Wavelength conversion material and manufacturing method thereof, wavelength conversion device and projection device

By adding fluorine ions and fluorine-containing compounds to the wavelength conversion material, the problem that the fluorescent color wheel is prone to deterioration at high temperatures is solved, the fluorescence conversion efficiency and sintering temperature are improved, and good optical quality is achieved.

CN114806577BActive Publication Date: 2024-10-29CORETRONIC CORPORATION
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202110088378.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-01-22
Publication Date
2024-10-29
Estimated Expiration
2041-01-22

AI Technical Summary

Technical Problem

Existing fluorescent color wheels are prone to deterioration at high temperatures, with low luminous efficiency and low reliability. In addition, the sintering temperature of the phosphor powder in the manufacturing process is high and the operability is poor.

Method used

Fluorine-containing wavelength conversion materials are used to replace oxygen ions in the crystal lattice or fill oxygen vacancies by adding fluorine ions to reduce lattice defects, improve fluorescence conversion efficiency, and reduce the sintering temperature by adding fluorine-containing compounds.

Benefits of technology

The fluorescence conversion efficiency is improved, the sintering temperature is reduced, the fluorescence conversion efficiency of the wavelength conversion device is enhanced, and the optical quality of the projection device is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114806577B_ABST
    Figure CN114806577B_ABST
Patent Text Reader

Abstract

The present invention provides a wavelength conversion material and a manufacturing method thereof, a wavelength conversion device and a projection device, wherein the wavelength conversion material has good fluorescence conversion efficiency. The wavelength conversion material includes a first phase, wherein the composition of the first phase is M3Al5(O 1‑ 0.5x F x ) 12 :Ce 3+ , wherein M is at least one selected from the group consisting of yttrium (Y), lutetium (Lu), gadolinium (Gd), terbium (Tb), praseodymium (Pr) and neodymium (Nd), and 0.012≦x≦0.3. The wavelength conversion material provided by the present invention has good fluorescence conversion efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a material and a manufacturing method thereof and an optical device, and in particular to a wavelength conversion material and a manufacturing method thereof, a wavelength conversion device and a projection device. Background Art

[0002] In recent years, projection devices based on solid-state light sources such as light-emitting diodes (LEDs) and laser diodes have gradually gained a foothold in the market. Since laser diodes have a luminous efficiency of more than 20%, in order to break through the light source limitation of LEDs, laser light sources have gradually been developed to excite phosphors to produce the pure color light source required for projectors.

[0003] Generally speaking, the manufacturing process of the existing fluorescent color wheel is to coat the fluorescent powder mixed with silicone on the substrate of the fluorescent color wheel. However, silicone has the characteristics of not being able to withstand high temperatures and low thermal conductivity. Therefore, when the laser excites the fluorescent color wheel for a long time, the silicone cannot withstand high temperatures and is easily degraded or burned, which will affect the luminous efficiency and reliability of this fluorescent color wheel. On the other hand, there is another process for the fluorescent color wheel that replaces silicone with phosphor by glass glue. The fluorescent color wheel formed by this process has better thermal conductivity and light transmittance. However, there are oxygen lattice defects in general phosphors, so the fluorescence conversion efficiency of the phosphors is still insufficient and the sintering temperature required in the process of the phosphors is relatively high, and the operability is poor.

[0004] U.S. Patent No. 9738828 states that the fluorescent ceramic composition is Y3Al5O 12 :Ce、Lu3(Ga,Al)5O 12 :Ce, Mg3Al8[SiO]3:Ce, the fluorescent ceramic has a grain boundary that causes the diffusion of fluorescence; the composition of the main phase is recorded in U.S. Patent No. 9952491 as Ce: Y3Al5O 12 The composition of the second phase is Ce: YAlO3, CeO2, Y2O3 or Ce: Y2O3; Patent No. 104177078 of the People's Republic of China records MgAl2O4 / (Ce x Lu y Y 1-x-y )3Al5O 12 , where the ranges of x and y are: 0.013≦x≦0.015, 0.016≦y≦0.018); Patent No. 104177079 of the People's Republic of China records that MgAl2O4 / (Ce x Sr y Y 1-x-y )3Al5O 12, where the value ranges of x and y are: 0.001≦x≦0.03, 0.001≦y≦0.03).

[0005] The "background technology" section is only used to help understand the content of the present invention. Therefore, the content disclosed in the "background technology" section may contain some known technologies that are not known to those skilled in the art. The content disclosed in the "background technology" section does not mean that the content or the problems to be solved by one or more embodiments of the present invention have been known or recognized by those skilled in the art before the application of the present invention. Summary of the invention

[0006] The invention provides a wavelength conversion material with good fluorescence conversion efficiency.

[0007] The invention provides a method for manufacturing a wavelength conversion material, which can provide a wavelength conversion material with good fluorescence conversion efficiency and can reduce the sintering temperature in the sintering step and has good operability.

[0008] The invention provides a wavelength conversion device with good fluorescence conversion efficiency.

[0009] The invention provides a projection device with good optical quality.

[0010] Other purposes and advantages of the present invention can be further understood from the technical features disclosed in the present invention.

[0011] To achieve one or part or all of the above purposes or other purposes, one embodiment of the present invention provides a wavelength conversion material. The wavelength conversion material includes: a first phase, whose composition is M3Al5(O 1-0.5x F x ) 12 :Ce 3+ , wherein M is at least one selected from the group consisting of yttrium (Y), lutetium (Lu), gadolinium (Gd), terbium (Tb), praseodymium (Pr) and neodymium (Nd), and 0.012≦x≦0.3.

[0012] To achieve one or part or all of the above purposes or other purposes, one embodiment of the present invention provides a method for manufacturing a wavelength conversion material. The method for manufacturing a wavelength conversion material includes: sintering a precursor composition, wherein the precursor composition includes a first metal oxide, a second metal oxide, a fluorine-containing compound, and a cerium-containing compound. The first metal oxide is at least one selected from the group consisting of yttrium oxide, lutetium oxide, gadolinium oxide, terbium oxide, praseodymium oxide, and neodymium oxide. The second metal oxide includes aluminum oxide.

[0013] To achieve one or part or all of the above purposes or other purposes, one embodiment of the present invention provides a wavelength conversion device. The wavelength conversion device includes: a substrate; and at least one wavelength conversion layer. The at least one wavelength conversion layer is located on the substrate, and the at least one wavelength conversion layer includes the above-mentioned wavelength conversion material.

[0014] In order to achieve one or part or all of the above purposes or other purposes, one embodiment of the present invention proposes a projection device. The projection device includes: the above-mentioned wavelength conversion device, an excitation light source, a light valve and a projection lens. The wavelength conversion device has at least one wavelength conversion optical zone, and at least one wavelength conversion layer is arranged corresponding to the at least one wavelength conversion optical zone. The excitation light source is used to emit an excitation light beam, wherein the excitation light beam is transmitted to the wavelength conversion device and converted into a conversion light beam by the wavelength conversion device. The light valve is located on the transmission path of the conversion light beam and is used to convert the conversion light beam into an image light beam. The projection lens is located on the transmission path of the image light beam and is used to convert the image light beam into a projection light beam.

[0015] Based on the above, the embodiments of the present invention have at least one of the following advantages or effects. In the embodiments of the present invention, the wavelength conversion material replaces oxygen ions in the lattice or fills oxygen vacancies by adding fluorine to reduce lattice defects and increase fluorescence conversion efficiency. In addition, the manufacturing method of the wavelength conversion material of the embodiments of the present invention can also reduce the sintering temperature in the sintering step by adding fluorine-containing compounds. In addition, the wavelength conversion device using the above wavelength conversion material has good fluorescence conversion efficiency, and the projection device using the above wavelength conversion material has good optical quality.

[0016] In order to make the above features and advantages of the present invention more clearly understood, embodiments are given below with reference to the accompanying drawings for detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1A It is a cross-sectional schematic diagram of a wavelength conversion device according to an embodiment of the present invention.

[0018] Figure 1B yes Figure 1A A top view of a wavelength conversion device.

[0019] Figure 2A The present invention is a flowchart of a process for isostatic pressing of a wavelength conversion material according to an embodiment of the present invention.

[0020] Figure 2B The figure is a flow chart of a hot pressing sintering process of a wavelength conversion material according to another embodiment of the present invention.

[0021] Figure 3 It is a schematic diagram of the structure of a projection device according to an embodiment of the present invention.

[0022] Figure 4A This is a photograph of the appearance of the wavelength conversion material of Experimental Example 1.

[0023] Figure 4B This is a photograph of the appearance of the wavelength conversion material of Comparative Example 1.

[0024] Figure 5A This is a scanning electron microscope (SEM) image of the surface morphology of the wavelength conversion material of Experimental Example 1.

[0025] Figure 5B This is a SEM image of the surface morphology of the wavelength conversion material of Comparative Example 1.

[0026] Fig. 6A yes Figure 5A Energy dispersive X-ray spectrum of the sampling point M1 in .

[0027] Figure 6B yes Figure 5A Energy dispersive X-ray spectrum of the sampling point M2 in .

[0028] Figure 7 3 is a comparison chart of the fluorescence conversion efficiency and quantum efficiency (QE) of the wavelength conversion materials of Experimental Example 1 and Comparative Example 1. DETAILED DESCRIPTION

[0029] The above-mentioned other technical contents, features and effects of the present invention will be clearly presented in the following detailed description of a preferred embodiment with reference to the accompanying drawings. The directional terms mentioned in the following embodiments, such as up, down, left, right, front or back, etc., are only the directions with reference to the accompanying drawings. Therefore, the directional terms used are used to illustrate and not to limit the present invention.

[0030] Figure 1A It is a cross-sectional schematic diagram of a wavelength conversion device according to an embodiment of the present invention. Figure 1B yes Figure 1A A top view of a wavelength conversion device. Figure 1A and Figure 1B The wavelength conversion device 100 of the present embodiment has at least one wavelength conversion optical region WR and a light passing region TR, and the wavelength conversion device 100 includes a substrate 110 and at least one wavelength conversion layer 10. Specifically, Figure 1A As shown, in this embodiment, at least one wavelength conversion layer 10 is located on the substrate 110 and is disposed corresponding to at least one wavelength conversion optical region WR. Figure 1A As shown, in this embodiment, the wavelength conversion layer 10 includes a wavelength conversion material WM, and is correspondingly disposed on the wavelength conversion region WR.

[0031] In one embodiment, the wavelength conversion layer 10 includes a plurality of wavelength conversion regions WR, and a plurality of wavelength conversion materials are disposed on the plurality of wavelength conversion regions WR, which can be used to convert the excitation beam into a plurality of conversion beams, and the plurality of conversion beams are, for example, green, red, and yellow, respectively.

[0032] In this embodiment, the wavelength conversion material WM includes: a first phase, wherein the composition of the first phase is M3Al5(O 1-0.5x F x ) 12 :Ce 3+ , wherein M is at least one selected from the group consisting of yttrium (Y), lutetium (Lu), gadolinium (Gd), terbium (Tb), praseodymium (Pr) and neodymium (Nd), and 0.012≦x≦0.3.

[0033] Generally speaking, the sintering step of forming the wavelength conversion material WM often uses a reducing atmosphere, mainly to maintain the valence of the fluorescent activation element Ce at trivalent (Ce 3+ ), so it is easy to form oxygen vacancies (Oxygen Vacancies) defects in the reduction process, affecting the fluorescence conversion efficiency. In this embodiment, the first phase of the wavelength conversion material WM contains fluorine (i.e., fluorine ions), wherein the ion radius of the fluorine ions is 0.133nm, which is close to the oxygen ion radius of 0.140nm. Therefore, the fluorine ions can easily replace the oxygen ions in the lattice or fill the oxygen vacancies to reduce the lattice defects and increase the fluorescence conversion efficiency. In this way, the fluorine-containing wavelength conversion material WM can enable the wavelength conversion device 100 to have good fluorescence conversion efficiency.

[0034] More specifically, in one embodiment, the fluorine-containing wavelength conversion material WM can improve the fluorescence conversion efficiency by more than 5%. In another embodiment, the fluorine-containing wavelength conversion material WM can improve the fluorescence conversion efficiency by more than 7%.

[0035] In one embodiment, the wavelength conversion material WM may further include a second phase, which is mainly composed of aluminum oxide and may also include MgAl2O4, ZnAl2O4, Al6Si2O 13 , NaAlO2, or a combination thereof. MgAl2O4, ZnAl2O4, Al6Si2O 13 、NaAlO2 as the second phase can increase the thermal conductivity of the wavelength conversion material WM itself to improve the fluorescence conversion efficiency. MgAl2O4、ZnAl2O4、Al6Si2O 13, NaAlO2 are components derived from the sintering of magnesium oxide, zinc oxide, silicon oxide, and sodium oxide with aluminum oxide, respectively. Magnesium oxide, zinc oxide, silicon oxide, and sodium oxide can be used as sintering aids to reduce the sintering temperature in the process. By including Al2O3 as the second phase, the wavelength conversion material WM can increase the thermal conductivity of the wavelength conversion material WM itself to improve the fluorescence conversion efficiency.

[0036] In one embodiment, based on 100 wt % (weight percentage) of the wavelength conversion material WM, the second phase is greater than 0 wt % and less than 30 wt %.

[0037] In another embodiment, the wavelength conversion layer 10 may further include a bonding material. The material of the bonding material is not particularly limited and can be selected accordingly according to the process or product requirements. The material of the bonding material includes glass glue, silicone, or a combination thereof. When the material of the bonding material is glass glue, the thermal conductivity and light transmittance of the wavelength conversion layer 10 can be improved.

[0038] The wavelength conversion material WM is uniformly dispersed in the bonding material to form a wavelength conversion layer 10 .

[0039] The following will be Figure 2A and Figure 2B The method for manufacturing the wavelength conversion material WM is described below. The method for manufacturing the wavelength conversion material WM is not particularly limited, for example, the precursor composition is subjected to an isostatic pressing process or a hot-press sintering process.

[0040] Figure 2A The present invention is a flowchart of a process for isostatic pressing of a wavelength conversion material according to an embodiment of the present invention.

[0041] First, step S101 is performed to mix the components contained in the precursor composition. The mixing method is not particularly limited, for example, the components contained in the precursor composition are uniformly mixed by physical mixing.

[0042] The precursor composition includes a first metal oxide, a second metal oxide, a fluorine-containing compound and a cerium-containing compound.

[0043] Specifically, in one embodiment, the first metal oxide is at least one selected from the group consisting of yttrium oxide (Y2O3), lutetium oxide (Lu2O3), gadolinium oxide (Gd2O3), terbium oxide (Tb2O3), praseodymium oxide (Pr2O3) and neodymium oxide (Nd2O3).

[0044] In one embodiment, based on 100 wt % of the precursor composition, the first metal oxide is 35 wt % to 55 wt %.

[0045] In one embodiment, the second metal oxide includes aluminum oxide, which can cause the wavelength conversion material WM to produce a second phase of Al2O3, thereby increasing the thermal conductivity of the wavelength conversion material WM itself, thereby improving the fluorescence conversion efficiency.

[0046] The reaction formula of the first metal oxide and the second metal oxide is described below. When the first metal oxide is yttrium oxide (Y2O3) and the second metal oxide is aluminum oxide (Al2O3), the following three reaction formulas may be included according to the increase in the sintering temperature described later:

[0047] Reaction equation 1: 2Y2O3+Al2O3→Y4Al2O9 (at 900-1000℃).

[0048] Reaction equation 2: Y4Al2O9+Al2O3→4YAlO3 (at 1100~1250℃).

[0049] Reaction 3: 3YAlO3+Al2O3→Y3Al5O 12 (at 1400~1800℃).

[0050] Furthermore, when the precursor composition includes a fluorine-containing compound and a cerium-containing compound, the fluorine-containing compound and the cerium-containing compound can replace the first metal oxide and the second metal oxide to participate in the reaction. Specifically, the fluorine atom in the fluorine-containing compound can replace the oxygen atom, and the cerium atom in the cerium-containing compound can react as a doping atom.

[0051] In another embodiment, the second metal oxide includes not only aluminum oxide, but also magnesium oxide, zinc oxide, silicon oxide and sodium oxide, or a combination thereof, wherein magnesium oxide, zinc oxide, silicon oxide and sodium oxide can be used as sintering aids to reduce the sintering temperature in the process. By including the second metal oxide, the precursor composition can further generate MgAl2O4, ZnAl2O4, Al6Si2O4 in the second phase. 13 , NaAlO2, to increase the thermal conductivity of the wavelength conversion material WM itself, so as to improve the fluorescence conversion efficiency.

[0052] In one embodiment, based on 100 wt % of the precursor composition, the second metal oxide is greater than 40 wt % and less than 60 wt %.

[0053] In one embodiment, the fluorine-containing compound is an alkali metal fluoride, an alkaline earth fluoride, or a combination thereof. In another embodiment, the fluorine-containing compound may be sodium fluoride (NaF), magnesium fluoride (MgF2), or a combination thereof. It is worth noting that the present embodiment can reduce the sintering temperature in the subsequent sintering step by adding the fluorine-containing compound to the precursor composition, thereby improving operability. For example, the sintering temperature in the subsequent sintering step is reduced from above 1800°C to about 1700°C, so that the precursor composition can achieve the effect of liquid phase sintering at 1700°C. In more detail, the melting point of alkali metal fluorides such as sodium fluoride (NaF) is 993°C, and the melting point of alkaline earth fluorides such as magnesium fluoride (MgF2) is 1260°C, which is much lower than the melting point of yttrium aluminum garnet (yttriumaluminium garnet, YAG) (1950°C), so the added alkali metal fluorides and alkaline earth fluorides can be used as sintering aids in the subsequent sintering steps to reduce the sintering temperature. In one embodiment, the fluorine-containing compound is 0.5% to 10% by weight (weight percentage is 0.5% to 10%) based on 100% by weight of the precursor composition.

[0054] In one embodiment, the cerium-containing compound is cerium oxide (CeO2), cerium fluoride (CeF3), or a combination thereof. When the cerium-containing compound is cerium fluoride, cerium fluoride can be used as both a cerium-containing compound and a fluorine-containing compound, and can simultaneously play the role of cerium doping and sintering aid. In this way, the materials included in the precursor composition can be simplified.

[0055] In one embodiment, based on 100 wt % of the precursor composition, the cerium-containing compound is in an amount of 0.3 wt % to 5 wt %.

[0056] Next, step S102 is performed to wet-grind the precursor composition so that the precursor composition forms particles with a particle size of less than 1 micron. There is no particular limitation on the method of the wet-grinding step, for example, the precursor composition mixed solvent is ground by mechanical grinding. Specifically, for example, aluminum oxide or zirconium oxide grinding ceramic balls are placed in a ball mill jar with the precursor composition and solvent, and ground and mixed with a ball mill. There is no particular limitation on the solvent, as long as it does not react with the precursor composition. The solvent is, for example, an alcohol solvent such as methanol, ethanol, isopropanol, etc.

[0057] Then, step S103 is performed to dry the precursor composition. There is no particular limitation on the method of the drying step, and for example, the precursor composition is placed in an oven for drying. There is no particular limitation on the drying temperature and time, as long as the solvent used in the wet grinding step can be volatilized. The drying temperature is, for example, 60 to 80° C. The drying time is, for example, 8 to 16 hours.

[0058] Next, step S104 is performed to screen the precursor composition. The particle size of the precursor composition after screening is, for example, less than 300 meshes.

[0059] Then, step S105 is performed to dry-press the precursor composition to form a block. The dry-pressing step is not particularly limited as long as the precursor composition can be formed into a block.

[0060] Next, step S106 is performed to perform a cold isostatic pressing step on the block of the precursor composition. There is no particular limitation on the method of the cold isostatic pressing (CIP) step, as long as the shape of the block can be fixed. The pressure of the cold isostatic pressing step can be above 200 MPa.

[0061] Finally, step S107 is performed to perform a vacuum sintering step on the block of the precursor composition. Here, the vacuum sintering step refers to a sintering step performed under a vacuum environment. There is no particular limitation on the method of the vacuum sintering step, as long as the precursor composition can be formed into the target wavelength conversion material. There is no particular limitation on the temperature of the vacuum sintering step, for example, it is greater than 1700°C. There is no particular limitation on the time of the vacuum sintering step, for example, 2 hours to 48 hours.

[0062] Figure 2B This is a flow chart of a hot pressing sintering process of a wavelength conversion material according to another embodiment of the present invention. Figure 2B The hot pressing sintering process of the wavelength conversion material of this embodiment is similar to Figure 2A The isostatic pressing process shown is similar, and the main difference between the two is that in the hot pressing sintering process, after step S104, step S205 is executed to perform a pressure sintering step on the precursor composition. There is no special restriction on the method of the pressure sintering step, as long as the precursor composition can be formed into the target wavelength conversion material. There is no special restriction on the pressure of the pressure sintering step, for example, 150MPa to 300MPa. There is no special restriction on the temperature of the pressure sintering step, for example, it is greater than or equal to 1600°C. There is no special restriction on the time of the pressure sintering step, for example, 2 hours to 12 hours. The pressure sintering step is, for example, carried out in a reducing atmosphere, wherein the reducing gas is, for example, a mixture of hydrogen and argon or a mixture of hydrogen and nitrogen.

[0063] There is no particular limitation on the method of forming the wavelength conversion layer 10 with the wavelength conversion material WM, as long as the wavelength conversion material WM can be fixed on the substrate 110. For example, the wavelength conversion material WM can be mixed with a bonding material, and then the wavelength conversion material WM and the bonding material can be cured to fix the wavelength conversion material WM on the substrate 110. In this way, the aforementioned Figure 1AIn this embodiment, the wavelength conversion layer 10 is formed by using the wavelength conversion material WM containing fluorine ions, so that the wavelength conversion device 100 can have good fluorescence conversion efficiency.

[0064] Figure 3 Schematic diagram of a projection device according to an embodiment of the present invention. Figure 1A and Figure 3 The projection device 200 includes an excitation light source 210, a light splitting unit 220, a wavelength conversion device 100 including a wavelength conversion layer 10, a light valve 250, and a projection lens 260. In the present embodiment, the structures of the wavelength conversion layer 10 and the wavelength conversion device 100 have been described in detail above and are not described again here. In the present embodiment, the light valve 250 is, for example, a digital micro-mirror device (DMD) or a liquid-crystal-on-silicon panel (LCOS panel). However, in other embodiments, the light valve 250 may also be a transmissive liquid crystal panel or other beam modulators.

[0065] like Figure 3 As shown, in this embodiment, the excitation light source 210 is used to emit an excitation light beam 50. In this embodiment, the excitation light source 210 is a laser light source, and the excitation light beam 50 is a blue laser light beam. For example, the excitation light source 210 may include a plurality of blue laser diodes (not shown) arranged in an array, but the present invention is not limited thereto.

[0066] Specifically, if Figure 3 As shown, in the present embodiment, the spectroscopic unit 220 is arranged on the transmission path of the excitation light beam 50, and is located between the excitation light source 210 and the wavelength conversion device 100. Specifically, the spectroscopic unit 220 can be a partially transmissive and partially reflective element, a color separation element, a polarization spectroscopic element, or other various elements that can separate light beams. For example, in the present embodiment, the spectroscopic unit 220 can allow a blue light beam to pass through, and provide a reflection effect for light beams of other colors (such as red, green, yellow, etc.). In other words, the spectroscopic unit 220 allows the blue excitation light beam 50 to pass through, so that the excitation light beam 50 can pass through the spectroscopic unit 220 and be incident on the wavelength conversion device 100.

[0067] For example, Figure 1A , Figure 1B and Figure 3As shown, the wavelength conversion device 100 is located on the transmission path of the excitation light beam 50, and at least one wavelength conversion optical region WR of the wavelength conversion device 100 is used to convert the excitation light beam 50 into at least one conversion light beam 60, and the light passing region TR of the wavelength conversion device 100 is used to allow the excitation light beam 50 to pass through and be transmitted to the subsequent optical element. In addition, the wavelength conversion device 100 further includes a first actuator MR1, which is used to allow the light passing region TR and at least one wavelength conversion optical region WR to enter the irradiation range of the excitation light beam 50 at different times, and selectively allow the excitation light beam 50 to pass through or be converted into at least one conversion light beam 60.

[0068] For example, Figure 3 As shown, the projection device 200 further includes a filter module 230, which is located on the transmission path of the excitation light beam 50 and the conversion light beam 60, and has a filter optical area (not shown) and a light-transmitting area (not shown). The filter module 230 further includes a second actuator MR2, which is used to make the filter optical area (not shown) correspondingly enter the irradiation range of the conversion light beam 60 at different times to form red light and green light respectively. On the other hand, the light-transmitting area (not shown) will also correspondingly enter the irradiation range of the excitation light beam 50 transmitted to the filter module 230 at different times to form blue light. In this way, the excitation light beam 50 and the conversion light beam 60 can be converted into illumination light beams 70 with multiple different colors in a timely manner.

[0069] On the other hand, Figure 3 As shown, in this embodiment, the projection device 200 further includes a light homogenizing element 240, which is located on the transmission path of the illumination light beam 70. In this embodiment, the light homogenizing element 240 includes an integrating rod, but the present invention is not limited thereto. Figure 3 As shown, when the illumination light beam 70 is transmitted to the light homogenizing element 240 via the illumination system, the light homogenizing element 240 may homogenize the illumination light beam 70 and transmit the light beam 70 to the light valve 250 .

[0070] Then, if Figure 3 As shown, the light valve 250 is located on the transmission path of the illumination light beam 70 and is used to convert the illumination light beam 70 into an image light beam 80. The projection lens 260 is located on the transmission path of the image light beam 80 to project the image light beam 80 onto a screen (not shown) to form a projection light beam 90 constituting an image frame. Since the illumination light beam 70 is converged on the light valve 250, the light valve 250 sequentially converts the illumination light beam 70 into image light beams 80 of different colors and transmits them to the projection lens 260. Therefore, the image frame projected by the image light beam 80 converted by the light valve 250 can become a color frame.

[0071] As a result, the projection device 200 can have good optical quality by using the wavelength conversion device 100 with good fluorescence conversion efficiency.

[0072] The following will give experimental examples of wavelength conversion materials. However, the experimental examples listed below are not intended to limit the present invention, and any person skilled in the art may make appropriate changes to the parameters or settings after referring to the present invention, but they should still fall within the scope of the present invention.

[0073] Experimental Example 1

[0074] First, a precursor composition including 48 grams of yttrium oxide (Y2O3), 1 gram of sodium fluoride (NaF), 52 grams of aluminum oxide (Al2O3) and 0.5 grams of cerium oxide (CeO2) is placed in a ball mill and 200 grams of ethanol solvent and aluminum oxide or zirconium oxide grinding ceramic balls are added, and then the ball mill is placed in a ball mill for grinding and mixing. Then, the precursor composition mixed with the solvent after grinding and mixing is poured out and the grinding ceramic balls are sieved out to a beaker or a drying container. Then, the beaker or drying container is transferred to a 60-80°C oven for drying for 12 hours. Then, the powder of the dried precursor composition is sieved with a 300 mesh screen, and the precursor composition is dry-pressed with a mold to obtain a block. Then, it is formed by cold isostatic pressing (CIP) at a pressure of 200MPa to make the block stack more compact. Finally, the block is placed in a vacuum sintering furnace and sintered at a sintering temperature of 1700° C. for 10 hours to obtain the wavelength conversion material of Experimental Example 1.

[0075] Comparative Example 1

[0076] The wavelength conversion material of Comparative Example 1 is prepared by the same steps as those of Experimental Example 1, except that the components of the precursor composition and the sintering temperature are changed (as shown in Table 1).

[0077] [Table 1]

[0078]

[0079]

[0080] Figure 4A and Figure 4B The following are photos of the appearance of the wavelength conversion materials of Experimental Example 1 and Comparative Example 1 taken through a low-magnification microscope. Figure 4A and Figure 4BIt can be seen that the wavelength conversion materials of Experimental Example 1 and Comparative Example 1 are both yellow fluorescent ceramics. The yellow fluorescent ceramics of Experimental Example 1 present a bright yellow glass-like color, indicating good sintering density and uniformity. Some areas of the yellow fluorescent ceramics of Comparative Example 1 present a bright yellow glass-like color, but most areas present a beige color with many pores, indicating poor sintering density and uniformity of the ceramics.

[0081] Figure 5A and Figure 5B The following are scanning electron microscope (SEM) images of the surface morphology of the wavelength conversion materials of Experimental Example 1 and Comparative Example 1, respectively. Figure 5A and Figure 5B In the graph, the light-colored area is the first phase P1, and the dark-colored area is the second phase P2. As shown in Table 1, the first phase P1 of Experimental Example 1 is Y3Al5(O 1-0.5x F x ) 12 :Ce 3+ (where x = 0.05), the second phase P2 is aluminum oxide; the first phase P1 of Comparative Example 1 is Y3Al5O 12 :Ce 3+ , the second phase P2 is aluminum oxide.

[0082] In addition, the energy dispersive X-ray detector (EDX) attached to the SEM can be used to detect Figure 5A Component analysis is performed on the sampling points M1 and M2 in the graph, wherein the sampling point M1 corresponds to the first phase P1 and the sampling point M2 corresponds to the second phase P2. Fig. 6A and Figure 6B They are Figure 5A The energy dispersive X-ray spectra of the sampling points M1 and M2 in Fig. 6A and Figure 6B It can be further confirmed that the first phase P1 of Experimental Example 1 is Y3Al5(O 1-0.5x F x ) 12 :Ce 3+ (where x=0.05), the second phase P2 is aluminum oxide.

[0083] Then, the wavelength conversion materials of Experimental Example 1 and Comparative Example 1 are directly placed in a projector system for measurement, and the fluorescence conversion efficiency and quantum efficiency (QE) gain of the wavelength conversion materials of Experimental Example 1 and Comparative Example 1 are analyzed. Figure 7 : is a comparison chart of the fluorescence conversion efficiency and quantum efficiency gain of the wavelength conversion materials of Experimental Example 1 and Comparative Example 1. Figure 7It can be seen that the fluorescence conversion efficiency and quantum efficiency of the wavelength conversion material of Experimental Example 1 are both higher than those of Comparative Example 1. Therefore, it can be seen that the fluorine-containing wavelength conversion material of Experimental Example 1 can improve the fluorescence conversion efficiency and increase the quantum efficiency.

[0084] In summary, the embodiments of the present invention have at least one of the following advantages or effects. In the embodiments of the present invention, the wavelength conversion material reduces lattice defects and increases fluorescence conversion efficiency by adding fluorine to replace oxygen ions in the lattice or fill oxygen vacancies. In addition, the manufacturing method of the wavelength conversion material of the embodiments of the present invention can also reduce the sintering temperature in the sintering step by adding fluorine-containing compounds. In addition, the wavelength conversion device using the above-mentioned wavelength conversion material has good fluorescence conversion efficiency, and the projection device using the above-mentioned wavelength conversion material has good optical quality.

[0085] However, the above is only the preferred embodiment of the present invention, and it cannot be used to limit the scope of the implementation of the present invention. That is, all simple equivalent changes and modifications made according to the claims and the content of the invention of the present invention are still within the scope of the patent of the present invention. In addition, any embodiment or claim of the present invention does not need to achieve all the purposes, advantages or features disclosed by the present invention. In addition, the abstract and the name of the invention are only used to assist in the retrieval of patent documents, and are not used to limit the scope of rights of the present invention. In addition, the terms "first", "second", etc. mentioned in this specification or claims are only used to name the name of the element or distinguish different embodiments or scopes, and are not used to limit the upper or lower limit of the number of elements.

[0086] Description of reference numerals:

[0087] 10: Wavelength conversion layer

[0088] 50: Excitation beam

[0089] 60: Convert beam

[0090] 70: Illumination beam

[0091] 80: Image beam

[0092] 90: Projection beam

[0093] 100: Wavelength conversion device

[0094] 110:Substrate

[0095] 200: Projection device

[0096] 210: Excitation light source

[0097] 220: Spectroscopic unit

[0098] 230: Filter module

[0099] 240: Light homogenization element

[0100] 250: Light valve

[0101] 260: Projection lens

[0102] P1: First phase

[0103] P2: Second phase

[0104] MR1: First actuator

[0105] MR2: Second actuator

[0106] S101, S102, S103, S104, S105, S106, S107, S205: Steps

[0107] TR: Light passing zone

[0108] WM: Wavelength conversion material

[0109] WR: Wavelength conversion optical region.

Claims

1. A wavelength conversion material, characterized in that: The wavelength conversion material comprises a first phase and a second phase, wherein: The composition of the first phase is M3Al5(O 1-0.5x F x ) 12 :Ce 3+ , wherein M is at least one selected from the group consisting of yttrium (Y), lutetium (Lu), gadolinium (Gd), terbium (Tb), praseodymium (Pr) and neodymium (Nd), 0.012≦x≦0.3; and The second phase includes Al2O3, and the second phase also includes MgAl2O4, ZnAl2O4, Al6Si2O 13 , NaAlO2, or a combination thereof, Wherein, based on 100 weight % of the wavelength conversion material, the second phase is greater than 0 weight % and less than 30 weight %.

2. A method for manufacturing a wavelength conversion material, characterized in that: include: performing a sintering step on the precursor composition to form the wavelength conversion material, The precursor composition includes a first metal oxide, a second metal oxide, a fluorine-containing compound and a cerium-containing compound. The first metal oxide is at least one selected from the group consisting of yttrium oxide, lutetium oxide, gadolinium oxide, terbium oxide, praseodymium oxide, and neodymium oxide. The second metal oxide includes aluminum oxide, magnesium oxide, zinc oxide, silicon oxide, sodium oxide, or a combination thereof. The wavelength conversion material includes a first phase and a second phase, and the composition of the first phase is M3Al5(O 1-0.5x F x ) 12 :Ce 3+ , wherein M is at least one selected from the group consisting of yttrium (Y), lutetium (Lu), gadolinium (Gd), terbium (Tb), praseodymium (Pr) and neodymium (Nd), 0.012≦x≦0.3, the second phase includes Al2O3, and the second phase also includes MgAl2O4, ZnAl2O4, Al6Si2O 13 , NaAlO2, or a combination thereof, wherein the second phase is greater than 0 wt% and less than 30 wt% based on 100 wt% of the wavelength conversion material.

3. The method for manufacturing a wavelength conversion material according to claim 2, characterized in that: Based on 100 wt % of the precursor composition, the fluorine-containing compound accounts for 0.5 wt % to 10 wt %.

4. The method for manufacturing a wavelength conversion material according to claim 2, characterized in that: Based on 100 weight % of the precursor composition, the second metal oxide accounts for more than 40 weight % and less than 60 weight %.

5. The method for manufacturing a wavelength conversion material according to claim 2, characterized in that: Before the sintering step, the method further comprises: Performing a wet grinding step on the precursor composition to form particles having a particle size of less than 1 micron; performing a drying step on the precursor composition; and The precursor composition is subjected to a screening step.

6. The method for manufacturing a wavelength conversion material according to claim 5, characterized in that: After the screening step, the method further comprises: performing a dry pressing step on the precursor composition to form a block; and The block formed by the precursor composition is subjected to a cold isostatic pressing step.

7. The method for manufacturing a wavelength conversion material according to claim 2, characterized in that: The sintering step is performed under a vacuum environment.

8. The method for manufacturing a wavelength conversion material according to claim 2, characterized in that: The sintering step is a pressure sintering step.

9. A wavelength conversion device, characterized in that: The wavelength conversion device comprises a substrate and at least one wavelength conversion layer, wherein: The at least one wavelength conversion layer is located on the substrate and comprises a wavelength conversion material, wherein the wavelength conversion material comprises a first phase and a second phase, wherein: The composition of the first phase is M3Al5(O 1-0.5x F x ) 12 :Ce 3+ , wherein M is at least one selected from the group consisting of yttrium (Y), lutetium (Lu), gadolinium (Gd), terbium (Tb), praseodymium (Pr) and neodymium (Nd), 0.012≦x≦0.3; and The second phase includes Al2O3, and the second phase also includes MgAl2O4, ZnAl2O4, Al6Si2O 13 , NaAlO2, or a combination thereof, Wherein, based on 100 weight % of the wavelength conversion material, the second phase is greater than 0 weight % and less than 30 weight %.

10. A projection device, characterized in that: The projection device comprises a wavelength conversion device, an excitation light source, a light valve and a projection lens, wherein: The wavelength conversion device has at least one wavelength conversion optical zone, and the wavelength conversion device includes a substrate and at least one wavelength conversion layer, wherein: The at least one wavelength conversion layer is located on the substrate and is disposed corresponding to the at least one wavelength conversion optical zone, wherein the at least one wavelength conversion layer comprises a wavelength conversion material, the wavelength conversion material comprises a first phase and a second phase, and the composition of the first phase is M3Al5(O 1-0.5x F x ) 12 :Ce 3+ , wherein M is at least one selected from the group consisting of yttrium (Y), lutetium (Lu), gadolinium (Gd), terbium (Tb), praseodymium (Pr) and neodymium (Nd), 0.012≦x≦0.3, the second phase includes Al2O3, and the second phase also includes MgAl2O4, ZnAl2O4, Al6Si2O 13 , NaAlO2, or a combination thereof, wherein the second phase is greater than 0 wt% and less than 30 wt% based on 100 wt% of the wavelength conversion material; The excitation light source is used to emit an excitation light beam, wherein the excitation light beam is transmitted to the wavelength conversion device and converted into a conversion light beam by the wavelength conversion device; The light valve is located on the transmission path of the converted light beam and is used to convert the converted light beam into an image light beam; and The projection lens is located on the transmission path of the image beam and is used for converting the image beam into a projection beam.

Citation Information

Patent Citations

  • Optical converter for high luminances

    US9738828B2

  • Phosphor, wavelength conversion element, light source device, and projector

    US9952491B2

  • YAG transparent ceramic for white light LED, and preparation method thereof

    CN102924072A

  • Wavelength conversion element, forming method thereof, wavelength conversion module and projection device

    CN110488560A