A method for evaluating the rough broken wire rate of steel cord wire rod
A method using carbon equivalent calculation, torsion, and bending tests addresses the challenge of evaluating cord steel wire rod breaking rates, ensuring consistent quality and reducing material waste by quantifying internal structure and plasticity.
Patent Information
- Application Number
- CN202210407911.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-19
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-04-19
AI Technical Summary
Current methods lack a specific and effective way to evaluate the rough breaking rate of cord steel wire rods, particularly the flush fracture type, which is the most frequent and impactful, leading to material waste, increased manual labor, and user dissatisfaction due to unpredictable breakage during mechanical descaling.
A method involving carbon equivalent calculation, unidirectional torsion tests, and repeated bending tests to determine the rough breaking parameters, using specific coefficients for different steel grades to quantify the rough breaking rate.
The method provides a reliable and simple means to predict the rough breaking rate, ensuring consistent quality and reducing user complaints by accurately assessing the wire rod's internal structure and plasticity before production, thereby improving material uniformity and reducing waste.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steelmaking, and in particular to a method for evaluating the rough broken wire rate of a cord steel wire rod. Background Art
[0002] Cord steel wire rod is the raw material for manufacturing tire radials, and the demand is high. Its downstream deep processing process includes many processes, among which the first process is mechanical descaling. The specific process is: the wire rod passes through the bending wheel and undergoes bending plastic deformation under the action of tension. The surface iron oxide scale is brittle and has a small elongation, so it cannot be deformed at the same time, so it is torn and finally detached from the surface of the wire rod. During the mechanical descaling process, the wire rod is subjected to alternating stress. In addition, there is friction between the wire rod and the bending wheel. The outer metal is mainly subjected to tensile stress, while the inner metal is subjected to compressive stress. Relatively speaking, the outer metal is more likely to fail and break. During the mechanical descaling process, the wire rod is not subjected to drawing deformation treatment (the diameter does not change), and the fracture that occurs in this process is called rough break. After the wire rod is roughly broken, manual welding is required, which will increase the risk of material breakage in the subsequent processing process, generate unnecessary manual labor, and cause some material waste. Users have clear requirements for the rough breaking rate of cord steel. The rough breaking rate of grade 70 cord steel should be less than 1.0 times / thousand tons, the rough breaking rate of grade 80 cord steel should be less than 3.0 times / thousand tons, and the rough breaking rate of grade 90 cord steel should be less than 5.0 times / thousand tons.
[0003] According to the type of rough-drawn fracture, the rough-drawn fracture types of cord steel wire rods can be divided into three categories: foreign body intrusion, necking and flush brittle fracture. Foreign body intrusion means that foreign matter is pressed into the surface of the wire rod, such as the cutting nodules that are not cleaned up at the end of the billet, the broken roller ring particles that are not cleaned up in the rolling line, etc., which destroy the integrity of the wire rod. The appearance of this type of fracture is that there are pits of varying depths on one side of the fracture. The necking fracture is mainly due to the fluctuation of the tension of the wire rod during the rolling process, the local diameter of the wire rod becomes thinner, and the force is the same during the drawing process, so it is directly pulled apart. The appearance of this type of fracture is that both ends of the fracture show a uniform diameter gradient. The appearance of the flush fracture is that the fracture section is flush and the diameter does not change. There are many reasons for the flush fracture, mainly including the surface quality and internal structural defects of the wire rod. The surface of the wire rod is scratched during the reverse transportation or the plasticity of the steel itself is poor, which will lead to rough pulling. The causes of pits and necking fractures are clear, and the control methods are clear. They can be effectively controlled by stabilizing the process and strengthening management. However, there are currently no specific and effective measures for the flush drawing fractures, which have the highest frequency and the greatest impact. However, through the analysis of relevant literature and a large number of organizational and performance test statistics, it is found that the main cause of the flush fracture has a corresponding relationship with the surface quality and internal microstructure of the wire rod.
[0004] The cord steel needs to be processed point by point during the mechanical descaling process. According to the weight of a single roll of φ5.5mm cord steel of 2.0 tons, the length of a single roll of cord steel exceeds 10,000 meters. Even for the 92-grade cord steel with the loosest rough breaking requirement (<5.0 times / 1,000 tons), the total length of 1,000 tons of 92-grade cord steel exceeds 5 million meters, and the number of rough breaking wires that occurs is less than 5.0 times, which is converted to: one million meters of cord steel will have a maximum of one break. Due to the lack of effective direct evaluation methods in the actual detection process, and rough breaking is a key material property that cord steel users are concerned about, it is very important to design an indirect evaluation method. Summary of the invention
[0005] The object of the present invention is to provide a simple and reliable method for evaluating the rate of broken wires of steel cords in view of the shortcomings of the prior art.
[0006] The technical solution adopted by the present invention is: a method for evaluating the rough broken wire rate of a cord steel wire rod, the method specifically comprising the following steps:
[0007] Step 1: Calculate the carbon equivalent of the cord steel wire rod and grade the wire rod.
[0008] Step 2: Perform multiple sets of unidirectional torsion tests on the wire rod to obtain the actual number of torsion turns of the wire rod.
[0009] Step 3: Resample the wire rod and conduct multiple sets of repeated bending tests to obtain the actual number of repeated bending times of the wire rod.
[0010] Step 4: Calculate the rough breaking parameters of the wire rod according to the wire rod classification, torsion test results and repeated bending test results, and evaluate the rough breaking rate of the wire rod according to the rough breaking parameters.
[0011] According to the above scheme, in step 4, the rough breaking parameter of the wire rod = (number of twisting circles × 5 + number of repeated bending times × 3.5) × steel type coefficient, and the steel type coefficients corresponding to grade 70, grade 80 and grade 90 steels are 1.0, 1.2 and 1.38.
[0012] According to the above scheme, in step four, when the rough breaking parameter of the cord steel wire rod is ≥125, the rough breaking rate of the wire rod is <1.0 times / kiloton; when the rough breaking parameter of the cord steel wire rod is 100-125, the rough breaking rate of the wire rod is 1.0-3.0 times / kiloton; when the rough breaking parameter of the cord steel wire rod is 75-100, the rough breaking rate of the wire rod is 3.0-5.0 / kiloton; when the rough breaking parameter of the cord steel wire rod is <75, the rough breaking rate of the wire rod is ≥5.0 times / kiloton.
[0013] According to the above scheme, in step one, the carbon equivalent of the cord steel wire rod is calculated according to the formula CE=C+Mn / 6, in which CE refers to the carbon equivalent of the material, C is the carbon content of the material, and Mn is the manganese content of the material.
[0014] According to the above scheme, in step one, the wire rod is graded according to the carbon equivalent: when CE < 0.81%, the wire rod is grade 70; when 0.81% ≤ CE < 0.91%, the wire rod is grade 80; when CE ≥ 0.91%, the wire rod is grade 90.
[0015] According to the above scheme, in step 2, the method of unidirectional torsion test of wire rod is as follows: one end of the wire rod is fixed by a chuck, and the other end is clamped by another chuck for unidirectional torsion, and a tensile force of 200N is applied; the distance between the two chucks is 200±10mm, and the torsion test speed is 30r / min; the external room temperature range of the test is required to be 15-35℃; the torsion test is carried out for at least 10 groups, and a torsion number is obtained for each group. After excluding invalid results, the average value is taken as the actual torsion number of the wire rod.
[0016] According to the above scheme, in step three, the method of repeated bending test is: the length of the wire rod sample is 150±10mm, the diameter of the elbow used in the test is 60mm, the test bending angle is ±90°, the test speed is 10 times / min, and the external room temperature range of the test is required to be 10-35℃; the repeated bending test is carried out for at least 5 groups, and a repeated bending number is obtained after each group of tests, and the average value is taken as the actual repeated bending number of the wire rod.
[0017] The beneficial effects of the present invention are as follows: under the premise of ensuring the surface quality and uniform size of the wire rod, the present invention comprehensively considers the steel grade, torsion and bending properties of the wire rod to quantify the relationship between the internal structure of the wire rod and the rough breaking rate, derives the rough breaking rate of the wire rod, and is verified through multiple rounds of batch tests. The inferred results are highly consistent with the actual application effects, and the application effects of the wire rod can be preliminarily understood before leaving the factory, which greatly reduces user complaints and is beneficial to the quality improvement of the wire rod. The method described in the present invention is simple and reliable. DETAILED DESCRIPTION
[0018] In order to better understand the present invention, the present invention is further described below in conjunction with specific embodiments.
[0019] A method for evaluating the rough broken wire rate of a cord steel wire rod, the method specifically comprising the following steps:
[0020] Step 1: Calculate the carbon equivalent of the cord steel wire rod and grade the wire rod.
[0021] According to the formula CE=C+Mn / 6, the carbon equivalent of the cord steel wire rod is calculated, and the wire rod is graded according to the carbon equivalent: if CE<0.81%, the wire rod is grade 70; when 0.81%≤CE<0.91%, the wire rod is grade 80; when CE≥0.91%, the wire rod is grade 90.
[0022] In the formula CE=C+Mn / 6, CE refers to the carbon equivalent of the material, C is the carbon content of the material, and Mn is the manganese content of the material.
[0023] Step 2: Perform multiple sets of unidirectional torsion tests on the wire rod to obtain the actual number of torsion turns of the wire rod.
[0024] The wire rod is sampled and subjected to a unidirectional torsion test. The purpose of the torsion experiment is to obtain the number of torsion circles of the wire rod. This is an effective method to judge the uniformity of the wire rod structure. There are widely accepted torsion sample methods and torsion circle acquisition methods in the industry. The wire rod is not straightened, and the iron oxide scale is required to be complete, without surface defects such as transverse scratches on the surface or linear longitudinal scratches visible to the naked eye. During the unidirectional torsion test, one end of the wire rod is fixed with a chuck, and the other end is clamped by another chuck for unidirectional torsion, and a tensile force of 200N is applied. The distance between the two chucks is 200±10mm, and the torsion test speed is 30r / min. The external room temperature range of the test is required to be 15~35℃. If the torsion fracture is located at the chuck position or connected to the chuck, the test result is an invalid result. The torsion test is carried out for at least 10 groups, and each group obtains a torsion circle. After excluding invalid results, the average is taken as the actual torsion circle of the wire rod.
[0025] Step 3: Resample the wire rod and conduct multiple sets of repeated bending tests to obtain the actual number of repeated bending times of the wire rod.
[0026] After the wire rod is resampled, it is subjected to repeated bending tests. The repeated bending is to obtain the toughness limit of the local area and to inspect the specific parts. The parameter obtained is the number of repeated bending times of the material; repeated bending is also a conventional wire inspection method. The wire rod is not straightened, and the iron oxide scale is required to be complete, without surface defects such as transverse scratches on the surface or linear longitudinal scratches visible to the naked eye. The length of the wire rod sample is 150±10mm, the diameter of the elbow used in the test is 60mm, the test bending angle is ±90°, the test speed is 10 times / min, and the external room temperature range of the test is required to be 10-35℃. At least 5 groups of repeated bending tests are carried out, and a number of repeated bending times is obtained after each group of tests. The average value is taken as the actual number of repeated bending times of the wire rod.
[0027] Step 4: Calculate the rough breaking parameters of the wire rod according to the wire rod classification, torsion test results and repeated bending test results, and evaluate the rough breaking rate of the wire rod according to the rough breaking parameters.
[0028] In the present invention, the rough breaking parameter = (number of twisting turns × 5 + number of repeated bending times × 3.5) × steel type coefficient, wherein the steel type coefficients corresponding to grade 70, grade 80 and grade 90 steels are 1.0, 1.2 and 1.38.
[0029] The evaluation criteria are: when the rough breaking parameter of the cord steel wire rod is ≥125, the predicted rough breaking rate of the wire rod is <1.0 times / thousand tons; when the rough breaking parameter of the cord steel wire rod is 100-125, the predicted rough breaking rate of the wire rod is 1.0-3.0 times / thousand tons; when the rough breaking parameter of the cord steel wire rod is 75-100, the predicted rough breaking rate of the wire rod is 3.0-5.0 / thousand tons; when the rough breaking parameter of the cord steel wire rod is <75, the predicted rough breaking rate of the wire rod is ≥5.0 times / thousand tons.
[0030] In the present invention, the evaluation criteria are obtained by combining theoretical derivation with a large amount of actual production data statistics and verification. The rough wire break rate is a method for testing the uniformity and plastic toughness of the wire rod. Due to the randomness and uncertainty of the occurrence of rough breakage, there is currently no feasible test method, and it can only be obtained by using statistical data in the process. However, rough breakage is actually caused by the lack of plasticity and uniformity of the material. The uniformity and plasticity of the material are quantified by torsion and repeated bending, and combined with the strength base (carbon equivalent) of the material, its rough breakage can be effectively characterized.
[0031] Embodiments 1 to 4
[0032] The present invention was verified by taking 4 groups of tests, and the diameter of the cord steel wire rods was φ5.5 mm. The relevant test parameters and test results are shown in Table 1.
[0033] Table 1 Relevant experimental parameters and test results of Examples 1 to 4
[0034]
[0035] In the present invention, the actual rough wire breakage rate is obtained by using the batch of wire rods completely and tracking and recording the whole process during use. As shown in Table 1, the rough wire breakage rate of wire rods obtained by the method of the present invention is consistent with the actual rough wire breakage rate.
[0036] The method for evaluating the rough wire breakage rate introduced in the present invention is to quantify the relationship between the internal structure performance of the wire rod and the rough wire breakage under the premise of ensuring the surface quality and uniform size of the wire rod. All the cord steel wire rods in the embodiment are uniform in size and have no surface defects visible to the naked eye. At present, the diameter of most cord steel wire rods on the market is φ5.5mm, so the diameter of all cord steel wire rods in the embodiment is φ5.5mm.
[0037] Finally, it should be noted that the above are only preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to replace some of the technical features therein with equivalents. However, any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for evaluating the rough broken wire rate of a cord steel wire rod, characterized in that: The method specifically comprises the following steps: Step 1: Calculate the carbon equivalent of the cord steel wire rod and classify the wire rod; Step 2, performing multiple sets of unidirectional torsion tests on the wire rod to obtain the actual number of torsion turns of the wire rod; Step 3: re-sample the wire rod and conduct multiple sets of repeated bending tests to obtain the actual number of repeated bending times of the wire rod; Step 4: Calculate the rough breaking parameters of the wire rod according to the wire rod classification, torsion test results and repeated bending test results, and evaluate the rough breaking rate of the wire rod according to the rough breaking parameters; In step 1, the carbon equivalent of the cord steel wire rod is calculated according to the formula CE=C+Mn / 6, where CE refers to the carbon equivalent of the material, C refers to the carbon content of the material, and Mn refers to the manganese content of the material; In step 1, the wire rod is graded according to the carbon equivalent: when CE < 0.81%, the wire rod is grade 70; when 0.81% ≤ CE < 0.91%, the wire rod is grade 80; when CE ≥ 0.91%, the wire rod is grade 90; In step 2, the method of the unidirectional torsion test of the wire rod is as follows: one end of the wire rod is fixed by a chuck, and the other end is clamped by another chuck for unidirectional torsion, and a tensile force of 200N is applied; the distance between the two chucks is 200±10mm, and the torsion test speed is 30r / min; the external room temperature range of the test is required to be 15-35℃; the torsion test is performed for at least 10 groups, and a torsion number is obtained for each group. After excluding invalid results, the average value is taken as the actual torsion number of the wire rod; In step 3, the method of repeated bending test is as follows: the length of the wire rod sample is 150±10mm, the diameter of the elbow used in the test is 60mm, the test bending angle is ±90°, the test speed is 10 times / min, and the test external room temperature range is required to be 10-35°C; the repeated bending test is performed for at least 5 groups, and a repeated bending number is obtained after each group of tests, and the average value is taken as the actual repeated bending number of the wire rod; In step 4, the rough breaking parameter of the wire rod = (number of twisting circles × 5 + number of repeated bending times × 3.5) × steel type coefficient, and the steel type coefficients corresponding to grade 70, grade 80 and grade 90 steel are 1.0, 1.2 and 1.38; In step 4, when the rough breaking parameter of the cord steel wire rod is ≥125, the rough breaking rate of the wire rod is <1.0 times / kiloton; when the rough breaking parameter of the cord steel wire rod is 100-125, the rough breaking rate of the wire rod is 1.0-3.0 times / kiloton; when the rough breaking parameter of the cord steel wire rod is 75-100, the rough breaking rate of the wire rod is 3.0-5.0 / kiloton; when the rough breaking parameter of the cord steel wire rod is <75, the rough breaking rate of the wire rod is ≥5.0 times / kiloton.