was prepared by mixing LiNO 3 , carbon black and polyvinylidene fluoride in a ratio of 6:2:2 in N-methylpyrrolidone based on weight percentage.

[0223] The source material was coated on a copper foil and then dried at 60° C. to prepare the LiNO 3 powder negative electrode of Experimental Example 1-13.

[0224] Preparation of electrode powder and electrode of Experimental Examples 1-14

[0225] The LiCl powder negative electrode of Experimental Example 1-14 was prepared in the same manner as that of Experimental Example 1-13, using LiCl as the lithium compound.

[0226] Fig. 22 Graphs for illustrating the charge and discharge characteristics of the secondary battery including the electrodes of Experimental Examples 1 to 13 of the present application, Fig.23 It is a diagram for explaining the charge and discharge characteristics of the secondary battery including the electrode of Experimental Example 1-14 of the present application.

[0227] Reference Fig. 22 and Fig.23 The electrodes of Experimental Examples 1-13 and 1-14 were placed on both sides to prepare a battery. -2 The current density and 2mAhcm -2 The charge and discharge characteristics are evaluated and the coulombic efficiency is measured.

[0228] pass Fig. 22 and Fig.23 It can be seen that the battery including the electrodes of Experimental Examples 1-13 and 1-14 can be driven stably for a long time. In other words, it can be seen that the negative electrode can be prepared in the air using a powdered lithium compound by a simple method, and in this case, it can be driven stably.

[0229] Fig.24 It is a diagram for comparing and explaining the charge and discharge characteristics of secondary batteries including the electrodes of Experimental Examples 1-13 and 1-14 of the present application.

[0230] Reference Fig.24 A battery was prepared using the electrodes of Experimental Examples 1-13 and 1-14 and tetrahydrofuran electrolyte, and was charged and discharged 100 times at 1C.

[0231] pass Fig.24 It can be seen that the secondary battery containing the LNO3 powder of Experimental Example 1-13 and the secondary battery containing the LiCl powder of Experimental Example 1-14 have a capacity of 2500 mAhg -1 Furthermore, it can be seen that the capacity and life characteristics of the secondary battery containing the LNO3 powder of Experimental Example 1-12 are superior to the capacity and life characteristics of the secondary battery containing the LiCl powder of Experimental Example 1-14.

[0232] Preparation of electrode powder and electrode of Experimental Examples 1-15

[0233] Rice and rice leaves were prepared as biomass, and hydrochloric acid was prepared as an acidic solution.

[0234] Rice and rice leaves were heat treated at 300°C in an oxygen atmosphere for 1 hour and treated with hydrochloric acid to prepare a porous silicon oxide with a three-dimensional structure. The porous silicon oxide with a three-dimensional structure was mixed with magnesium powder and then heat treated at 600°C in a nitrogen atmosphere for 3 hours. Then, high-concentration hydrochloric acid (37 weight percent, 12M) was provided as a cleaning solution for 10 minutes, and after removing the magnesium phase, ethanol was used for cleaning, and the silicon electrode powder of Experimental Examples 1-15 with activated three-dimensional silicon was prepared by drying in a vacuum atmosphere.

[0235] Carbon black was prepared as a conductive material, and lithium polyacrylate was prepared as a binder.

[0236] Then, the electrode powder of Experimental Example 1-15, a conductive material, and a binder were mixed in a ratio of 6:2:2 and applied onto a current collector to prepare the electrode of Experimental Example 1-15.

[0237] Preparation of electrode powder and electrode of Experimental Examples 1-16

[0238] The silicon-magnesium alloy electrode powder of Experimental Example 1-16 was prepared in the same manner as in Experimental Example 1-15, except that high-concentration hydrochloric acid (1 M) was provided as a cleaning solution for 1 hour to allow magnesium to remain.

[0239] Then, other electrode powders, a conductive material, and a binder were mixed with Experimental Example 1-16 at a ratio of 8:1:1 and then applied onto a current collector to prepare an electrode of Experimental Example 1-16.

[0240] Preparation of electrode powder and electrode of Experimental Examples 1-17

[0241] Ti3AlC2 was prepared as a metal precursor, and LiF was prepared as a solvent.

[0242] LiF and Ti3AlC2 were slowly added to 6M hydrochloric acid at 40°C to react for 30 minutes. Then, ultrasonic treatment was performed to prepare Ti3C2 nanosheet electrode powder of Experimental Example 1-17.

[0243] Then, other electrode powders, a conductive material, and a binder were mixed with Experimental Example 1-17 at a ratio of 7:1:2 and then applied onto a current collector to prepare an electrode of Experimental Example 1-17.

[0244] Preparation of electrode powder and electrode of Experimental Examples 1-18

[0245] Prepare Bi(NO3)3 as a metal precursor, prepare PEG6000 as a polymer, and prepare nitric acid as a solvent.

[0246] 0.02M Bi(NO3)3, 0.03g PEG6000 and 0.25M nitric acid were mixed for 30 minutes and then placed at 80°C for 1 hour. Then, the reactant was filtered, washed with deionized water, and dried under vacuum to prepare the Bi nanosheet electrode powder of Experimental Example 1-18.

[0247] Then, other electrode powders, a conductive material, and a binder were mixed with Experimental Example 1-18 at a ratio of 8:1:1 and then applied onto a current collector to prepare an electrode of Experimental Example 1-18.

[0248] Preparation of electrodes of Experimental Examples 1-19

[0249] Aluminum powder was purchased and the electrode of Experimental Example 1-19 was prepared in the same manner as in Experimental Example 1-15.

[0250] The electrode powders of Experimental Examples 1-15 to 1-19 can be organized as shown in Table 2 below.

[0251] Table 2

[0252] distinguish Electrode powder Experimental Example 1-15 Si Experimental Example 1-16 Mg-Si Experimental Example 1-17 <![CDATA[Ti2C3]]> Experimental Example 1-18 Bi Experimental Example 1-19 Al(Purchased commercial products)

[0253] Fig.25 The scanning electron microscope images of the electrode powders of Experimental Examples 1-15 to 1-18 of the present application are taken.

[0254] Reference Fig.25 , scanning electron microscope images were taken of the electrode powders of Experimental Examples 1-15 to 1-18.

[0255] pass Fig.25 It can be seen that the electrode powders of Experimental Examples 1-15 to 1-18 have a three-dimensional porous structure. Compared with the Si electrode powder of Experimental Example 1-15, it can be confirmed that the network of the Mg-Si electrode powder of Experimental Example 1-16 is somewhat thick. In addition, it can be confirmed that the Ti2C3 electrode powder of Experimental Example 1-17 and the Bi electrode powder of Experimental Example 1-18 form a plate shape.

[0256] Figure 26 to Figure 29 These are graphs for explaining the charge and discharge characteristics of secondary batteries including the electrodes of Experimental Examples 1-15 to 1-18 of the present application.

[0257] Reference Figure 26 to Figure 29 , the electrodes of Experimental Examples 1-15 to 1-18 were arranged on both sides to prepare a battery, and at 1 mA cm -2 The current density and 2mAhcm -2The charge and discharge characteristics were evaluated under the conditions of capacity and coulombic efficiency was measured.

[0258] exist Figure 26 to Figure 29 It was confirmed that the battery including the electrodes of Experimental Examples 1-15 to 1-18 could be driven stably for a long time. In particular, it was confirmed that the battery including the Si electrode powder of Experimental Example 1-15 and the Mg-Si electrode powder of Experimental Example 1-16 could be driven stably for a long time.

[0259] Fig.30 It is a graph for comparing and explaining the charge and discharge characteristics of secondary batteries including the electrodes of Experimental Examples 1-15 to 1-19 of the present application.

[0260] Reference Fig.30 , batteries were prepared using the electrodes of Experimental Examples 1-15 to 1-19 and tetrahydrofuran electrolyte, and were charged and discharged 100 times under 1C conditions.

[0261] exist Fig.30 It can be confirmed that the secondary batteries containing the electrode powders of Experimental Examples 1-15 to 1-19 can be stably driven. In particular, it can be confirmed that the Si electrode powder of Experimental Example 1-15 and the Mg-Si electrode powder of Experimental Example 1-16 have 3404 mAhg -1 and 3550mAhg -1 The capacity of the battery is 93% and 97% respectively after 100 charge and discharge cycles.

[0262] Hereinafter, a solid electrolyte including a compound bonded by positive ions and negative ions and the results of evaluating its characteristics will be described based on specific experimental examples of the present application.

[0263] Preparation of the compound of Experimental Example 2-1

[0264] Acetonitrile was supplied to a conical flask, dichloromethane was added, and then stirred at room temperature for 10 minutes to prepare a solution containing an alkyl group. In this case, the solution containing an alkyl group was prepared in a glove box without moisture.

[0265] After adding thiophene to the solution containing the alkyl group while stirring, the uniformly mixed solution was slowly stirred at room temperature for 4 days to prepare a thiophene salt having a methyl group as a positive ion source.

[0266] The washing step is performed by supplying the thiophene salt and a solvent of ethyl acetate and diethyl ether into a rotary concentrator.

[0267] 1 M hydrofluoric acid and the balance of water were added to a conical flask, followed by stirring for 10 minutes to prepare a hydrofluoric acid salt precursor as a negative ion source.

[0268] A thiophene salt is added to a hydrofluoric acid salt precursor to prepare a mixed solution, and the mixed solution is placed at a temperature of -70°C for 24 hours to prepare a compound combining a thiophene salt and a hydrofluoric acid salt.

[0269] After providing the above compound in a glove box with a nitrogen atmosphere, the compound was placed at room temperature for 2 to 3 hours to remove volatile gas. Then, the compound was provided in a rotary concentrator for a drying step to prepare the compound of Experimental Example 2-1 in which a thiophene cation having a methyl group (R1) and a hydrofluoric acid anion were bonded.

[0270] Preparation of the compound of Experimental Example 2-2

[0271] The same method as in Experimental Example 2-1 was used to prepare ethyl chloride instead of dichloromethane. In addition, in the preparation step of thiophene, the reaction was carried out at a temperature of 60° C. to 80° C. for 2 to 3 days instead of at room temperature for 4 days, thereby preparing the compound of Experimental Example 2-2 in which a thiophene cation having an ethyl group (R1) and a hydrofluoric acid anion were combined.

[0272] Preparation of the compound of Experimental Example 2-3

[0273] The same method as in Experimental Example 2-1 was used to prepare the compound of Experimental Example 2-3 in which a thiophene cation having a propyl group (R1) and a hydrofluoric acid anion were combined, except that propyl chloride was used to replace dichloromethane. In addition, in the preparation step of thiophene, the reaction was carried out at a temperature of 60°C to 80°C for 2 to 3 days instead of at room temperature for 4 days, thereby preparing the compound of Experimental Example 2-3 in which a thiophene cation having a propyl group (R1) and a hydrofluoric acid anion were combined.

[0274] Preparation of the compound of Experimental Example 2-4

[0275] The same method as in Experimental Example 2-1 was used to prepare butyl chloride instead of dichloromethane. In addition, in the preparation step of thiophene, the reaction was carried out at a temperature of 60° C. to 80° C. for 2 to 3 days instead of at room temperature for 4 days, thereby preparing the compound of Experimental Example 2-4 in which a thiophene cation having a butyl group (R1) and a hydrofluoric acid anion were combined.

[0276] Preparation of the compound of Experimental Example 3-1

[0277] The thiazoline was added to the solution containing the alkyl group to prepare the thiazolium salt as the positive ion source in the same manner as in the above Experimental Example 2-1.

[0278] Then, the thiazole salt was reacted with the hydrofluoric acid salt precursor in the same manner as in Experimental Example 2-1 to prepare the compound of Experimental Example 3-1 in which a thiazole cation having a methyl group (R1) and a hydrofluoric acid salt anion were bonded.

[0279] Preparation of the compound of Experimental Example 3-2

[0280] The thiazoline was added to the solution containing the alkyl group in the same manner as in Experimental Example 2-2 to prepare a thiazolium salt as a positive ion source.

[0281] Then, the thiazolium salt was reacted with the hydrofluoric acid salt precursor in the same manner as in Experimental Example 2-2, thereby preparing the compound of Experimental Example 3-2 in which a thiazolium cation having an ethyl group (R1) and a hydrofluoric acid salt anion were bonded.

[0282] Preparation of the compound of Experimental Example 3-3

[0283] The thiazoline was added to the solution containing the alkyl group to prepare the thiazolium salt as the positive ion source in the same manner as in the above Experimental Example 2-3.

[0284] Then, the thiazole salt was reacted with the hydrofluoric acid salt precursor in the same manner as in Experimental Example 2-3, thereby preparing the compound of Experimental Example 3-3 in which the thiazole cation having a propyl group (R1) and the hydrofluoric acid salt anion were bonded.

[0285] Preparation of the compound of Experimental Example 3-4

[0286] The thiazoline was added to the solution containing the alkyl group to prepare the thiazolium salt as the positive ion source in the same manner as in the above Experimental Example 2-4.

[0287] Then, the thiazole salt was reacted with the hydrofluoric acid salt precursor in the same manner as in Experimental Example 2-4, thereby preparing the compound of Experimental Example 3-4 in which the thiazole cation having a butyl group (R1) and the hydrofluoric acid salt anion were bonded.

[0288] Preparation of the compound of Experimental Example 4-1

[0289] Phospholane was prepared as a positive ion, and the hydrofluoride prepared according to the above Experimental Example 2-1 was used as a negative ion to prepare the compound of Experimental Example 4-1 in which the phospholane positive ion having a methyl group (R1) and an ethyl group (R2) was combined with the hydrofluoride negative ion.

[0290] Preparation of the compound of Experimental Example 4-2

[0291] The compound of Experimental Example 4-2 in which a phospholane cation having a methyl group (R1) and a propyl group (R2) and a hydrofluoric acid salt anion were bonded was prepared in the same manner as in Experimental Example 4-1.

[0292] Preparation of the compound of Experimental Example 4-3

[0293] The compound of Experimental Example 4-3 in which a phospholane cation having a methyl group (R1) and a butyl group (R2) and a hydrofluoric acid salt anion were bonded was prepared in the same manner as in Experimental Example 4-1.

[0294] Preparation of the compound of Experimental Example 4-4

[0295] The compound of Experimental Example 4-4 in which a phospholane cation having an ethyl group (R1) and a butyl group (R2) and a hydrofluoric acid salt anion were bonded was prepared in the same manner as in Experimental Example 4-1.

[0296] Preparation of the compound of Experimental Example 4-5

[0297] The compound of Experimental Example 4-5 in which a phospholane cation having a methyl group (R1) and a methyl group (R2) and a hydrofluoric acid salt anion were bonded was prepared in the same manner as in Experimental Example 4-1.

[0298] Preparation of the compound of Experimental Example 5-1

[0299] Oxathiolane represented by Chemical Formula 8 was prepared as a positive ion, and the hydrofluoride prepared according to the above Experimental Example 2-1 was used as a negative ion to prepare the compound of Experimental Example 5-1 in which the oxathiolane positive ion having a methyl group (R1) was combined with the hydrofluoride negative ion.

[0300] Preparation of the compound of Experimental Example 5-2

[0301] The compound of Experimental Example 5-2 in which an oxathiolane cation having an ethyl group (R1) and a hydrofluoric acid salt anion were bonded was prepared in the same manner as in Experimental Example 5-1.

[0302] Preparation of the compound of Experimental Example 5-3

[0303] The compound of Experimental Example 5-3 in which an oxathiolane cation having a propyl group (R1) and a hydrofluoric acid salt anion were bonded was prepared in the same manner as in Experimental Example 5-1.

[0304] Preparation of the compound of Experimental Example 5-4

[0305] The compound of Experimental Example 5-3 in which an oxathiolane cation having a butyl group (R1) and a hydrofluoric acid salt anion were bonded was prepared in the same manner as in Experimental Example 5-1.

[0306] Preparation of the compound of Experimental Example 6-1

[0307] Prepare thiazolidine as a positive ion, use the hydrofluoride prepared according to the above Experimental Example 2-1 as a negative ion, and prepare the compound of Experimental Example 6-1 in which a thiazolidine positive ion having a methyl group (R1) and an ethyl group (R2) bonded to a nitrogen element and two methyl groups bonded to a sulfur element are combined with a hydrofluoride negative ion.

[0308] Preparation of the compound of Experimental Example 6-2

[0309] The compound of Experimental Example 6-2 was prepared by the same method as Experimental Example 6-1, wherein a thiazolidine cation having a methyl group (R1) and a propyl group (R2) bonded with a nitrogen element and two methyl groups bonded with a sulfur element were bonded to a hydrofluoride anion.

[0310] Preparation of the compound of Experimental Example 6-3

[0311] The compound of Experimental Example 6-3 was prepared by the same method as Experimental Example 6-1, wherein a thiazolidine cation having a methyl group (R1) and a butyl group (R2) bonded with a nitrogen element and two methyl groups bonded with a sulfur element were bonded to a hydrofluoride anion.

[0312] Preparation of the compound of Experimental Example 6-4

[0313] The compound of Experimental Example 6-4 was prepared by the same method as Experimental Example 6-1, wherein a thiazolidine cation having an ethyl group (R1) and a butyl group (R2) bonded with a nitrogen element and two methyl groups bonded with a sulfur element were bonded to a hydrofluoride anion.

[0314] The ionic conductivity of the compounds of Experimental Examples 2-1 to 6-4 was measured at room temperature, and the ionic molecular weight of the positive ions and the state information of the compounds of Experimental Examples 2-1 to 6-4 were sorted out as shown in Table 3.

[0315] Table 3

[0316]

[0317]

[0318] It can be confirmed in Table 3 that the cases containing thiophene as a positive ion (Experimental Examples 2-1 to 2-4), the cases containing thiazole having a methyl group, an ethyl group or a propyl group (Experimental Examples 3-1 to 3-3), the cases containing phosphotrimidine having a methyl / propyl group, a methyl / butyl group, an ethyl / butyl group or a methyl / methyl group (Experimental Examples 4-2 to 3-5), the cases containing oxathiolane having an ethyl group, a propyl group or a butyl group (Experimental Examples 5-2 to 5-4), and the cases containing thiazolidine having a methyl / ethyl group, a methyl / propyl group or a methyl / butyl group (Experimental Examples 6-1 to 6-3) all have high ionic conductivity.

[0319] Thiophene having a methyl group confirmed to have the highest ion conductivity in Table 3 was fixed as a positive ion, and different types of negative ions were used to prepare compounds for solid electrolytes according to Experimental Examples 7-1 and 7-2.

[0320] Preparation of the compound of Experimental Example 7-1

[0321] A cyano(nitroso)methanide was prepared as a negative ion, and the compound of Experimental Example 7-1 in which the thiophene positive ion having a methyl group of Experimental Example 2-1 and the cyano(nitroso)methanide negative ion were bonded was prepared.

[0322] Preparation of the compound of Experimental Example 7-2

[0323] Tetrazolidinium was prepared as a negative ion, and the compound of Experimental Example 7-2 in which the thiophene positive ion having a methyl group of Experimental Example 2-1 was combined with the tetrazolidinium negative ion was prepared.

[0324] The ionic conductivity of the compounds of Experimental Examples 7-1 and 7-2 was measured at room temperature, and the molecular weight of the negative ions and the state information of the compounds of Experimental Examples 7-1 and 7-2 were sorted out as shown in Table 4.

[0325] Table 4

[0326]

[0327] As shown in Table 4, it can be confirmed that the case of containing hydrofluoric acid salt as negative ions (Experimental Example 2-1), the case of containing cyano(nitro)methanide (Experimental Example 7-1), or the case of containing tetrazolidine (Experimental Example 7-2) all have high ion conductivity.

[0328] Preparation of the solid electrolyte of Experimental Example 8-1

[0329] After adding 1 M hydrofluoric acid aqueous solution and lithium chloride (LiCl) into a container, the container was left at -70°C for 24 hours to prepare lithium hydrofluoride.

[0330] The compound having a methyl group of Experimental Example 2-1 was heated to 60° C., and 1 mol % of lithium hydrofluoride was added and reacted for 2 hours to prepare a solid electrolyte of Experimental Example 8-1.

[0331] Preparation of the solid electrolyte of Experimental Example 8-2

[0332] The solid electrolyte of Experimental Example 8-2 was prepared by the same method as Experimental Example 8-1, except that 5 mol % of lithium hydrofluoride was added instead of 1 mol %.

[0333] Preparation of the solid electrolyte of Experimental Example 8-3

[0334] The solid electrolyte of Experimental Example 8-3 was prepared by the same method as Experimental Example 8-1, except that lithium hydrofluoride was added at 10 mol % instead of 1 mol %.

[0335] Fig.31 It is a curve chart of the compound of Experimental Example 2-1 and the solid electrolyte of Experimental Example 8-3 of the present application detected by differential scanning calorimetry.

[0336] Reference Fig.31 , a state change between solid-liquid or solid-solid according to temperature can be observed in the compound of Experimental Example 2-1 and the solid electrolyte of Experimental Example 8-3.

[0337] like Fig.31 As shown, the compound of Experimental Example 2-1 observed a solid-liquid state change at a temperature of 90° C. In contrast, the solid electrolyte of Experimental Example 8-3 observed a solid-liquid state change at a temperature of 70° C.

[0338] Furthermore, the compound of Experimental Example 2-1 was observed to have two solid-solid state changes, specifically, the compound of Experimental Example 2-1 may have a first crystalline phase in the temperature range of 28° C. to 90° C., and a second crystalline phase in the temperature range of 22° C. to 28° C. On the contrary, the solid electrolyte of Experimental Example 8-3 was observed to have only one solid-solid state change, specifically, it can be confirmed that it has one crystalline phase in the temperature range of 22° C. to 70° C.

[0339] Fig.32 This is a curve chart of the compounds of Experimental Example 7-1 and Experimental Example 7-2 of the present application detected by differential scanning calorimetry.

[0340] Reference Fig.32 , the temperature state changes of the compounds of Experimental Examples 7-1 and 7-2 were observed.

[0341] exist Fig.32It can be seen that the compounds of Experimental Examples 7-1 and 7-2 can be confirmed to stably maintain a solid crystalline phase within a relatively low temperature range. Specifically, it can be confirmed that the compound of Experimental Example 7-1 can stably maintain a solid crystalline phase within a range of -15°C to 98°C, and the compound of Experimental Example 7-2 can stably maintain a solid crystalline phase within a range of -59°C to 129°C. Moreover, although the compounds of Experimental Examples 7-1 and 7-2 have lower ionic conductivity than the compound of Experimental Example 2-1, Fig.17 As shown, compared with the temperature range (28°C to 90°C) in which the compound of Experimental Example 2-1 stably maintains the first crystalline phase, the crystalline phase is stably maintained in a wider temperature range. Therefore, the compounds of Experimental Examples 7-1 and 7-2 can be easily used in military or aerospace fields, or in low temperature environments such as polar regions.

[0342] Fig.33 It is a diagram for explaining the crystal structure of the solid electrolyte of Experimental Examples 8-1 to 8-3 of the present application.

[0343] Reference Fig.33 The solid electrolytes of Experimental Examples 8-1 to 8-3 may include thiophene cations, hydrofluoric acid anions, and lithium salts.

[0344] The unit cell of the compound in which the thiophene cation and the hydrofluorate anion are combined has an orthorhombic crystal structure, and the thiophene cation can be provided to the vertex and the center of the face of the crystal structure, and the hydrofluorate anion can be provided to the edge center of the upper crystal structure. In this case, the solid electrolyte of Experimental Examples 8-1 to 8-3 can randomly provide lithium salt to the interstitial sites of the crystal structure. Specifically, the lithium salt can be lithium hydrofluoride.

[0345] The lithium salt is provided to the lattice gap of the crystal structure of the compound, thereby making it possible to easily move within the crystal structure. Therefore, the more the amount of lithium hydrofluoride added as the lithium salt is increased, the more the ion conductivity can be improved.

[0346] Fig.34 It is a graph showing the ionic conductivity of the compound of Experimental Example 2-1 and the solid electrolytes of Experimental Examples 8-1 to 8-3 of the present application versus temperature.

[0347] Reference Fig.34 , the lithium ion conductivity of the compound of Experimental Example 2-1 and the solid electrolytes of Experimental Examples 8-1 to 8-3 was measured. Fig.33As described above, lithium hydrofluoride can be randomly provided to the lattice gaps of the crystal structure of the compound of the solid electrolyte of Experimental Examples 8-1 to 8-3. Therefore, lithium hydrofluoride can easily move within the crystal structure, and accordingly, it is observed that when the amount of lithium hydrofluoride added is increased, higher ion conductivity is obtained.

[0348] In this case, lithium hydrofluoride can move to the lattice gap in the crystal structure where lithium hydrofluoride is not provided, thereby showing high ion conductivity. Therefore, the more the lattice gap provided with lithium hydrofluoride increases, the more the increase rate of ion conductivity can tend to saturate. That is, Fig.34 As shown, it can be confirmed that when the addition amount of lithium hydrofluoride is 5 mol % or more, the ion conductivity is substantially saturated.

[0349] Fig.35 This is a picture taken of an electrolyte membrane coated with the solid electrolyte of Experimental Example 8-1 of the present application.

[0350] Reference Fig.35 , a solid electrolyte membrane in the form of a thin film in which the solid electrolyte of Experimental Example 8-1 of the present application is coated on a polytetrafluoroethylene (PTFE) resin was photographed. In this case, it can be confirmed that the solid electrolyte membrane maintains the flexibility and transparency of the above-mentioned resin.

[0351] The preferred embodiments of the present application are described in detail above, but the scope of the present application is not limited to the specific embodiments, but should be interpreted by the scope of the attached claims. In addition, it should be understood that a person skilled in the art of the present invention can make various modifications and variations without departing from the scope of the present application.

[0352] Industrial Applicability

[0353] The electrodes of the embodiments of the present application can be used as electrodes of secondary batteries, supercapacitors, etc.

Claims

1. A method for preparing an electrode intermediate product, characterized in that: include: a step of preparing elementary particles comprising a metal, a metal oxide, a metal carbide or a carbon structure; a step of mixing the elementary particles and a coating source comprising a first metal to form a coating comprising the first metal on the surface of the elementary particles, wherein the first metal comprises lithium; and The step of heat-treating the primary particles having the coating layer and the second metal to form a molten source formed by melting the primary particles having the coating layer and the second metal, wherein the second metal includes lithium.

2. The method for preparing an electrode intermediate product according to claim 1, characterized in that: The above-mentioned elementary particles include at least one of SiO2, TiO2, Mg, Ti3C2, and CuO.

3. The method for preparing an electrode intermediate product according to claim 1, characterized in that: The above elementary particles include a carbon structure, Before mixing the primary particles with the coating source, the method further comprises the step of pretreating the primary particles with a metal nitric acid solution.

4. The method for preparing an electrode intermediate product according to claim 1, characterized in that: After the above-mentioned elementary particles and the above-mentioned coating source are mixed, heat treatment is performed at a temperature higher than normal temperature.

5. The method for preparing an electrode intermediate product according to claim 1, characterized in that: The method for preparing the coating source comprises: The steps of preparing a first precursor comprising sulfur and chlorine, a second precursor comprising sulfur and chlorine, and a third precursor comprising sulfur and nitrogen; A step of reacting the first precursor, the second precursor and the third precursor to prepare a first compound containing sulfur, chlorine, oxygen, nitrogen and hydrogen; A step of reacting the first compound with a fourth precursor containing fluorine to prepare a second compound; and a step of reacting the second compound with a metal salt containing a first metal to prepare a third compound, The coating source includes compounds of lithium, nitrogen, fluorine, sulfur, carbon and oxygen.

6. The method for preparing an electrode intermediate product according to claim 5, characterized in that: Before reacting the second compound and the metal salt, the method further comprises reacting the second compound with deionized water at a temperature lower than room temperature. The step of preparing the third compound includes the step of reacting the second compound reacted with deionized water with the metal salt.

7. An electrode film or electrode particle, characterized in that: It is formed by solidifying a molten source which melts together a primary particle including a metal, a metal oxide, a metal carbide or a carbon structure and a coating provided on the surface of the primary particle and including a first metal and a second metal, wherein the first metal and the second metal include lithium.

8. The electrode film or electrode particle according to claim 7, characterized in that: The elementary particles include at least one of silicon oxide, aluminum, aluminum oxide, copper, copper oxide, titanium, titanium oxide, titanium carbide, magnesium, tin, tin oxide, germanium, bismuth, molybdenum, or a carbon structure.

9. A negative electrode, characterized in that: Contains the electrode film or electrode particles according to claim 7.

Citation Information

Patent Citations

  • Cathode material for rechargeable solid state lithium ion battery

    CN108028371A

  • Electrode materials and method for preparing thereof

    KR1020030030818A