A phenolic resin cotton cloth laminate for automobiles and a preparation method thereof
By treating old cotton cloth with modified glue and combining composite phenolic resin solution, epoxy resin and other materials, a phenolic resin cotton cloth laminate for automobiles with excellent heat resistance and mechanical properties was prepared, which solved the poor heat resistance and resources in the existing technology. The problem of waste has achieved high performance and environmentally friendly laminate production.
Patent Information
- Application Number
- CN202210457949.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-28
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-04-28
AI Technical Summary
The existing phenolic cotton cloth laminates have poor heat resistance of cotton cloth and ordinary phenolic resins, resulting in a shortening of product service life, and the waste of old cotton cloth resources, and lack of methods to use old cotton cloth to produce phenolic resin cotton cloth laminates for automobiles.
Non-woven fabrics are prepared by using modified glue solution to prepare the old cotton fabric, and impregnated and pressed by composite phenolic resin solution, epoxy resin, SBS resin and other materials to form a laminate with high mechanical properties and heat resistance.
It significantly improves the heat resistance and mechanical properties of the laminate, reduces water absorption, and is used for a long time without formaldehyde in high temperature and high humidity environments, extends product life and reduces resource waste.
Smart Images

Figure BDA0003621097590000121 
Figure BDA0003621097590000122 
Figure BDA0003621097590000131
Abstract
Description
Technical Field
[0001] The invention belongs to the field of laminated boards, and in particular relates to a phenolic resin cotton cloth laminated board for automobiles and a preparation method thereof. Background Art
[0002] Laminate is a whole made of two or more layers of resin-impregnated fibers or fabrics that are laminated and hot-pressed. The performance of laminate depends on the substrate and adhesive as well as the molding process. Laminates can be divided into the following two types according to their composition, characteristics and heat resistance.
[0003] 1. Organic substrate laminate: wood pulp insulation paper, cotton fiber paper, cotton cloth, etc. are used as reinforcement materials. The long-term use temperature can reach 120°C, and synthetic fiber products are also developed as reinforcement materials.
[0004] 2. Inorganic substrate laminate: Inorganic glass fiber cloth, alkali-free glass fiber felt, etc. are used as reinforcing materials. The long-term use temperature is 130-180°C, and can even reach higher temperatures, depending on the adhesive resin.
[0005] The current phenolic cotton cloth laminate is made of cotton cloth impregnated with phenolic resin and then dried and hot pressed. It has high mechanical properties and is suitable for use as insulating structural parts in machinery, motors, and electrical equipment, and can be used in transformer oil. The general phenolic cotton cloth laminate has a short service life due to the poor heat resistance of cotton cloth and ordinary phenolic resin.
[0006] Cotton cloth is a cloth woven from cotton yarn, and is a general term for various cotton textiles. It is mostly used to make fashion, casual wear, underwear and shirts. Currently, there are many old cotton cloths, which are often discarded, resulting in a waste of resources. Therefore, it is necessary to propose a method for producing a phenolic resin cotton cloth laminate for automobiles using old cotton cloth and a preparation method thereof. Summary of the invention
[0007] In order to solve the above problems in the prior art, the present invention adopts the following technical solutions:
[0008] A phenolic resin cotton cloth laminate for automobiles, comprising multiple layers of reinforcing materials treated with a modified adhesive, wherein the reinforcing materials include non-woven fabrics obtained by treating old cotton cloth;
[0009] The modified rubber solution comprises the following raw materials in parts by weight:
[0010] 100-120 parts of composite phenolic resin solution, 1-3 parts of dibutyl phthalate, 0.2-0.5 parts of acetyl tributyl citrate, 0.1-0.5 parts of coupling agent, 2-4 parts of dispersant;
[0011] The coupling agent is an aluminate coupling agent, which can improve the physical properties of the product, such as improving the impact strength and heat deformation temperature; and has the characteristics of low cost, light color, non-toxicity, and easy use.
[0012] Furthermore, the dispersant is fatty acid polyethylene glycol ester; by adding fatty acid polyethylene glycol ester, the dispersibility of each component in the composite phenolic resin solution can be improved and the uniformity of the modified glue solution can be maintained.
[0013] Furthermore, the composite phenolic resin solution comprises the following raw materials in parts by weight:
[0014] 25-30 parts of phenolic resin, 5-10 parts of epoxy resin, 6-8 parts of SBS resin, 63-70 parts of solvent, and 1-2 parts of stabilizer.
[0015] Furthermore, the phenolic resin is a linear bisphenol A phenolic resin; the phenolic resin can be well fused with the epoxy resin, and the epoxy group in the epoxy resin can react with the phenolic hydroxyl group and the hydroxymethyl group in the phenolic resin to cure the phenolic resin, thereby improving the high temperature stability, heat resistance and dimensional stability of the phenolic resin, and the linear bisphenol A phenolic resin and the epoxy resin have good fusion properties, which can improve the problems of brown spots and discoloration;
[0016] In the present invention, the epoxy resin may be bisphenol F type epoxy resin, which has the characteristics of low viscosity and good impregnation property for cotton fiber.
[0017] In the present invention, SBS resin has excellent tensile strength, elasticity and electrical properties. It has small permanent deformation, good flexure and resilience, large surface friction, and similar ozone, oxygen and ultraviolet radiation resistance as styrene-butadiene rubber, and excellent air permeability; the SBS resin is used as a compatibilizing resin and a toughening resin to improve the bonding ability of the system, thereby improving the impregnation effect, and improving the co-melting ability of epoxy resin in phenolic resin. The specific SBS resin is a linear SBS resin.
[0018] Furthermore, the solvent includes any one or both of methanol and ethyl acetate; by adding the solvent, the phenolic resin, epoxy resin and SBS resin are dissolved, so as to facilitate the impregnation of the reinforcing material;
[0019] Furthermore, the stabilizer is polyester fiber with an average length of 5-6 mm. The addition of the stabilizer stabilizes the composite phenolic resin solution, which facilitates the subsequent application of the modified glue to the reinforcing material and the curing of the modified glue. The stabilizer can also slow down the reaction, maintain chemical balance, reduce surface tension, and prevent light, thermal decomposition or oxidative decomposition.
[0020] Furthermore, the old cotton cloth is waste polyester-cotton blended textile;
[0021] In the present invention, by adding dibutyl phthalate, it can be inserted between polymer molecular chains, weakening the interaction between polymer molecular chains, resulting in increased mobility of polymer molecular chains, reduced crystallinity of polymer molecular chains, thereby increasing the plasticity of the polymer, and having good compatibility with the resin, which can improve the durability and cold resistance of the resin.
[0022] In the present invention, by adding acetyl tributyl citrate, the solubility of dibutyl phthalate in the glue solution can be improved, which facilitates the impregnation; because it is compatible with various celluloses, vinyl resins, chlorinated rubber, etc., and is partially compatible with cellulose acetate and butyl acetate cellulose.
[0023] A method for preparing a phenolic resin cotton cloth laminate for automobiles comprises the following steps:
[0024] S1. Preparation of composite phenolic resin solution
[0025] Prepare the raw materials of the composite phenolic resin solution according to the weight parts; fully mix the phenolic resin and the solvent, heat to 60-65°C, add SBS resin, stir; add epoxy resin, stir, and then add stabilizer to obtain a composite phenolic resin solution; set aside;
[0026] S2. Preparation of modified glue solution
[0027] Prepare the modified adhesive liquid according to the weight of the raw materials; fully mix the composite phenolic resin solution and the dispersant, add the coupling agent, stir, then add dibutyl phthalate and acetyl tributyl citrate, stir, and stand to obtain the modified adhesive liquid; set aside;
[0028] S3. Treatment of old cotton cloth
[0029] After washing and drying the old cotton cloth, the polyester and cotton fibers obtained by alcoholysis are filtered through a polyester-cotton filter to obtain cotton fibers; the cotton fibers are laid and arranged, and then subjected to a hydroentanglement treatment to obtain a non-woven fabric;
[0030] S4. Impregnation treatment
[0031] The nonwoven fabric prepared in step S3 is coated with the modified adhesive solution prepared in step S2, and after the impregnation, it is dried to obtain a prepreg;
[0032] S5. Pressing
[0033] Multiple layers of prepregs are stacked together and pressed to obtain the laminate.
[0034] Furthermore, the hydroentanglement process is to entangle the cotton fiber web at a hydroentanglement pressure of 50-60*10 5Fixed under the pa.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] 1. Through the preparation of modified glue, the non-woven fabric is impregnated and then pressed to form a laminate with low water absorption and excellent mechanical properties.
[0037] 2. The heat resistance of the laminated board is significantly improved by preparing non-woven fabrics from waste polyester-cotton blended textiles and then impregnating and pressing the non-woven fabrics with modified adhesive.
[0038] 3. The laminate prepared by the present invention has no formaldehyde release detected and can be used for a long time in a high temperature and high humidity environment. DETAILED DESCRIPTION
[0039] The technical solution of the present invention is further described below, but the scope of protection claimed is not limited to the description.
[0040] Example 1
[0041] The non-woven fabric of the present invention is obtained by processing old cotton fabric; the specific preparation process of the non-woven fabric is as follows:
[0042] 120 kg / h of waste polyester-cotton blended textiles are weighed and melted in a screw. At the same time, 600 kg / h of ethylene glycol is added to the screw. The waste polyester-cotton blended textiles are alcoholyzed at normal pressure and a temperature of 200°C for 10 minutes. After alcoholyzation and melting in a rag melting machine, the waste polyester-cotton blended textiles are processed by a polyester-cotton filter system (processed by a polyester-cotton filter) to recover the cotton fibers. After the cotton fibers are evaporated to dryness, a carding machine is used to straighten the opened cotton fibers, and the carded cotton fibers are overlapped and laid on a net to make the cotton fibers into a cotton fiber net. The cotton fiber net is subjected to a spunlace process to entangle the cotton fibers into a non-woven fabric. The specific spunlace process is as follows: the cotton fiber net is subjected to a spunlace pressure of 50-60*10 5 The above steps can obtain a non-woven fabric with a thickness of 0.4-0.5 mm. The tear strength of the non-woven fabric is 20-21N.
[0043] Example 2
[0044] A phenolic resin cotton cloth laminate for automobiles, comprising multiple layers of reinforcing materials treated with modified adhesive,
[0045] The modified rubber solution comprises the following raw materials in parts by weight:
[0046] 1 part of dibutyl phthalate, 0.2 parts of acetyl tributyl citrate, 0.1 parts of aluminate coupling agent, 2 parts of fatty acid polyethylene glycol ester; 25 parts of linear bisphenol A phenolic resin, 5 parts of bisphenol F epoxy resin, 6 parts of linear SBS resin; 33 parts of methanol, 30 parts of ethyl acetate; 1 part of stabilizer, specifically polyester fiber, with an average length of 5-6mm;
[0047] The method for preparing the above-mentioned phenolic resin cotton cloth laminate for automobiles comprises the following steps:
[0048] S1. Preparation of composite phenolic resin solution
[0049] Prepare the materials according to the weight of the raw materials of the composite phenolic resin solution; stir the phenolic resin and the solvent at a stirring speed of 100 r / mim, mix for 1 hour, heat to 60°C, add the SBS resin, stir at a speed of 80 r / mim, mix for 1 hour; add the epoxy resin, stir at a stirring speed of 80 r / mim, mix for 1 hour, then add the stabilizer, stir at a speed of 80 r / mim, mix for 1 hour, and obtain the composite phenolic resin solution; set aside;
[0050] S2. Preparation of modified glue solution
[0051] Prepare the modified adhesive solution according to the weight of the raw materials; stir the composite phenolic resin solution and the dispersant at 35°C at a stirring speed of 50r / mim for 10 minutes, then add the coupling agent; stir at a stirring speed of 50r / mim for 5 minutes, then add dibutyl phthalate and acetyl tributyl citrate; stir at a stirring speed of 50r / mim for 5 minutes, cool to room temperature, and obtain the modified adhesive solution; set aside;
[0052] S3. Treatment of old cotton cloth
[0053] According to Example 1
[0054] S4. Impregnation treatment
[0055] The non-woven fabric prepared in step S3 is dipped into the modified glue solution in a horizontal dipping tank for gluing, and the dipping speed of the non-woven fabric is 3 m / min; after the dipping is completed, it is dried at 130° C. for 5 min to obtain a semi-solid sheet; the semi-solid sheet is controlled to have a glue content of 50-51%;
[0056] S5. Pressing
[0057] After stacking the prepregs obtained in step S4, preheat at 100°C for 15 min and raise the temperature to 150°C. 2 The laminate was pressed for 2 hours and then cooled to room temperature to obtain the laminate.
[0058] Example 3
[0059] A phenolic resin cotton cloth laminate for automobiles, comprising multiple layers of reinforcing materials treated with a modified adhesive solution;
[0060] The modified rubber solution comprises the following raw materials in parts by weight:
[0061] 2 parts of dibutyl phthalate, 0.3 parts of acetyl tributyl citrate, 0.3 parts of aluminate coupling agent, 3 parts of fatty acid polyethylene glycol ester; 28 parts of linear bisphenol A phenolic resin, 7 parts of bisphenol F epoxy resin, 7 parts of linear SBS resin; 20 parts of methanol, 46 parts of ethyl acetate; 1.5 parts of stabilizer, specifically polyester fiber, with an average length of 5-6mm;
[0062] The method for preparing the above-mentioned phenolic resin cotton cloth laminate for automobiles comprises the following steps:
[0063] S1. Preparation of composite phenolic resin solution
[0064] Prepare the raw materials of the composite phenolic resin solution according to the weight parts; stir the phenolic resin and the solvent at a stirring speed of 130r / mim, mix for 1h, heat to 63°C, add SBS resin, stir at a speed of 90r / mim, mix for 1h; add epoxy resin, stir at a stirring speed of 90r / mim, mix for 1h, then add stabilizer, stir at a stirring speed of 90r / mim, mix for 1h, and obtain a composite phenolic resin solution; set aside;
[0065] S2. Preparation of modified glue solution
[0066] Prepare the modified adhesive solution according to the weight of the raw materials; stir the composite phenolic resin solution and the dispersant at 38°C at a stirring speed of 55r / mim for 10min, then add the coupling agent; stir at a stirring speed of 55r / mim for 5min, then add dibutyl phthalate and acetyl tributyl citrate; stir at a stirring speed of 55r / mim for 5min, cool to room temperature to obtain the modified adhesive solution; set aside;
[0067] S3. Treatment of old cotton cloth
[0068] According to Example 1
[0069] S4. Impregnation treatment
[0070] The non-woven fabric prepared in step S3 is dipped into the modified glue solution in a horizontal dipping tank for gluing, and the dipping speed of the non-woven fabric is 3.5 m / min; after the dipping is completed, it is dried at 133° C. for 7 minutes to obtain a semi-solid sheet; the semi-solid sheet is controlled to have a glue content of 51-53%;
[0071] S5. Pressing
[0072] After stacking the prepregs obtained in step S4, preheat at 105°C for 18 min to 155°C and heat at 85 Kg / cm 2 The laminate was pressed for 2.3 hours and then cooled to room temperature to obtain the laminate.
[0073] Example 4
[0074] A phenolic resin cotton cloth laminate for automobiles, comprising multiple layers of reinforcing materials treated with modified adhesive,
[0075] The modified rubber solution comprises the following raw materials in parts by weight:
[0076] 3 parts of dibutyl phthalate, 0.5 parts of acetyl tributyl citrate, 0.5 parts of aluminate coupling agent, 4 parts of fatty acid polyethylene glycol ester; 30 parts of linear bisphenol A phenolic resin, 10 parts of bisphenol F epoxy resin, 8 parts of linear SBS resin; 35 parts of methanol, 35 parts of ethyl acetate; 2 parts of stabilizer, specifically polyester fiber, with an average length of 6 mm;
[0077] The method for preparing the above-mentioned phenolic resin cotton cloth laminate for automobiles comprises the following steps:
[0078] S1. Preparation of composite phenolic resin solution
[0079] Prepare the materials according to the weight of the raw materials of the composite phenolic resin solution; stir the phenolic resin and the solvent at a stirring speed of 150r / mim, mix for 1 hour, heat to 65°C, add the SBS resin, stir at a speed of 100r / mim, mix for 1 hour; add the epoxy resin, stir at a stirring speed of 100r / mim, mix for 1 hour, then add the stabilizer, stir at a speed of 100r / mim, mix for 1 hour, and obtain the composite phenolic resin solution; set aside;
[0080] S2. Preparation of modified glue solution
[0081] Prepare the modified adhesive liquid according to the weight of the raw materials; stir the composite phenolic resin solution and the dispersant at 40°C at a stirring speed of 60r / mim for 10 minutes, then add the coupling agent; stir at a stirring speed of 60r / mim for 5 minutes, then add dibutyl phthalate and acetyl tributyl citrate; stir at a stirring speed of 60r / mim for 5 minutes, cool to room temperature, and obtain the modified adhesive liquid; set aside;
[0082] S3. Treatment of old cotton cloth
[0083] According to Example 1
[0084] S4. Impregnation treatment
[0085] The non-woven fabric prepared in step S3 is dipped into the modified glue solution in a horizontal dipping tank for gluing, and the dipping speed of the non-woven fabric is 4 m / min; after the dipping is completed, it is dried at 135° C. for 8 min to obtain a semi-solid sheet; the semi-solid sheet is controlled to have a glue content of 55%;
[0086] S5. Pressing
[0087] After stacking the prepregs obtained in step S4, preheat at 110°C for 20 min to 160°C and heat at 90 Kg / cm 2 The laminate was pressed for 2.5 hours and then cooled to room temperature to obtain the laminate.
[0088] Example 5
[0089] A phenolic resin cotton cloth laminate for automobiles, comprising multiple layers of reinforcing materials treated with modified adhesive,
[0090] The modified rubber solution comprises the following raw materials in parts by weight:
[0091] 1 part of dibutyl phthalate, 0.4 parts of acetyl tributyl citrate, 0.5 parts of aluminate coupling agent, 2 parts of fatty acid polyethylene glycol ester; 30 parts of linear bisphenol A phenolic resin, 5 parts of bisphenol F epoxy resin, 8 parts of linear SBS resin; 30 parts of methanol, 40 parts of ethyl acetate; 1 part of stabilizer, specifically polyester fiber, with an average length of 5-6mm;
[0092] The method for preparing the above-mentioned phenolic resin cotton cloth laminate for automobiles comprises the following steps:
[0093] S1. Preparation of composite phenolic resin solution
[0094] Prepare the materials according to the weight of the raw materials of the composite phenolic resin solution; stir the phenolic resin and the solvent at a stirring speed of 100 r / mim, mix for 1 hour, heat to 65°C, add SBS resin, stir at a speed of 80 r / mim, mix for 1 hour; add epoxy resin, stir at a stirring speed of 100 r / mim, mix for 1 hour, then add stabilizer, stir at a speed of 80 r / mim, mix for 1 hour, and obtain a composite phenolic resin solution; set aside;
[0095] S2. Preparation of modified glue solution
[0096] Prepare the modified adhesive liquid according to the weight of the raw materials; stir the composite phenolic resin solution and the dispersant at 35°C at a stirring speed of 60r / mim for 10 minutes, then add the coupling agent; stir at a stirring speed of 50r / mim for 5 minutes, then add dibutyl phthalate and acetyl tributyl citrate; stir at a stirring speed of 60r / mim for 5 minutes, cool to room temperature, and obtain the modified adhesive liquid; set aside;
[0097] S3. Treatment of old cotton cloth
[0098] According to Example 1
[0099] S4. Impregnation treatment
[0100] The non-woven fabric prepared in step S3 is dipped into the modified glue solution in a horizontal dipping tank for gluing, and the dipping speed of the non-woven fabric is 4 m / min; after the dipping is completed, it is dried at 135° C. for 5 min to obtain a semi-solid sheet; the semi-solid sheet is controlled to have a glue content of 52-53%;
[0101] S5. Pressing
[0102] After stacking the prepregs obtained in step S4, preheat at 100°C for 15 min to 160°C and heat at 90 Kg / cm 2 The laminate was pressed for 2 hours and then cooled to room temperature to obtain the laminate.
[0103] Comparative Example 1
[0104] The non-woven fabric in step S3 is replaced with clean, unused cotton fabric (the size and thickness are consistent with the non-woven fabric); the other conditions are consistent with those in Example 2.
[0105] Comparative Example 2
[0106] The modified rubber solution comprises the following raw materials in parts by weight:
[0107] 1 part of dibutyl phthalate, 0.2 parts of acetyl tributyl citrate, 0.1 parts of aluminate coupling agent, 2 parts of fatty acid polyethylene glycol ester; 25 parts of linear bisphenol A phenolic resin; 33 parts of methanol, 30 parts of ethyl acetate; 1 part of stabilizer, specifically polyester fiber, with an average length of 5-6 mm; the other conditions are the same as those in Example 2;
[0108] The laminates prepared in Examples 2 to 4 and Comparative Examples 1 to 2 were tested for performance, and the relevant results are shown in Table 1 below:
[0109] Table 1
[0110]
[0111] It can be seen from the above results that the laminates prepared in Examples 2 to 5 have a low water absorption rate of only 0.02-0.06%; have high mechanical properties, with a tensile strength of 138-146MPa, a flexural strength of 126-134MPa, and a heat resistance of over 183°C, and can be used in construction, automobile and other fields.
[0112] Comparative Example 1 starts with clean cotton cloth, which is usually attached with polyester, which has a certain degree of influence on the combination of the modified glue and the cotton cloth, resulting in a slightly higher water absorption rate;
[0113] Comparative Example 2, in which the non-woven fabric is directly combined with the phenolic resin, has slightly poor adhesion, and the bending strength and tensile strength are also poor. At the same time, since the phenolic resin has not been modified and coupled, formaldehyde will be released, affecting its use.
[0114] The laminated boards prepared in the above Example 2 and Comparative Example 1-2 were subjected to a temperature of 70°C and a humidity of 65±5% for 1300 hours to test their performance after moisture absorption. The relevant results are shown in Table 2 below:
[0115] Table 2
[0116]
[0117]
[0118] Therefore, it can be seen that under the action of high temperature and high humidity, the water absorption rate of Example 2 has basically not changed, and the tensile strength reaches 137MPa, and the bending strength is 124MPa, and the tensile strength and bending strength are slightly reduced, which shows that the laminate of Example 2, the glue and the non-woven fabric are firmly combined, the gap is small, and the water absorption rate can be maintained at a low level, and thus the tensile strength and bending strength can be maintained at a high level. The starting material of Comparative Example 1 is clean cotton cloth, and the cotton cloth is generally attached with polyester. Under the action of high temperature and high humidity for a long time, the polyester will absorb water and cause expansion, so the moisture absorption rate of Comparative Example 1 increases, which in turn causes a decrease in tensile strength and bending strength; while Comparative Example 2 directly combines the non-woven fabric with phenolic resin, and the adhesion is poor. Under the action of high temperature and high humidity for a long time, part of the resin is detached, which makes the moisture absorption rate of Comparative Example 1 increase significantly, which in turn causes a significant decrease in tensile strength and bending strength;
[0119] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art of the present invention, several equivalent substitutions or obvious variations can be made without departing from the concept of the present invention, and the performance or use is the same, which should be regarded as belonging to the present invention.
Claims
1. A phenolic resin cotton cloth laminate for automobiles, comprising multiple layers of reinforcing materials treated with a modified adhesive, characterized in that: The reinforcing material comprises a nonwoven fabric; The modified rubber solution comprises the following raw materials in parts by weight: 100-120 parts of composite phenolic resin solution, 1-3 parts of dibutyl phthalate, 0.2-0.5 parts of acetyl tributyl citrate, 0.1-0.5 parts of coupling agent, 2-4 parts of dispersant; The preparation method of the phenolic resin cotton cloth laminate for automobiles comprises the following steps: S1. Preparation of composite phenolic resin solution Prepare the raw materials of the composite phenolic resin solution according to the weight parts; fully mix the phenolic resin and the solvent, heat to 60-65°C, add SBS resin, stir; add epoxy resin, stir, and then add stabilizer to obtain a composite phenolic resin solution; set aside; S2. Preparation of modified glue solution Prepare the modified adhesive liquid according to the weight of the raw materials; fully mix the composite phenolic resin solution and the dispersant, add the coupling agent, stir, then add dibutyl phthalate and acetyl tributyl citrate, stir, and stand to obtain the modified adhesive liquid; set aside; S3. Treatment of old cotton cloth After washing and drying the old cotton cloth, the polyester and cotton fibers obtained by alcoholysis are filtered through a polyester-cotton filter to obtain cotton fibers; the cotton fibers are laid and arranged, and then subjected to a hydroentanglement treatment to obtain a non-woven fabric; S4. Impregnation treatment The nonwoven fabric prepared in step S3 is coated with the modified adhesive solution prepared in step S2, and after the impregnation, it is dried to obtain a prepreg; S5. Pressing The prepreg obtained in the multi-layer step S4 is pressed and formed to obtain the laminated board; The hydroentanglement process is as follows: the cotton fiber web is subjected to a hydroentanglement pressure of 50-60*10 5 Fixed under the pa.
2. The phenolic resin cotton cloth laminate for automobiles according to claim 1, characterized in that: The coupling agent is an aluminate coupling agent.
3. The phenolic resin cotton cloth laminate for automobiles according to claim 1, characterized in that: The dispersant is fatty acid polyethylene glycol ester.
4. The phenolic resin cotton cloth laminate for automobiles according to claim 1, characterized in that: The composite phenolic resin solution comprises the following raw materials in parts by weight: 25-30 parts of phenolic resin, 5-10 parts of epoxy resin, 6-8 parts of SBS resin, 63-70 parts of solvent, and 1-2 parts of stabilizer.
5. The phenolic resin cotton cloth laminate for automobiles according to claim 4, characterized in that: The phenolic resin is a linear bisphenol A phenolic resin.
6. The phenolic resin cotton cloth laminate for automobiles according to claim 4, characterized in that: The solvent includes any one or both of methanol and ethyl acetate.
7. The phenolic resin cotton cloth laminate for automobiles according to claim 4, characterized in that: The stabilizer is polyester fiber with an average length of 5-6 mm.