Device and method for in-situ self-heating effect assisted 3D printing of TiAl complex metal components
Through in-situ autothermal effect assisted 3D printing technology, arc induction heating is used to promote the interfacial diffusion reaction between Ti and Al atoms, forming uniform intermetallic compounds of TiAl, which solves the problems of interfacial cracks and uneven distribution during LDED forming and improves TiAl Mechanical properties and service cycle of alloy components.
Patent Information
- Application Number
- CN202210294246.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-23
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-03-23
AI Technical Summary
During the existing LDED forming and manufacturing process, TiAl alloy 3D printed forming members are prone to interfacial cracks and uneven distribution of intermetallic compounds, resulting in uneven distribution of internal stresses of the material and reducing the service cycle of the components.
Using in-situ autothermal effect assisted 3D printing forming technology, the induction heating device is used to perform induction heating after each layer of the deposited body is completed, which promotes the diffusion and reaction of Ti and Al atoms at the interface, forms a uniform TiAl intermetallic compound and inhibits the formation of cracks. .
High-quality, high-precision, defect-free TiAl alloy component forming is achieved, improving the mechanical properties and service cycle of the components, and reducing the forming time and cost.
Smart Images

Figure CN114769624B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of 3D printing of metal components, and in particular relates to a device and method for in-situ self-heating effect assisted 3D printing of TiAl complex metal components. Background Art
[0002] TiAl alloy has unique comprehensive properties (high specific stiffness, elastic modulus and density ratio), and TiAl, Ti3Al, etc. are a new generation of high-performance structural materials. They have low density, high temperature strength, high melting point, excellent creep resistance, oxidation resistance and high specific stiffness. The above excellent material properties make them widely used in the field of aviation structures. Compared with traditional nickel-based high-temperature alloys and titanium alloys, TiAl alloy has a density of 3.5g / cm 3 ) is only about nickel-based high-temperature alloy (8.3g / cm 3 ) half; in terms of mechanical properties at room temperature: the specific stiffness of TiAl alloy (150GPa) is higher than that of titanium alloy (110GPa), but lower than that of nickel-based high-temperature alloy (206GPa); high-temperature mechanical properties: the creep limit (1000℃) and oxidation limit (1000℃) of TiAl alloy are higher than those of titanium alloy (creep limit is 600℃, oxidation limit is 600℃+), but slightly lower than those of nickel-based high-temperature alloy (creep limit is 1093℃, oxidation limit is 1093℃). It can be seen that although TiAl alloy is not as good as nickel-based high-temperature alloy in some aspects, the density of TiAl alloy is significantly lower than that of nickel-based high-temperature alloy, and the specific stiffness is comparable to that of nickel-based high-temperature alloy. Therefore, TiAl alloy is expected to replace the existing nickel-based high-temperature alloy system and has broad application prospects in the aviation industry and the automotive industry. TiAl alloy is considered to be the preferred material for stationary and rotating parts of new aerospace engines, such as nozzle adjustment fish scales, high-pressure compressor guide vanes and piston covers.
[0003] Traditional forming methods for TiAl alloys mainly include precision casting and powder metallurgy. There are two main types of precision casting: one is investment casting and the other is metal mold casting. Investment casting is mainly used to form TiAl alloy components with complex shapes; while metal mold casting is mainly used to produce components with regular shapes and large output. Components formed by precision casting mainly have the advantages of low cost and easy forming; but the casting process will have serious casting defects (pores, looseness, etc.) and the cooling process will easily cause component cracking, which greatly reduces the mechanical properties of the components, especially the ductility of the components at room temperature. Although investment casting can form components with relatively complex structures, it is difficult to achieve one-piece forming with sharp corners or thin-walled structures.
[0004] Powder metallurgy is another common method for forming TiAl alloy components. Powder metallurgy can avoid the problems of component segregation, coarse grains and uneven structure in casting, thereby improving the ductility of TiAl alloy components at room temperature. However, the binder added during the powder metallurgy process makes it difficult to control the interstitial element composition and microstructure and phase, which in turn limits the use of this method.
[0005] 3D printing technology can efficiently form complex metal components in one piece. Since 3D printing technology is different from traditional subtractive and equal-material forming methods, 3D printing uses high-energy beams to quickly melt and solidify metal powders, and forms three-dimensional components by metallurgical bonding of the two-dimensional cross-section of periodically fused components along the forming direction. Based on the three-dimensional-two-dimensional-three-dimensional forming principle, it can maximize the integrated forming of complex components. Therefore, 3D printing can basically prepare components of any complex structure.
[0006] Although complex structure TiAl alloy components can be formed by the existing 3D printing technology (laser directed energy deposition, abbreviated as LDED), due to the rapid heating and cooling of the LDED forming process, on the one hand, cracks are very likely to initiate at the interface position of the TiAl alloy 3D printed components during the forming process. On the other hand, it is also easy to cause uneven distribution of intermetallic compounds in the TiAl alloy 3D printed components. Therefore, when the TiAl alloy 3D printed components are under load, the presence of the interface and the TiAl intermetallic compounds makes the internal stress distribution of the material uneven, resulting in the initiation and expansion of cracks, which greatly reduces the service life of the components. Summary of the invention
[0007] Purpose of the invention: In view of the problems existing in the existing LDED forming manufacturing, the purpose of the present invention is to improve it, specifically to provide a device and method for in-situ self-heating effect assisted 3D printing of TiAl complex metal components, which drives the chemical components (Ti, Al) of the 3D printed components to diffuse and react at the 3D printing interface through the assistance of the in-situ thermal effect process during the 3D printing (LDED) forming process to form intermetallic compounds, so as to ultimately be able to produce high-quality, high-precision, defect-free and homogenized TiAl alloy components with complex structures.
[0008] In order to achieve the above technical objectives, the present invention will adopt the following technical solutions:
[0009] A device for in-situ self-heating effect assisted 3D printing of TiAl complex metal components, comprising LDED forming equipment and arc induction heating equipment; the LDED forming equipment comprises an LDED control device, a printing platform and a laser printing deposition head, and the laser printing deposition head, under the control of the LDED control device, can deposit on the printing platform according to a printing path preset in the LDED control device to form a deposition body, the deposition body comprising alternately stacked Ti deposition layers, Al deposition layers and an interface layer between the Ti deposition layers and the Al deposition layers; the arc induction heating equipment comprises a lifting mechanism, an arc induction coil and an induction relay;
[0010] The arc induction coil is arranged outside the outline of the deposition body, and the arc induction coil is connected to the power supply after being connected in series with the induction relay, and the arc induction coil is connected to the power output end of the lifting mechanism. The lifting mechanism can drive the arc induction coil to rise and fall relative to the printing platform under the control of the LDED control device;
[0011] After each N deposition layers are deposited on the deposition body, the portion with a height H among the deposited N deposition layers is induction heated synchronously by controlling the lifting mechanism; wherein:
[0012] H=H N -n
[0013] Where: H N It represents the total height of N deposited layers, N≥1; n represents the size parameter of the heat affected zone.
[0014] Preferably, the arc induction coil is a spiral heating coil; the spiral heating coil comprises several layers of heating coils, and an induction relay is installed on each layer of heating coils;
[0015] Each layer of heating coils corresponds to a deposition layer of the deposition body;
[0016] The LDED control device can dynamically open or close the corresponding induction relay on the spiral heating coil according to the deposition speed of each deposition layer in the deposition body.
[0017] Preferably, the LDED control device can determine the moving speed v of the spiral heating coil driven by the lifting mechanism according to the laser scanning rate v1 and the induction heating time τ required for the deposited body consisting of N deposited layers. r And the heating time t of each layer of heating coil.
[0018] Preferably, the moving speed v of the spiral heating coil is r satisfy:
[0019]
[0020] In the above formula, C represents the number of deposited layers that need induction heat treatment in the deposited body; k1, k2, k3 represent the velocity proportional coefficients under different ranges of the number of deposited layers, and x i is the thickness of the sediment layer.
[0021] Preferably, the number of turns of the heating coil required for a deposition body consisting of N deposition layers is:
[0022] ω=ΔI ω ×H / I
[0023] Where: ΔI ω It represents the ampere-turn per unit length of the heating coil, H represents the height of the portion that needs to be inductively heated in the deposition body composed of N deposition layers; I represents the current of the heating coil.
[0024] Preferably, the current I of the heating coil is:
[0025]
[0026] The electric power P of the induction heating coil Q :
[0027]
[0028] The induction heat Q required for a deposit consisting of N deposit layers:
[0029] Q=M×θ×(T m -T0)
[0030] Where: U represents the potential amplitude of the power supply; represents the electric power factor; η represents the thermal efficiency; τ represents the induction heating time required for the deposit composed of N layers of deposits; M represents the mass of the deposit composed of N layers of deposits; θ represents the specific heat capacity of the deposit; T m It represents the temperature of the deposited body consisting of N deposited layers after being heated by the induction heating coil; T0 represents the ambient temperature.
[0031] Preferably, the temperature of the deposited body composed of N deposited layers after being heated by the induction heating coil is T m satisfy:
[0032]
[0033]
[0034] H 2 = k′1τ k
[0035] Where: H represents the thickness of the deposited body consisting of N deposited layers that needs to be inductively heated; k is a constant related to material properties; D is the diffusion coefficient; τk is the diffusion time; k′1 is the diffusion layer growth coefficient; K is a constant; Q n is the diffusion activation energy; R is the gas constant; T m It is the temperature of the deposited body consisting of N deposited layers after being heated by the induction heating coil.
[0036] Preferably, the LDED control device can be controlled by adjusting the laser power P, the laser scanning rate v1 and the cooling rate v2.
[0037] Another technical purpose of the present invention is to provide a method for in-situ self-heating effect assisted 3D printing of TiAl complex metal components, which is based on the above-mentioned in-situ self-heating effect assisted 3D printing of TiAl complex metal components The method comprises the following steps:
[0038] Step 1: Use LDED forming process to print a deposit with a preset thickness
[0039] Based on LDED forming equipment, the LDED forming process is adopted to alternately print Ti and Al metal powders according to a preset printing path to obtain a deposited body with a preset thickness;
[0040] The deposited body comprises a stacked Ti deposited layer, an Al deposited layer and an interface layer at the interface of the Ti deposited layer and the Al deposited layer;
[0041] During the printing process of the deposited body, by adjusting the process parameters of the LDED forming process, a TiAl intermetallic compound wrapped between the Ti deposited layer and the Al deposited layer is formed in the interface layer to inhibit the TiAl intermetallic compound from forming cracks;
[0042] Step 2: In-situ thermal post-treatment process promotes the formation of TiAl intermetallic compounds in the interface layer of the deposit
[0043] Based on arc induction heating equipment, an in-situ thermal post-treatment process is used to perform induction heat treatment on the deposited body obtained in step one, so as to drive the metal Ti atoms of the Ti deposition layer to break free from their constraints and diffuse toward the interface layer, and the metal Al atoms of the Al deposition layer to break free from their constraints and diffuse toward the interface layer, thereby inducing the TiAl intermetallic compound formed in the interface layer to gradually grow, so as to promote the formation of the TiAl intermetallic compound, and make the TiAl intermetallic compound between the Ti deposition layer and the Al deposition layer uniform.
[0044] Preferably, in step 1, during the printing process of the deposited body, the process parameters of the LDED forming process to be regulated include the laser power P, the laser scanning rate v1 and the cooling rate v2; in step 2, the moving speed v of the spiral heating coil driven by the lifting mechanism is determined according to the laser scanning rate v1 and the induction heating time τ required for the deposited body composed of N deposited layers. r And the heating time t of each layer of heating coil.
[0045] Based on the above technical solution, compared with the prior art, the present invention has the following advantages:
[0046] (1) The present invention uses LDED technology and in-situ heat treatment composite process to achieve integrated forming of complex structures of TiAl materials with high defect tendency; at the same time, product customization can be achieved according to production needs and delivery cycle can be shortened. Compared with traditional processing methods, the yield rate and complexity of components can be improved. Therefore, it has good economic value.
[0047] (2) The present invention uses an in-situ self-heating effect method to simultaneously heat treat the deposited metal layer. -6 / K) and pure Al (23×10 -6 / K) thermal expansion coefficient and Poisson's ratio of Ti, Al and TiAl are 0.34, 0.25 and 0.24 respectively, which leads to a high volume expansion rate of Al in the forming process, and then micro cracks are prone to appear on the TiAl interface, which significantly reduces the mechanical properties of the material; at the same time, due to the difference in plastic deformation capacity of heterogeneous materials during the load-bearing process, micro cracks are prone to appear first on the side of the material with poor plasticity. An in-situ dynamic heat treatment scheme is adopted, and the heated tungsten wire dynamically acts on the pure Ti and pure Al areas, prompting the continuous diffusion reaction between atoms to produce TiAl intermetallic compounds. The above process can effectively eliminate the plastic deformation and micro cracks of the material caused by the difference in thermophysical parameters. At the same time, the homogenized TiAl intermetallic compounds formed under the combined action of LDED and in-situ heat treatment can effectively improve the mechanical properties of the overall metal components.
[0048] (3) The present invention adds a spiral heating tungsten wire to the substrate, so that the material can be heat treated synchronously during the laser processing process, which greatly reduces the forming time of a single metal component and reduces the time cost.
[0049] (4) The present invention designs a spiral heating tungsten wire for induction heating, and an induction relay is provided on each layer of the tungsten wire. When a layer of material is deposited, the induction relay receives a signal and converts the heat signal into an electrical signal, which is then transmitted to the induction heating coil. The tungsten wire receives the signal and is induction heated. Finally, the purpose of induction heating a layer of material after each layer of material is deposited is achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 The heat treatment equipment based on the in-situ self-heating effect of the present invention;
[0051] Figure 2 The Ti-Al phase diagram of the TiAl complex metal component printed by the present invention;
[0052] Figure 3 The particle size distribution of the special metal powder used in the present invention;
[0053] Figure 4a This is the Ti-Al interface microstructure diagram of the TiAl complex metal component slice obtained by the existing LDED forming technology under an optical microscope. Figure 4b A microstructure diagram of a Ti-Al interface of a TiAl complex metal component slice obtained by the method of the present invention under an optical microscope;
[0054] Figure 5a The Ti-Al interface microstructure of the TiAl complex metal component slice formed by LDED under a scanning electron microscope. Figure 5b A microstructure diagram of a Ti-Al interface of a TiAl complex metal component slice obtained by the method of the present invention under a scanning electron microscope;
[0055] Figure 6a , Figure 6b They respectively correspond to the area and diffraction pattern of the transmission electron microscope under the scanning electron microscope of the TiAl complex metal component slice obtained by the method of the present invention.
[0056] Figure 7 The present invention is a flowchart of the method.
[0057] Figure 8 ae represent the heat affected zone n of the TiAl alloy component at different deposition layers. DETAILED DESCRIPTION
[0058] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. Unless otherwise specified, the relative arrangement, expressions and numerical values of the components and steps described in these embodiments do not limit the scope of the present invention. The techniques, methods and devices known to ordinary technicians in the relevant fields may not be discussed in detail, but where appropriate, the techniques, methods and devices should be regarded as part of the authorization specification. In all examples shown and discussed here, any specific value should be interpreted as merely exemplary, not as a limitation. Therefore, other examples of the exemplary embodiments may have different values.
[0059] The present invention improves the performance of TiAl complex metal components obtained by existing LDED forming technology by changing the interface structure of TiAl complex metal components obtained by existing LDED forming technology. To this end, during the LDED forming process, the present invention uses an in-situ thermal effect auxiliary process to drive the chemical components (Ti, Al) of the 3D printed formed components to diffuse and react at the 3D printed interface. Specifically, based on the existing LDED forming equipment, an in-situ heat treatment equipment based on the self-heating effect (arc induction heating equipment, structured as Figure 1 As shown in the figure, the control device of the existing LDED forming equipment is adjusted so that the in-situ heat treatment equipment performs in-situ induction heat treatment after the LDED forming equipment completes a deposition body of a certain thickness (formed by alternating stacking of Ti deposition layers and Al deposition layers), so as to achieve the purpose of simultaneous treatment of the three-dimensional deposition of the component and the in-situ self-heating effect.
[0060] It can be seen that the device for in-situ self-heating effect assisted 3D printing of TiAl complex metal components described in the present invention includes LDED forming equipment and arc induction heating equipment; wherein:
[0061] The LDED forming equipment includes an LDED control device, a printing platform and a laser printing deposition head. Under the control of the LDED control device, the laser printing deposition head can deposit on the printing platform according to a printing path preset in the LDED control device to form a deposition body. The deposition body includes alternately stacked Ti deposition layers, Al deposition layers and an interface layer between the Ti deposition layers and the Al deposition layers.
[0062] The arc induction heating device comprises a lifting mechanism, an arc induction coil and an induction relay;
[0063] The arc induction coil is arranged outside the outline of the deposition body, and the arc induction coil is connected to the power supply after being connected in series with the induction relay, and the arc induction coil is connected to the power output end of the lifting mechanism. The lifting mechanism can drive the arc induction coil to rise and fall relative to the printing platform under the control of the LDED control device;
[0064] After each N deposition layers are deposited on the deposition body, the portion with a height H among the deposited N deposition layers is induction heated synchronously by controlling the lifting mechanism; wherein:
[0065] H=H N -n
[0066] Where: H N It represents the total height of N deposited layers, N≥1; n represents the size parameter of the heat affected zone.
[0067] Preferably, the arc induction coil is a spiral heating coil; the spiral heating coil includes several layers of heating coils, and an induction relay is installed on each layer of heating coils; each layer of heating coils corresponds to a deposition layer of the deposition body; the LDED control device can dynamically open or close the corresponding induction relay on the spiral heating coil according to the deposition speed of each deposition layer in the deposition body.
[0068] Preferably, the LDED control device can determine the moving speed v of the spiral heating coil driven by the lifting mechanism according to the laser scanning rate v1 and the induction heating time τ required for the deposited body consisting of N deposited layers. r And the heating time t of each layer of heating coil.
[0069] Preferably, the moving speed v of the spiral heating coil is r satisfy:
[0070]
[0071] In the above formula, C represents the number of deposited layers that need induction heat treatment in the deposited body; k1, k2, k3 represent the velocity proportional coefficients under different ranges of the number of deposited layers, and x i is the thickness of the sediment layer.
[0072] Preferably, the number of turns of the heating coil required for a deposition body consisting of N deposition layers is:
[0073] ω=ΔI ω ×H / I
[0074] Where: ΔI ω It represents the ampere-turn per unit length of the heating coil, H represents the height of the portion that needs to be inductively heated in the deposition body composed of N deposition layers; I represents the current of the heating coil.
[0075] Preferably, the current I of the heating coil is:
[0076]
[0077] The electric power P of the induction heating coil Q :
[0078]
[0079] The induction heat Q required for a deposit consisting of N deposit layers:
[0080] Q=M×θ×(T m -T0)
[0081] Where: U represents the potential amplitude of the power supply; represents the electric power factor; η represents the thermal efficiency; τ represents the induction heating time required for the deposit composed of N layers of deposits; M represents the mass of the deposit composed of N layers of deposits; θ represents the specific heat capacity of the deposit; T m It represents the temperature of the deposited body consisting of N deposited layers after being heated by the induction heating coil; T0 represents the ambient temperature.
[0082] Preferably, the temperature of the deposited body composed of N deposited layers after being heated by the induction heating coil is T m satisfy:
[0083]
[0084]
[0085] H 2 = k′1τ k
[0086] Where: H represents the thickness of the deposited body consisting of N deposited layers that needs to be inductively heated; k is a constant related to material properties; D is the diffusion coefficient; τ k is the diffusion time; k′1 is the diffusion layer growth coefficient; K is a constant; Q n is the diffusion activation energy; R is the gas constant; T m It is the temperature of the deposited body consisting of N deposited layers after being heated by the induction heating coil.
[0087] Preferably, the LDED control device can be controlled by adjusting the laser power P, the laser scanning rate v1 and the cooling rate v2.
[0088] Based on the above-mentioned device for in-situ self-heating effect assisted 3D printing of TiAl complex metal components, the present invention provides a method for in-situ self-heating effect assisted 3D printing of TiAl complex metal components, such as Figure 8As shown, the following steps are included:
[0089] Step 1: Use LDED forming process to print a deposit with a preset thickness
[0090] Using the LDED forming process, Ti and Al metal powders are alternately printed according to a preset printing path to obtain a deposited body with a preset thickness;
[0091] The deposited body comprises a stacked Ti deposited layer, an Al deposited layer and an interface layer at the interface of the Ti deposited layer and the Al deposited layer;
[0092] During the printing and forming process of the deposited body, the process parameters of the LDED forming process are adjusted so that a TiAl intermetallic compound wrapped between the Ti deposited layer and the Al deposited layer is formed in the interface layer to inhibit the TiAl intermetallic compound from forming cracks; specifically, the present invention selects the laser power P, scanning rate v1, powder feeding amount δ and material cooling rate v2 of the LDED forming process by studying the TiAl intermetallic compound phase region temperature in the TiAl alloy phase diagram, so that a TiAl intermetallic compound wrapped between the Ti deposited layer and the Al deposited layer is formed in the interface layer to inhibit the TiAl intermetallic compound from forming cracks.
[0093] Step 2: In-situ thermal post-treatment process promotes the formation of TiAl intermetallic compounds in the interface layer of the deposit
[0094] The deposited body obtained in step one is subjected to induction heat treatment by an in-situ thermal post-treatment process (mainly an in-situ induction heat treatment process) to drive the metal Ti atoms of the Ti deposition layer to break free from their constraints and diffuse toward the interface layer, and the metal Al atoms of the Al deposition layer to break free from their constraints and diffuse toward the interface layer, thereby inducing the TiAl intermetallic compound formed in the interface layer to gradually grow, so as to promote the formation of the TiAl intermetallic compound and make the TiAl intermetallic compound between the Ti deposition layer and the Al deposition layer uniform.
[0095] The in-situ induction heat treatment process is realized by an in-situ induction heat treatment device (arc induction heating device), and the key component of the arc induction heating device is the design of the induction heating coil. The present invention is aimed at the size of the formed component (volume V, surface area S and material mass M of the material), the structural shape and the thermal driving temperature (based on the surface unit power ΔP when the material is heated). s The material absorbs heat Q to complete the material needs to absorb heat to the induction heating coil electrical power P QThe in-situ heating coil design is completed by the conversion) and stress relief annealing temperature T (the current I of the heating coil, the number of heating coil turns ω required for the deposition body composed of N deposited layers in the induction heating coil). During the forming process of the component LDED, the coil can be adjusted according to the scanning rate v1 and the deposition rate v c The moving speed v of the induction heating coil is determined by the time τ that the material needs to be heat treated. r , so that the material forming and the in-situ heat treatment of the material can be carried out simultaneously; at the same time, the digital drive coil moves synchronously according to the spatial deposition speed of the component, so that the overall heat treatment process of the material can be completed automatically. After the in-situ heat treatment, the whole material is a TiAl intermetallic compound, thereby improving the performance of the overall component.
[0096] The LDED forming equipment deposits powders of Ti and Al alternately. By adjusting the forming process parameters, laser power P, laser scanning rate v1 and cooling rate v2, TiAl metal compounds are stably generated on the interface when the TiAl metal component is formed. Specifically, by observing the TiAl phase diagram (such as Figure 2 The stable phase region of the TiAl intermetallic compound in the material is determined by the laser power P and the scanning rate v1, and the cooling rate v2 of the material is determined. The laser power P and the scanning rate v1 are controlled to cool the material along the phase region of the TiAl intermetallic compound during the deposition and forming process, so as to achieve the purpose of obtaining the TiAl intermetallic compound during the three-dimensional deposition and forming process of the component. At the same time, the deposition thickness of the Ti and Al layers are recorded as h1 and h2 respectively. In step 2, the heat treatment temperature that needs to be reached by the in-situ self-heating effect of the formed component is calculated as T m ; The ambient temperature is T0. The outer diameter of the deposition cylinder is D w , inner diameter is D n , the overall height of the component is H1, and the specific heat capacity of the component material is θ. Therefore, the volume of the material heated is:
[0097]
[0098] The surface area of the material after heating is recorded as:
[0099]
[0100] The mass of the component is recorded as:
[0101]
[0102] In the above formula, γ is the density of the heated material.
[0103] The amount of heat that the material needs to absorb during in-situ heat treatment is:
[0104] Q=M×θ×(T m-T0) (4)
[0105] The heat required for heating the component is converted into the electrical power of the induction heating coil:
[0106]
[0107] In the above formula, η is the thermal efficiency during heating (the heating efficiency can be taken as 0.8), and τ is the time required for heating.
[0108] The current of the heating coil is:
[0109]
[0110] In the above formula It is the power factor of the power supply (the power factor can be 0.8).
[0111] The power per unit surface area of the heated component is:
[0112] ΔP s =P Q ×1000 / S (7)
[0113] Therefore, we calculated the number of heating coil turns required for a deposit consisting of N deposit layers as:
[0114] ω=ΔI ω ×H / I (8)
[0115] In the above formula, ΔI ω is ampere-turn per unit length, which can be calculated based on ΔP s With ΔI ω The curvilinear relationship between them is obtained.
[0116] After the component is formed, the metal component is post-processed using the designed in-situ self-heating effect heat treatment device. The arc induction heater is equipped with an induction relay. After the N layer of Ti or Al material ts is deposited by LDED, the previous Nn (n is the size parameter of the heat affected zone) deposition layer is induction heated simultaneously.
[0117] Because the heat of the first deposited Ti or Al deposition layer will be transferred in the depth direction, the heat affected zone of the current deposited Ti or Al deposition layer will expand. Therefore, the temperature of the later deposited layer is higher than that of the earlier deposited layer and the temperature tends to be stable after a certain number of layers are deposited. In order to achieve the goal of synchronous treatment of the three-dimensional deposition of the component and the in-situ self-heating effect, the induction heater will move synchronously in the Z direction with the deposition rate to achieve the goal of dynamic synchronous heat treatment of the component. Therefore, when the electromagnetic induction heating coil heats the first deposited layer, the heat affected zone is smaller and the temperature is lower, so a longer heating time is required. The moving speed v of the electromagnetic induction heating coil is rThe later deposited layer has a larger heat affected zone and a higher temperature, so the required heating time is shorter than that of the earlier deposited layer. The moving speed of the electromagnetic induction heating coil is v r Faster. Specifically, the moving speed v r for:
[0118]
[0119] In the above formula, k1, k2, k3 are velocity proportional coefficients in the range of 0<C≤2, 3≤C≤4, C≥5 of the sedimentary layer, respectively, and x i is the thickness of the sediment layer.
[0120] Finally, the homogenization process of TiAl compounds generated by the deposition interface and thermal diffusion reaction of LDED formed components is achieved, that is, all metal components are TiAl intermetallic compounds. Thanks to the excellent material properties of TiAl intermetallic compounds, the one-piece formed metal components have excellent mechanical properties.
[0121] As a preferred embodiment of the present invention, the cooling rate v2 is obtained by controlling the laser power P during laser scanning, the laser scanning rate v1, and the phase region where the TiAl intermetallic compound exists observed through the TiAl phase diagram to estimate, thereby achieving effective regulation of the formation of the TiAl intermetallic compound.
[0122] As a preferred embodiment of the present invention, during the forming process, we use the in-situ self-heating effect to heat treat the metal components after forming, so as to realize the continuous diffusion and reaction of Ti and Al atoms to form TiAl intermetallic compounds, so as to achieve the goal of homogenizing the TiAl intermetallic compounds.
[0123] As a preferred embodiment of the present invention, based on the arc induction in-situ dynamic heating method, the induction heating device is placed outside the contour of the pre-deposition body, and then the Z-direction deposition speed v of the LDED formed component is determined. c The in-situ heat treatment device and the metal component forming are dynamically synchronized with the size n of the heat-affected zone.
[0124] As a preferred embodiment of the present invention, an induction relay is installed on the heating coil of each layer, so that the induction relay can dynamically turn off / on the heat treatment according to the material deposition speed, and the heating time t of the coil and the coil movement speed v can be determined according to the laser scanning rate v1 and the heat treatment time τ of the metal component. r .
[0125] As a preferred embodiment of the present invention, when laser additive manufacturing is used to form TiAl intermetallic compounds, the elastic modulus and thermal expansion coefficient of pure Ti and pure Al are different (the elastic modulus and thermal expansion coefficient of pure Ti are 106.4 GPa and 8.6×10 -6 / K; the elastic modulus and thermal expansion coefficient of pure Al are 70GPa and 23×10 -6 / K), resulting in tiny cracks at the interface of different deposited layers during the forming process. However, the in-situ self-heating effect method of the LDED deposition process proposed by the present invention: (1) the thermal stress and volume change stress of the TiAl intermetallic compound formed at the interface of Ti and Al during the LDED deposition process are wrapped by the Ti and Al materials with excellent plasticity, (2) the in-situ self-heating effect combined with the LDED forming heat-affected zone can promote the diffusion of Ti and Al atoms while reducing the residual stress and cracking tendency, and ultimately achieve the goal of overall material homogenization.
[0126] The thickness of the component reaction diffusion layer is related to the electromagnetic induction heating time and heating temperature. As the temperature rises, the component Gibbs free energy G gradually increases; when the Gibbs free energy G exceeds the energy barrier required for atomic motion (i.e., the diffusion activation energy Q n ), Ti and Al atoms break away from the bond between atoms, so that the atoms in the Ti and Al deposition layers react and diffuse with each other, so as to achieve the purpose of expanding the TiAl intermetallic compound phase region. The relationship between the diffusion reaction layer thickness and the diffusion time is parabolic:
[0127]
[0128] x 2 = k′1τ k (11)
[0129]
[0130] In the above formula, x is the thickness of the diffusion layer; k is a constant related to material properties; D is the diffusion coefficient; τ k is the diffusion time; k′1 is the diffusion layer growth coefficient; K is a constant; Q n is the diffusion activation energy; R is the gas constant; T m It is the temperature of the deposited body consisting of N deposited layers after being heated by the induction heating coil.
[0131] Figure 4a This is the Ti-Al interface microstructure diagram of the TiAl complex metal component slice obtained by the existing LDED forming technology under an optical microscope. Figure 4bThe microstructure diagram of the Ti-Al interface of the TiAl complex metal component slice obtained by the method of the present invention under an optical microscope. Through analysis, before the material undergoes in-situ self-heating effect, micro cracks will still be generated at the TiAl deposition interface due to the rapid heating and cooling during the LDED forming process. After the in-situ self-heating effect interacts with the heat-affected zone during LDED forming, the TiAl intermetallic compound is wrapped by the Ti and Al materials with excellent plasticity, so that the internal stress and deformation of the TiAl intermetallic compound under the LDED forming cycle heat treatment are absorbed by the Ti and Al materials, inhibiting the formation of cracks in the TiAl intermetallic compound.
[0132] Figure 5a The Ti-Al interface microstructure of the TiAl complex metal component slice formed by LDED under a scanning electron microscope. Figure 5b A microstructure diagram of a Ti-Al interface of a TiAl complex metal component slice obtained by the method of the present invention under a scanning electron microscope;
[0133] Figure 6a , Figure 6b They correspond to the area and diffraction pattern of the transmission electron microscope under the scanning electron microscope of the TiAl complex metal component slice obtained by the method of the present invention. After the in-situ self-heating effect of the component interacts with the LDED forming heat-affected zone, the TiAl intermetallic compound area gradually grows. By analyzing the growing area through the transmission electron microscope, it can be determined that the growing intermetallic compound is a TiAl intermetallic compound.
[0134] Application Examples
[0135] The raw material Ti and Al powders are 40 to 80 μm in size. High-energy beams are used to rapidly melt and solidify the metal powders, and the two-dimensional cross-sections of the periodic molten components are metallurgically bonded along the forming direction to form three-dimensional components. The laser scanning rate is 3 mm / s, the laser power is 2000 W, and the powder feeding rate is 10 r / min. The inner diameter of the formed component is D n 160mm, outer diameter D w The wall thickness is 170mm, the wall thickness is 10mm, and the height H1 is 205mm.
[0136] The volume and surface area of the component are calculated by the above formulas (1) and (2).
[0137] After LDED forming, the metal components are post-processed using an in-situ self-heating effect heat treatment device. The heat treatment temperature is 650℃, which is recorded as T m, the heating time is τ. And an induction relay is equipped on the arc induction coil. After each deposition of N layers of material ts, the previous Nn (n is the size parameter of the heat-affected zone) deposition layers are induction heated synchronously to achieve the purpose of simultaneous treatment of the three-dimensional deposition of the component and the in-situ self-heating effect. The thermal efficiency is 0.8, and the number of heating coil turns ω required for the deposition body composed of N layers of deposition layers is calculated. The heat Q required to be absorbed by the component to achieve homogenization is calculated, and the required heat Q is converted into the electrical power P of the induction heating coil Q (Calculated by formula 3 above). By calculating the electric power P of the induction heating coil required to heat the material to the required temperature Q , and calculate the current I of the heating coil and the unit power ΔP of the surface area s , through the unit length ampere-turn ΔI ω Power per unit surface area ΔP s The relationship curve between the electromagnetic induction coil and the ampere-turn per unit length ΔI is determined ω The number of turns of the electromagnetic induction coil is calculated by the above formula (8).
[0138] According to the simulation results, the range of the heat affected zone is determined in the number of layers C of the deposited layers that need induction heat treatment in the deposited body. Determine the range of the heat affected zone of the formed component, the number of layers C of the deposited layers that need induction heat treatment in the deposited body, and the moving speed v of the electromagnetic induction heating coil. r .
[0139] During the deposition process, as the number of deposition layers of the component increases, the heat affected zone of the material (Figure 5) gradually increases. When the deposition layer increases from one layer to five layers, the sizes of the heat affected zone of the material are 0.834mm, 0.995mm, 1.609mm, 1.974mm, and 2.302mm, respectively. The moving speed of the electromagnetic induction heating coil should satisfy the relationship between the number of deposition layers in the above formula (10). When C≤2, the moving speed v of the electromagnetic induction heating coil is r satisfy: When 3≤C≤4, the moving speed v of the electromagnetic induction heating coil r satisfy: When C≥5, the moving speed v of the electromagnetic induction heating coil r satisfy:
[0140] When the component is heat treated by in-situ self-heating effect, the thickness of the reaction diffusion layer is related to the electromagnetic induction heating time and heating temperature. As the temperature rises, the component Gibbs free energy G gradually increases; the relationship between the atomic diffusion distance and the diffusion activation energy can be known from the Arrhenius equation (6). When the Gibbs free energy G exceeds the energy barrier required for atomic movement (i.e., the diffusion activation energy), the Ti and Al atoms break away from the constraints between atoms, causing the atoms in the Ti and Al deposition layers to react and diffuse with each other, so as to achieve the purpose of expanding the TiAl intermetallic compound phase region. The relationship between the diffusion reaction layer thickness and the diffusion time is parabolic:
[0141]
[0142] x 2 = k′1τ k
[0143]
[0144] In the above formula, x is the thickness of the diffusion layer; k is a constant related to material properties; D is the diffusion coefficient; τ k is the diffusion time; k′1 is the diffusion layer growth coefficient; K is a constant; Q is the diffusion activation energy; R is the gas constant; T m It is the temperature of the deposited body consisting of N deposited layers after being heated by the induction heating coil.
[0145] Because the TiAl intermetallic compound is wrapped by Ti and Al materials with excellent plasticity, the internal stress and deformation of the TiAl intermetallic compound under the heat of the LDED forming cycle are absorbed by the Ti and Al materials, thereby inhibiting the internal stress and deformation of the TiAl intermetallic compound from being absorbed by the Ti and Al materials, thereby inhibiting the formation of cracks in the TiAl intermetallic compound. Subsequently, the in-situ thermal effect is used to drive the interlayer Ti and Al elements to diffuse and react to form TiAl intermetallic compounds, thereby forming a homogenized TiAl intermetallic compound component.
Claims
1. A device for in-situ self-heating effect assisted 3D printing of TiAl complex metal components, comprising an LDED forming device; the LDED forming device comprises an LDED control device, a printing platform and a laser printing deposition head, and the laser printing deposition head, under the control of the LDED control device, can deposit on the printing platform according to a printing path preset in the LDED control device to form a deposited body, the deposited body comprising alternately stacked Ti deposited layers, Al deposited layers and an interface layer between the Ti deposited layers and the Al deposited layers, characterized in that: It also includes an arc induction heating device; the arc induction heating device includes a lifting mechanism, an arc induction coil and an induction relay; The arc induction coil is arranged outside the outline of the deposition body, and the arc induction coil is connected to the power supply after being connected in series with the induction relay, and the arc induction coil is connected to the power output end of the lifting mechanism. The lifting mechanism can drive the arc induction coil to rise and fall relative to the printing platform under the control of the LDED control device; After each N deposition layers are deposited on the deposition body, the portion with a height H among the deposited N deposition layers is induction heated synchronously by controlling the lifting mechanism; wherein: ; Where: represents the total height of N sedimentary layers, N ≥ 1; n Indicates the size parameter of the heat affected zone; The arc induction coil is a spiral heating coil; the spiral heating coil includes several layers of heating coils, and an induction relay is installed on each layer of heating coils; Each layer of heating coils corresponds to a deposition layer of the deposition body; The LDED control device can dynamically open or close the corresponding induction relay on the spiral heating coil according to the deposition speed of each deposition layer in the deposition body; The moving speed of the spiral heating coil satisfy: ; In the above formula, Indicates the number of layers in the sediment body where the sediment layer that needs induction heat treatment is located; , , They represent the velocity proportional coefficients under different ranges of sedimentary layer numbers, is the thickness of the sedimentary layer; It indicates the induction heating time required for a deposited body consisting of N deposited layers.
2. The device for in-situ self-heating effect assisted 3D printing of TiAl complex metal components according to claim 1, characterized in that: The number of heating coil turns required for a deposit consisting of N deposited layers for: ; Where: It represents the ampere-turn per unit length of the heating coil. It represents the height of the portion to be inductively heated in the deposit body consisting of N deposit layers; Indicates the current of the heating coil.
3. The device for in-situ self-heating effect assisted 3D printing of TiAl complex metal components according to claim 2, characterized in that: Heating coil current for: ; Electrical power of induction heating coil : ; The induction heat required for the deposit composed of N layers Q : ; Where: Indicates the potential amplitude of the power supply; Indicates the electrical power factor; It represents thermal efficiency; It represents the induction heating time required for a deposit consisting of N deposit layers; It represents the mass of a sedimentary body consisting of N sedimentary layers; represents the specific heat capacity of the sediment; It indicates the temperature of the deposited body consisting of N deposited layers after being heated by the induction heating coil; Indicates the ambient temperature.
4. The device for in-situ self-heating effect assisted 3D printing of TiAl complex metal components according to claim 3, characterized in that: The temperature of the deposit composed of N layers after being heated by the induction heating coil satisfy: ; ; ; Where: It represents the height of the portion to be inductively heated in the deposit body consisting of N deposit layers; k is a constant related to material properties; D is the diffusion coefficient; is the diffusion time; is the diffusion layer growth coefficient; K is a constant; is the diffusion activation energy; R is the gas constant; T m It is the temperature of the deposited body consisting of N deposited layers after being heated by the induction heating coil.
5. The device for in-situ self-heating effect assisted 3D printing of TiAl complex metal components according to claim 1, characterized in that: The LDED control device can adjust the laser power P , laser scanning rate v 1 and cooling rate v 2 to control.
6. A method for in-situ self-heating effect assisted 3D printing of TiAl complex metal components, which is realized based on the device for in-situ self-heating effect assisted 3D printing of TiAl complex metal components according to claim 1, characterized in that: The steps include: Step 1: Use LDED forming process to print a deposited body with a preset thickness: Based on LDED forming equipment, the LDED forming process is adopted to alternately print Ti and Al metal powders according to a preset printing path to obtain a deposited body with a preset thickness; The deposited body comprises a stacked Ti deposited layer, an Al deposited layer and an interface layer at the interface of the Ti deposited layer and the Al deposited layer; During the printing process of the deposited body, by adjusting the process parameters of the LDED forming process, a TiAl intermetallic compound wrapped between the Ti deposited layer and the Al deposited layer is formed in the interface layer to inhibit the TiAl intermetallic compound from forming cracks; Step 2: In-situ thermal post-treatment process promotes the formation of TiAl intermetallic compounds in the interface layer of the deposit: Based on arc induction heating equipment, an in-situ thermal post-treatment process is used to perform induction heat treatment on the deposited body obtained in step one, so as to drive the metal Ti atoms of the Ti deposition layer to break free from their constraints and diffuse toward the interface layer, and the metal Al atoms of the Al deposition layer to break free from their constraints and diffuse toward the interface layer, thereby inducing the TiAl intermetallic compound formed in the interface layer to gradually grow, so as to promote the formation of the TiAl intermetallic compound, and make the TiAl intermetallic compound between the Ti deposition layer and the Al deposition layer uniform.
Citation Information
Patent Citations
Layered manufacturing of single crystal alloy components
CN105705278A
Electromagnetic induction heating assisted titanium matrix composite laser additive manufacturing device and method
CN109663917A
Eddy current sensor array for additive manufacturing and eddy current sensor system
CN111189907A
3D printing part temperature gradient control device and method
CN112024874A
Synchronous heating stress deformation control system and method for robot electric arc additive shaft part