GaN-based light-emitting diode based on C-doped current spreading layer and preparation method thereof
By adopting a three-layer structure n-type GaN layer with C doped in GaN-based light emitting diodes, the current congestion effect in transverse structure LEDs is solved, the device efficiency and reliability are improved, the process flow is simplified, and the existing technology is solved Problems of process complexity and luminescent quantum well quality.
Patent Information
- Application Number
- CN202210183114.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-02-27
AI Technical Summary
In the existing GaN-based light-emitting diodes, the carrier distribution and local overheating are caused by the current congestion effect of the transverse structure LED, which reduces the device efficiency and reliability. The existing current expansion layer method increases the process complexity and affects the luminescent quantum. crystal mass of the well.
Using a three-layer structure n-type GaN layer based on C doping, the Si source is turned off, the growth temperature is reduced, and the C-doped GaN layer with poor conductivity is inserted to alleviate the Current congestion effect and simplify process flow.
It effectively alleviates the current congestion effect in lateral structure LEDs, improves device efficiency and reliability, and simplifies the preparation process of GaN-based light-emitting diodes, reducing costs and complexity.
Smart Images

Figure CN114843374B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of microelectronics and relates to a GaN-based light-emitting diode based on a C-doped current extension layer and a preparation method thereof. Background Art
[0002] GaN-based light-emitting diodes (LEDs) have the advantages of high efficiency, energy saving, environmental protection, long life, small size, good color rendering and response speed. LED-based semiconductor lighting has gradually replaced traditional lighting.
[0003] Due to the price and size restrictions of GaN single crystals, GaN is currently usually grown by heteroepitaxial growth. Sapphire is the most commonly used substrate for GaN growth, with the advantages of mature production technology, moderate price, high mechanical strength, and high cost performance. However, since sapphire is an insulator, it is impossible to make vertical structure devices, and the current lateral structure LED is the mainstream. Since the p-type electrode and n-type electrode of the lateral structure LED chip are located on the same side, and the conductivity of the p-type material and the n-type material is different, there is inevitably a current congestion effect, which leads to uneven carrier distribution and local overheating, reducing device efficiency and reliability. Therefore, the current spreading layer came into being. It is by introducing a layer of low resistivity layer structure in the structure, increasing the longitudinal resistance of the LED, and redistributing the current, thereby improving the lateral current spreading of the chip. The reported current spreading layers include transparent conductive oxide films, current blocking layers under the p-type electrode, and AlGaN layers in the n-type layer.
[0004] However, these methods require additional growth steps, which increase the process complexity, and the additional inserted layer structure may affect the crystal quality of the light-emitting quantum well layer. Summary of the invention
[0005] In order to solve the above problems existing in the prior art, the present invention provides a GaN-based light-emitting diode based on a C-doped current spreading layer and a preparation method thereof. The technical problem to be solved by the present invention is achieved by the following technical solutions:
[0006] An embodiment of the present invention provides a method for preparing a GaN-based light-emitting diode based on a C-doped current spreading layer, and the method for preparing a GaN-based light-emitting diode comprises:
[0007] Selecting a sapphire substrate layer;
[0008] growing an AlN nucleation layer on the sapphire substrate layer;
[0009] growing a U-type GaN layer on the AlN nucleation layer;
[0010] growing a first n-type GaN layer on the U-type GaN layer;
[0011] growing a second C-doped GaN layer on the first n-type GaN layer;
[0012] growing a third n-type GaN layer on the second C-doped GaN layer, wherein the first n-type GaN layer, the second C-doped GaN layer and the third n-type GaN layer constitute a three-layer structure of n-type GaN layers;
[0013] A multi-quantum well structure is grown on the third n-type GaN layer, wherein the multi-quantum well structure includes quantum wells of several periods, wherein the quantum wells include In x Ga 1-x The N well layer and the In x Ga 1-x A GaN barrier layer on the N-well layer;
[0014] Growing a p-type GaN layer on the multi-quantum well structure;
[0015] Etching the n-type electrode contact region to expose the first n-type GaN layer;
[0016] An n-type electrode is deposited on the first n-type GaN layer in the n-type electrode contact region and a p-type electrode is deposited on the p-type GaN layer to complete the manufacture of a GaN-based light-emitting diode.
[0017] In one embodiment of the present invention, a sapphire substrate layer is selected, including:
[0018] Cleaning the sapphire substrate layer;
[0019] The sapphire substrate layer is heat treated at a temperature of 900-1200° C. for 5-10 minutes;
[0020] The sapphire substrate layer after heat treatment is subjected to nitridation treatment for 3-5 minutes under the temperature condition of 1000-1100°C.
[0021] In one embodiment of the present invention, growing an AlN nucleation layer on the sapphire substrate layer comprises:
[0022] An AlN nucleation layer with a thickness of 20-50 nm is grown on the nitrided sapphire substrate layer using a MOCVD process.
[0023] In one embodiment of the present invention, growing a U-type GaN layer on the AlN nucleation layer comprises:
[0024] A U-type GaN layer with a thickness of 2-3 μm is grown on the AlN nucleation layer by using a MOCVD process.
[0025] In one embodiment of the present invention, growing a first n-type GaN layer on the U-type GaN layer comprises:
[0026] Ammonia, a gallium source and a silicon source are introduced, and the first n-type GaN layer is grown on the U-type GaN layer using a MOCVD process.
[0027] In one embodiment of the present invention, growing a second C-doped GaN layer on the first n-type GaN layer comprises:
[0028] The silicon source is turned off, the flow rates of ammonia and gallium source are kept unchanged, and a second C-doped GaN layer is grown on the first n-type GaN layer by using an MOCVD process under a second temperature condition, wherein the second temperature is lower than the first temperature.
[0029] In one embodiment of the present invention, growing a third n-type GaN layer on the second C-doped GaN layer comprises:
[0030] A silicon source is introduced, the flow rates of ammonia and gallium source are kept unchanged, and a third n-type GaN layer is grown on the second C-doped GaN layer by using an MOCVD process under a first temperature condition.
[0031] In one embodiment of the present invention, a single layer of In x Ga 1-x The thickness of the N well layer is 2-5 nm, and the thickness of the single-layer GaN barrier layer is 9-15 nm, wherein the adjustment range of the In content x is 0.1-0.7.
[0032] In one embodiment of the present invention, etching the n-type electrode contact region to expose the first n-type GaN layer includes:
[0033] The p-type GaN layer, the multi-quantum well structure, the third n-type GaN layer, the second C-doped GaN layer and a portion of the first n-type GaN layer at one end are etched away by a photolithography process to expose the remaining first n-type GaN layer.
[0034] Another embodiment of the present invention provides a GaN-based light-emitting diode based on a C-doped current spreading layer, which is prepared using the method for preparing a GaN-based light-emitting diode described in any of the above embodiments, and the GaN-based light-emitting diode includes:
[0035] Sapphire substrate layer;
[0036] An AlN nucleation layer is located on the sapphire substrate layer;
[0037] A U-type GaN layer, located on the AlN nucleation layer;
[0038] A first n-type GaN layer is located on the U-type GaN layer, and the first n-type GaN layer has a first upper surface and a second upper surface, and the second upper surface is located below the first upper surface;
[0039] A second C-doped GaN layer is located on a first upper surface of the first n-type GaN layer;
[0040] A third n-type GaN layer, located on the second C-doped GaN layer;
[0041] A multi-quantum well structure is located on the third n-type GaN layer, wherein the multi-quantum well structure includes a plurality of periodic quantum wells, wherein the quantum wells include In x Ga 1-x The N well layer and the In x Ga 1-x A GaN barrier layer on the N-well layer;
[0042] A p-type GaN layer, located on the multi-quantum well structure;
[0043] An n-type electrode is located on the second upper surface of the first n-type GaN layer;
[0044] The p-type electrode is located on the p-type GaN layer.
[0045] Compared with the prior art, the present invention has the following beneficial effects:
[0046] 1. The LED of the present invention has a three-layer structure of an n-type GaN layer, specifically, a C-doped GaN layer is inserted between two n-type GaN layers, and the C-doped GaN layer uses C impurities as acceptors to reduce the carrier concentration of the C-doped GaN layer, thereby reducing the conductivity of the C-doped GaN layer. Inserting a C-doped GaN layer with poor conductivity can increase the lateral expansion of the current, effectively alleviate the current congestion effect in the lateral structure LED, and improve the device efficiency and reliability.
[0047] 2. The present invention utilizes the unintentional doping phenomenon of C in the Ga source during the growth of GaN, lowers the growth temperature, and turns off the Si source to achieve C doping without introducing other growth sources during the growth process (i.e., no additional C source is required). The process for preparing GaN-based light-emitting diodes is simple and has strong applicability.
[0048] Other aspects and features of the present invention will become apparent from the following detailed description with reference to the accompanying drawings. It should be understood, however, that the drawings are designed for illustrative purposes only and are not intended to limit the scope of the present invention, as reference should be made to the appended claims. It should also be understood that, unless otherwise indicated, the drawings are not necessarily drawn to scale and are intended merely to conceptually illustrate the structures and processes described herein. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 A schematic flow chart of a method for preparing a GaN-based light-emitting diode based on a C-doped current spreading layer provided in an embodiment of the present invention;
[0050] FIG2 is a schematic diagram of a process of manufacturing a GaN-based light-emitting diode based on a C-doped current spreading layer provided by an embodiment of the present invention;
[0051] Figure 3 A schematic structural diagram of a GaN-based light-emitting diode based on a C-doped current spreading layer provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0052] The present invention is further described in detail below with reference to specific embodiments, but the embodiments of the present invention are not limited thereto.
[0053] Embodiment 1
[0054] See also Figure 1 and Figure 2, Figure 1 FIG2 is a schematic diagram of a process of preparing a GaN-based light-emitting diode based on a C-doped current spreading layer provided in an embodiment of the present invention. FIG2 is a schematic diagram of a process of preparing a GaN-based light-emitting diode based on a C-doped current spreading layer provided in an embodiment of the present invention. The present invention provides a method for preparing a GaN-based light-emitting diode based on a C-doped current spreading layer, and the method for preparing a GaN-based light-emitting diode comprises:
[0055] Step 1: Please refer to Figure 2a , select a sapphire substrate layer.
[0056] Step 1.1, clean the sapphire substrate layer.
[0057] Step 1.2: heat-treat the sapphire substrate layer at 900-1200° C. for 5-10 minutes.
[0058] Specifically, the vacuum degree of the reaction chamber is reduced to less than 2×10 -2 Torr; then hydrogen is introduced into the reaction chamber, and when the pressure of the MOCVD reaction chamber reaches 20-760 Torr, the sapphire substrate layer is heated to a temperature of 900-1200°C and maintained for 5-10 minutes to complete the heat treatment of the sapphire substrate layer.
[0059] Step 1.3: Perform a nitridation treatment on the heat-treated sapphire substrate layer at a temperature of 1000-1100° C. for 3-5 minutes.
[0060] Specifically, the heat-treated sapphire substrate layer is placed in a reaction chamber at a temperature of 1000-1100° C., and ammonia gas with a flow rate of 3000-4000 sccm is introduced, and the nitridation treatment is continued for 3-5 minutes.
[0061] Step 2: Please refer to Figure 2a , an AlN nucleation layer is grown on a sapphire substrate layer.
[0062] Specifically, an AlN nucleation layer with a thickness of 20-50 nm is grown on the nitrided sapphire substrate layer using a MOCVD process. In order to solve the mismatch problem between the sapphire substrate layer and the U-type GaN layer, an AlN nucleation layer is grown between the sapphire substrate layer and the U-type GaN layer.
[0063] Step 3, see Figure 2b , a U-type GaN layer (not intentionally doped with GaN) is grown on the AlN nucleation layer.
[0064] Specifically, a U-type GaN layer with a thickness of 2-3 μm is grown on the AlN nucleation layer by using a MOCVD process.
[0065] Step 4: Please refer to Figure 2c , a first n-type GaN layer is grown on the U-type GaN layer.
[0066] Specifically, ammonia, a gallium source and a silicon source are introduced, and a first n-type GaN layer is grown on the U-type GaN layer by using a MOCVD process under a first temperature condition.
[0067] Preferably, the first temperature is 1050°C.
[0068] Preferably, the Si doping concentration is 10 18 -10 19 cm -3 .
[0069] Furthermore, under the condition that the reaction chamber temperature is 1050°C, ammonia, gallium source and silicon source are introduced at the same time, and the MOCVD process is used to grow a first n-type GaN layer with a thickness of 1-1.5μm on the U-type GaN layer. In order to ensure that the second C-doped GaN layer can effectively reduce the current congestion effect without increasing the cost, the thickness of the first n-type GaN layer is set to 1-1.5μm.
[0070] Step 5: Please refer to Figure 2d , a second C-doped GaN layer is grown on the first n-type GaN layer.
[0071] Specifically, the silicon source is turned off, and the flow rates of ammonia and gallium sources are kept unchanged (i.e., the same as step 4). Under the second temperature condition, a second C-doped GaN layer is grown on the first n-type GaN layer using an MOCVD process, wherein the second temperature is lower than the first temperature. In order to effectively reduce the conductivity of the second C-doped GaN layer, the silicon source needs to be turned off. At the same time, in order to allow more C doping, the second temperature is lower than the first temperature.
[0072] Preferably, the second temperature is 600-850°C, because if the temperature is too high, the C doping will be less, thereby failing to effectively reduce the conductivity, while if the temperature is too low, it will be unfavorable for the growth of GaN, so the second temperature is set to 600-850°C.
[0073] Furthermore, the silicon source is turned off, the flow rates of ammonia and gallium sources are kept unchanged, the growth temperature is lowered from 1050°C to 600-850°C, and a second C-doped GaN layer with a thickness of 50-200nm is grown on the first n-type GaN layer using the MOCVD process. If the thickness of the second C-doped GaN layer is too thin, the conductivity cannot be effectively reduced, and if the thickness of the second C-doped GaN layer is too thick, the overall conductivity will be affected. The second C-doped GaN layer of 50-200nm can ensure the effective reduction of conductivity while maintaining good overall conductivity.
[0074] The Ga source of this embodiment can come from trimethylgallium or triethylgallium. Since there is carbon in the Ga source, C impurities will be doped into the material when the second C-doped GaN layer is grown, thereby making the second temperature lower than the first temperature, so as to allow more C doping by lowering the growth temperature.
[0075] Step 6. Please refer to Figure 2e A third n-type GaN layer is grown on the second C-doped GaN layer, and the first n-type GaN layer, the second C-doped GaN layer and the third n-type GaN layer constitute a three-layer structure of n-type GaN layers.
[0076] Specifically, a silicon source is introduced, the flow rates of ammonia and gallium source are kept unchanged (ie, the same as step 4), and a third n-type GaN layer is grown on the second C-doped GaN layer by using an MOCVD process under the first temperature condition.
[0077] Furthermore, a silicon source is introduced, the flow rates of ammonia and gallium sources are kept constant, the growth temperature is increased from 600-850°C to 1050°C, and a second C-doped GaN layer with a thickness of 300-500nm is grown on the first n-type GaN layer using an MOCVD process.
[0078] Step 7, see Figure 2fA multi-quantum well structure is grown on the third n-type GaN layer. The multi-quantum well structure includes several periods of quantum wells. The quantum wells include In x Ga 1-x The N well layer and the In x Ga 1-x The GaN barrier layer on the N-well layer may have, for example, 8-12 periods, specifically, 9 periods.
[0079] Preferably, a single layer of In x Ga 1-x The thickness of the N well layer is 2-5 nm, and the thickness of the single-layer GaN barrier layer is 9-15 nm, wherein the adjustment range of the In content x is 0.1-0.7.
[0080] Step 8. Please refer to Figure 2g , a p-type GaN layer is grown on the multi-quantum well structure.
[0081] Specifically, a Mg source is introduced, and a p-type GaN layer with a thickness of 100-200 nm is grown on the multi-quantum well structure using a MOCVD process, and the Mg doping concentration is 10 19 -10 22 cm -3 , then maintain the reaction chamber temperature at 800-1100°C and anneal for 5-10 minutes in a H2 atmosphere.
[0082] Step 9. Please refer to Figure 2h , etching the n-type electrode contact region to expose the first n-type GaN layer.
[0083] Specifically, the p-type GaN layer at one end, the multi-quantum well structure, the third n-type GaN layer, the second C-doped GaN layer and a portion of the first n-type GaN layer are etched away by photolithography to expose the remaining first n-type GaN layer.
[0084] Step 10. Please refer to Figure 2i , depositing an n-type electrode on the first n-type GaN layer in the n-type electrode contact region and depositing a p-type electrode on the p-type GaN layer to complete the fabrication of a GaN-based light-emitting diode.
[0085] Specifically, the n-type electrode is deposited on the first n-type GaN layer and the p-type electrode is deposited on the p-type GaN layer by sputtering metal, so as to complete the manufacture of the GaN-based light-emitting diode.
[0086] Because, in the current structure, there is a current gathering (also called current congestion) effect in the process of current flowing from the p-type electrode to the n-type electrode. Since the first n-type GaN layer and the third n-type GaN layer are conductive layers with many carriers, a C-doped GaN layer is added between the first n-type GaN layer and the third n-type GaN layer, which can neutralize some electrons and reduce the conductivity of the C-doped GaN layer. Inserting a C-doped GaN layer with poor conductivity can increase the lateral expansion of the current, thereby effectively alleviating the current congestion effect in the lateral structure LED and improving the device efficiency and reliability.
[0087] 2. The present invention utilizes the unintentional doping of C in the Ga source during the growth of GaN to reduce the growth temperature. Therefore, when growing the C-doped GaN layer, the Si source is turned off to achieve C doping. Therefore, C doping can be achieved without introducing other growth sources during the growth process (i.e., no additional C source is required). Therefore, this method can alleviate the current congestion effect in the lateral structure LED without increasing the process flow. At the same time, the process for preparing GaN-based light-emitting diodes is simple and has strong applicability.
[0088] Embodiment 2
[0089] The present invention further provides a method for preparing a C-doped blue LED with a light emission wavelength of 450 nm on the basis of the first embodiment. The method comprises:
[0090] Step 1: Heat treatment.
[0091] After cleaning, the sapphire substrate layer was placed in the MOCVD reaction chamber and the vacuum degree of the reaction chamber was reduced to 2×10 -2 Torr; then hydrogen is introduced into the reaction chamber, and when the pressure in the MOCVD reaction chamber reaches 20 Torr, the sapphire substrate layer is heated to 900°C and maintained for 10 minutes to complete the heat treatment of the sapphire substrate layer.
[0092] Step 2: High temperature nitriding.
[0093] The heat-treated sapphire substrate layer was placed in a reaction chamber at a temperature of 1000° C., and ammonia gas with a flow rate of 3500 sccm was introduced for 5 minutes to perform nitridation to complete the nitridation.
[0094] Step 3: growing an AlN nucleation layer.
[0095] See also Figure 2a Under the condition of a reaction chamber temperature of 1000°C, ammonia gas with a flow rate of 3000sccm and an aluminum source with a flow rate of 40sccm were introduced simultaneously, and an AlN nucleation layer with a thickness of 20nm was grown on the nitrided sapphire substrate layer using a MOCVD process.
[0096] Step 4: growing a U-type GaN layer.
[0097] See also Figure 2b Under the condition of a reaction chamber temperature of 950°C, ammonia gas with a flow rate of 2500sccm and a gallium source with a flow rate of 150sccm were introduced simultaneously, and a U-type GaN layer with a thickness of 2μm was grown on the AlN nucleation layer by MOCVD process while maintaining the pressure at 20Torr.
[0098] Step 5: Grow a three-layer n-type GaN layer.
[0099] 5a) Please see Figure 2c Under the condition of 1050℃ in the reaction chamber, ammonia with a flow rate of 2500sccm, gallium source with a flow rate of 150sccm and silicon source with a flow rate of 40sccm were introduced at the same time. Under the condition of maintaining the pressure at 20Torr, MOCVD process was used to grow a 1μm thick U-type GaN layer with a Si doping concentration of 1×10 18 cm -3 The first n-type GaN layer.
[0100] 5b) See Figure 2d , turn off the Si source, keep the flow rates of ammonia and gallium sources unchanged, lower the growth temperature to 850°C, and grow a second C-doped GaN layer with a thickness of 50 nm on the first n-type GaN layer;
[0101] 5c) See Figure 2e , a silicon source with a flow rate of 40 sccm was introduced, the flow rates of ammonia and gallium sources were kept unchanged, the growth temperature was increased to 1050°C, and a 300nm thick Si doping concentration of 1×10 18 cm -3 The third n-type GaN layer.
[0102] Step 6: Please refer to Figure 2f , grow In with a luminescent wavelength of 450nm 0.15 Ga 0.85 N / GaN multiple quantum well structure.
[0103] Under the condition of 40Torr pressure in the reaction chamber, nine periods of In were grown on the third n-type GaN layer using MOCVD process. 0.15 Ga 0.85 N / GaN multiple quantum well structure, where:
[0104] Each cycle of single layer In 0.15 Ga 0.85The thickness of the N-well layer is 2 nm, the growth temperature is 750°C, and during the growth process, the flow rate of the nitrogen source is maintained at 1100 sccm, the flow rate of the gallium source is 50 sccm, and the flow rate of the indium source is 200 sccm;
[0105] The thickness of the single-layer GaN barrier layer in each period is 9 nm, the growth temperature is 850° C., and the flow rate of the nitrogen source is maintained at 2000 sccm and the flow rate of the gallium source is maintained at 150 sccm during the growth process.
[0106] Step 7: Please refer to Figure 2g , grow a p-type GaN layer.
[0107] 7a) Under the condition of a reaction chamber temperature of 1060°C, ammonia with a flow rate of 2500 sccm, a gallium source with a flow rate of 150 sccm and a magnesium source with a flow rate of 100 sccm were introduced simultaneously, and the pressure was maintained at 20 Torr, and an MOCVD process was used in In 0.15 Ga 0.85 The thickness of the N / GaN multi-quantum well structure is 100nm and the Mg doping concentration is 1×10 19 cm -3 p-type GaN layer;
[0108] 7b) Maintain the reaction chamber temperature at 860° C. and anneal for 5 min in a H 2 atmosphere.
[0109] Step 8: Please refer to Figure 2h , etching the n-type electrode contact area.
[0110] A portion of GaN is etched away by using a photolithography process to expose the first n-type GaN layer, and the etching depth is such that the second C-doped GaN layer and a portion of the first n-type GaN layer are etched.
[0111] For step nine, see Figure 2i , depositing electrodes.
[0112] The n-type electrode is deposited on the first n-type GaN layer and the p-type electrode is deposited on the p-type GaN layer by sputtering metal to complete the production of the blue light LED device.
[0113] Embodiment 3
[0114] The present invention further provides a method for preparing a C-doped green LED with a light emission wavelength of 520 nm on the basis of the first embodiment. The method comprises:
[0115] Step 1: Heat treatment.
[0116] After cleaning, the sapphire substrate layer was placed in the MOCVD reaction chamber and the vacuum degree of the reaction chamber was reduced to 2×10 -2Torr; then hydrogen is introduced into the reaction chamber, and when the pressure in the MOCVD reaction chamber reaches 400 Torr, the sapphire substrate layer is heated to a temperature of 1000°C and maintained for 7 minutes to complete the heat treatment of the sapphire substrate layer.
[0117] Step 2: High temperature nitriding.
[0118] The heat-treated sapphire substrate layer was placed in a reaction chamber at a temperature of 1050° C., and ammonia gas was introduced at a flow rate of 3500 sccm for 4 minutes to complete the nitridation.
[0119] Step 3: growing an AlN nucleation layer.
[0120] See also Figure 2a Under the condition of a reaction chamber temperature of 1000°C, an ammonia gas with a flow rate of 3000sccm and an aluminum source with a flow rate of 40sccm were introduced simultaneously, and an AlN nucleation layer with a thickness of 30nm was grown on the nitrided sapphire substrate layer using a MOCVD process.
[0121] Step 4: growing a U-type GaN layer.
[0122] See also Figure 2b Under the condition of a reaction chamber temperature of 950°C, ammonia gas with a flow rate of 2500sccm and a gallium source with a flow rate of 150sccm were introduced simultaneously, and a U-type GaN layer with a thickness of 2.5μm was grown on the AlN nucleation layer by MOCVD process while maintaining a pressure of 20Torr.
[0123] Step 5: Grow a three-layer n-type GaN layer.
[0124] 5a) Please see Figure 2c Under the condition of 1050℃ in the reaction chamber, ammonia with a flow rate of 2500sccm, gallium source with a flow rate of 150sccm and silicon source with a flow rate of 50sccm were introduced at the same time. Under the condition of maintaining the pressure at 20Torr, MOCVD process was used to grow a 1.3μm thick U-type GaN layer with a Si doping concentration of 5×10 18 cm -3 The first n-type GaN layer.
[0125] 5b) See Figure 2d , turn off the Si source, keep the flow rates of ammonia and gallium sources unchanged, lower the growth temperature to 700°C, and grow a second C-doped GaN layer with a thickness of 100 nm on the first n-type GaN layer;
[0126] 5c) See Figure 2e, a silicon source with a flow rate of 50 sccm was introduced, the flow rates of ammonia and gallium sources were kept unchanged, the growth temperature was increased to 1050°C, and a 400nm thick Si doping concentration of 5×10 18 cm -3 The third n-type GaN layer.
[0127] Step 6: Please refer to Figure 2f , grow In with a luminescent wavelength of 520nm 0.32 Ga 0.68 N / GaN multiple quantum well structure.
[0128] Under the condition of 40Torr pressure in the reaction chamber, nine periods of In were grown on the third n-type GaN layer using MOCVD process. 0.32 Ga 0.68 N / GaN multiple quantum well structure, where:
[0129] Each cycle of single layer In 0.32 Ga 0.68 The thickness of the N-well layer is 3 nm, the growth temperature is 750°C, the flow rate of the nitrogen source is maintained at 1100 sccm, the flow rate of the gallium source is 50 sccm, and the flow rate of the indium source is 250 sccm during the growth process;
[0130] The thickness of the single-layer GaN barrier layer in each period is 12 nm, the growth temperature is 850° C., and the flow rate of the nitrogen source is maintained at 2000 sccm and the flow rate of the gallium source is maintained at 150 sccm during the growth process.
[0131] Step 7: Please refer to Figure 2g , grow a p-type GaN layer.
[0132] 7a) Under the condition of a reaction chamber temperature of 1060°C, ammonia with a flow rate of 2500 sccm, a gallium source with a flow rate of 150 sccm, and a magnesium source with a flow rate of 150 sccm were introduced simultaneously, and the pressure was maintained at 20 Torr, and an MOCVD process was used in In 0.32 Ga 0.68 The N / GaN multi-quantum well structure has a growth thickness of 150nm and a Mg doping concentration of 1×10 20 cm -3 p-type GaN layer;
[0133] 7b) Maintain the reaction chamber temperature at 900° C. and anneal for 8 min in a H 2 atmosphere.
[0134] Step 8. Please refer to Figure 2h , etching the n-type electrode contact area.
[0135] A portion of GaN is etched away by using a photolithography process to expose the first n-type GaN layer, and the etching depth is such that the second C-doped GaN layer and a portion of the first n-type GaN layer are etched.
[0136] For step nine, see Figure 2i , depositing electrodes.
[0137] The n-type electrode is deposited on the first n-type GaN layer and the p-type electrode is deposited on the p-type GaN layer by sputtering metal to complete the production of the green light LED device.
[0138] Embodiment 4
[0139] The present invention further provides a method for preparing a C-doped yellow LED with a light emission wavelength of 600 nm on the basis of the first embodiment. The method comprises:
[0140] Step 1: Heat treatment.
[0141] After cleaning, the sapphire substrate layer was placed in the MOCVD reaction chamber and the vacuum degree of the reaction chamber was reduced to 2×10 -2 Torr; then hydrogen is introduced into the reaction chamber, and when the pressure in the MOCVD reaction chamber reaches 760 Torr, the sapphire substrate layer is heated to a temperature of 1200°C and maintained for 10 minutes to complete the heat treatment of the sapphire substrate layer.
[0142] Step 2: High temperature nitriding.
[0143] The heat-treated sapphire substrate layer was placed in a reaction chamber at a temperature of 1100° C., and ammonia gas with a flow rate of 4000 sccm was introduced for 5 minutes to perform nitridation to complete the nitridation.
[0144] Step 3: growing an AlN nucleation layer.
[0145] See also Figure 2a Under the condition of a reaction chamber temperature of 1000°C, ammonia gas with a flow rate of 3000sccm and an aluminum source with a flow rate of 40sccm were introduced simultaneously, and an AlN nucleation layer with a thickness of 50nm was grown on the nitrided sapphire substrate layer using a MOCVD process.
[0146] Step 4: growing a U-type GaN layer.
[0147] See also Figure 2b Under the condition of a reaction chamber temperature of 950°C, ammonia gas with a flow rate of 2500sccm and a gallium source with a flow rate of 150sccm were introduced simultaneously, and a U-type GaN layer with a thickness of 3μm was grown on the AlN nucleation layer by MOCVD process while maintaining the pressure at 20Torr.
[0148] Step 5: Grow a three-layer n-type GaN layer.
[0149] 5a) Please see Figure 2c Under the condition of 1050℃ in the reaction chamber, ammonia with a flow rate of 2500sccm, gallium source with a flow rate of 150sccm and silicon source with a flow rate of 60sccm were introduced at the same time. Under the condition of maintaining the pressure at 20Torr, MOCVD process was used to grow a U-type GaN layer with a thickness of 1.5μm and a Si doping concentration of 1×10 19 cm -3 The first n-type GaN layer.
[0150] 5b) See Figure 2d , turn off the Si source, keep the flow rates of ammonia and gallium sources unchanged, lower the growth temperature to 600°C, and grow a second C-doped GaN layer with a thickness of 200 nm on the first n-type GaN layer;
[0151] 5c) See Figure 2e , a silicon source with a flow rate of 60 sccm was introduced, the flow rates of ammonia and gallium sources were kept unchanged, the growth temperature was increased to 1050°C, and a 500nm thick Si doping concentration of 1×10 19 cm -3 The third n-type GaN layer.
[0152] Step 6: Please refer to Figure 2f , grow In with a luminescent wavelength of 600nm 0.4 Ga 0.6 N / GaN multiple quantum well structure.
[0153] Under the condition of 40Torr pressure in the reaction chamber, nine periods of In were grown on the third n-type GaN layer using MOCVD process. 0.4 Ga 0.6 N / GaN multiple quantum well structure, where:
[0154] Each cycle of single layer In 0.4 Ga 0.6 The thickness of the N-well layer is 5 nm, the growth temperature is 750°C, and during the growth process, the flow rate of the nitrogen source is maintained at 1100 sccm, the flow rate of the gallium source is 50 sccm, and the flow rate of the indium source is 300 sccm;
[0155] The thickness of the single-layer GaN barrier layer in each period is 15 nm, the growth temperature is 850° C., and the flow rate of the nitrogen source is maintained at 2000 sccm and the flow rate of the gallium source is maintained at 150 sccm during the growth process.
[0156] Step 7: Please refer to Figure 2g , grow a p-type GaN layer.
[0157] 7a) Under the condition of a reaction chamber temperature of 1060°C, ammonia with a flow rate of 2500 sccm, a gallium source with a flow rate of 150 sccm and a magnesium source with a flow rate of 300 sccm were introduced simultaneously, and the pressure was maintained at 20 Torr, and an MOCVD process was used in In 0.4 Ga 0.6 The thickness of the N / GaN multi-quantum well structure is 200nm and the Mg doping concentration is 1×10 22 cm -3 p-type GaN layer;
[0158] 7b) Maintain the reaction chamber temperature at 1100° C. and anneal for 10 min in a H 2 atmosphere.
[0159] Step 8: Please refer to Figure 2h , etching the n-type electrode contact area.
[0160] A portion of GaN is etched away by using a photolithography process to expose the first n-type GaN layer, and the etching depth is such that the second C-doped GaN layer and a portion of the first n-type GaN layer are etched.
[0161] For step nine, see Figure 2i , depositing electrodes.
[0162] The n-type electrode is deposited on the first n-type GaN layer and the p-type electrode is deposited on the p-type GaN layer by sputtering metal to complete the manufacture of the yellow light LED device.
[0163] Embodiment 5
[0164] See also Figure 3 , Figure 3 A schematic diagram of the structure of a GaN-based light-emitting diode based on a C-doped current spreading layer provided in an embodiment of the present invention. Based on the above embodiment, the present invention further provides a GaN-based light-emitting diode based on a C-doped current spreading layer, the GaN-based light-emitting diode comprising:
[0165] Sapphire substrate layer;
[0166] An AlN nucleation layer, located on a sapphire substrate layer;
[0167] U-type GaN layer, located on the AlN nucleation layer;
[0168] A first n-type GaN layer is located on the U-type GaN layer, and the first n-type GaN layer has a first upper surface and a second upper surface, and the second upper surface is located below the first upper surface;
[0169] A second C-doped GaN layer is located on a first upper surface of the first n-type GaN layer;
[0170] A third n-type GaN layer is located on the second C-doped GaN layer;
[0171] The multi-quantum well structure is located on the third n-type GaN layer. The multi-quantum well structure includes several periods of quantum wells, including In x Ga 1-x The N well layer and the In x Ga 1-x A GaN barrier layer on the N-well layer;
[0172] A p-type GaN layer located on a multi-quantum well structure;
[0173] An n-type electrode is located on the second upper surface of the first n-type GaN layer;
[0174] The p-type electrode is located on the p-type GaN layer.
[0175] Preferably, the thickness of the AlN nucleation layer is in the range of 20-50 nm.
[0176] Preferably, the thickness of the U-type GaN layer is in the range of 2-3 μm.
[0177] Preferably, the thickness of the first n-type GaN layer is in the range of 1-1.5 μm, and the Si doping concentration is 10 18 -10 19 cm -3 The thickness of the second C-doped GaN layer is in the range of 50-200nm, the thickness of the third n-type GaN layer is in the range of 300-500nm, and the Si doping concentration is 10 18 -10 19 cm -3 .
[0178] Preferably, the multi-quantum well structure includes nine periods of quantum wells, each period of quantum wells including In x Ga 1- x The N well layer and the In x Ga 1-x GaN barrier layer on the N well layer, In x Ga 1-x The thickness of the N-well layer and the GaN barrier layer ranges from 2-5 nm and 9-15 nm, respectively.
[0179] Preferably, In x Ga 1-x The adjustment range of the In content parameter x in the N well layer is 0.1-0.7. Quantum wells with different In contents can produce LEDs with different emission wavelengths.
[0180] Preferably, the thickness of the p-type GaN layer is in the range of 100-200 nm.
[0181] In the description of the present invention, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0182] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or special data points described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or special data points described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.
[0183] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.
Claims
1. A method for preparing a GaN-based light-emitting diode based on a C-doped current spreading layer, characterized in that: The preparation method of the GaN-based light-emitting diode comprises: Selecting a sapphire substrate layer; growing an AlN nucleation layer on the sapphire substrate layer; growing a U-type GaN layer on the AlN nucleation layer; growing a first n-type GaN layer on the U-type GaN layer; growing a second C-doped GaN layer on the first n-type GaN layer; growing a third n-type GaN layer on the second C-doped GaN layer, wherein the first n-type GaN layer, the second C-doped GaN layer and the third n-type GaN layer constitute a three-layer structure of n-type GaN layers; A multi-quantum well structure is grown on the third n-type GaN layer, wherein the multi-quantum well structure includes quantum wells of several periods, wherein the quantum wells include In x Ga 1-x The N well layer and the In x Ga 1-x A GaN barrier layer on the N-well layer; Growing a p-type GaN layer on the multi-quantum well structure; Etching the n-type electrode contact region to expose the first n-type GaN layer; An n-type electrode is deposited on the first n-type GaN layer in the n-type electrode contact region and a p-type electrode is deposited on the p-type GaN layer to complete the production of a GaN-based light-emitting diode, wherein: Growing a first n-type GaN layer on the U-type GaN layer, comprising: introducing ammonia, a gallium source and a silicon source, and growing the first n-type GaN layer on the U-type GaN layer by using an MOCVD process under a first temperature condition; Growing a second C-doped GaN layer on the first n-type GaN layer, comprising: Turn off the silicon source, keep the flow rates of ammonia and gallium source unchanged, and grow a second C-doped GaN layer on the first n-type GaN layer by MOCVD process under a second temperature condition, wherein the second temperature is lower than the first temperature; Growing a third n-type GaN layer on the second C-doped GaN layer, comprising: A silicon source is introduced, the flow rates of ammonia and gallium source are kept unchanged, and a third n-type GaN layer is grown on the second C-doped GaN layer by using an MOCVD process under a first temperature condition.
2. The method for preparing a GaN-based light-emitting diode according to claim 1, characterized in that: Select the sapphire substrate layer, including: Cleaning the sapphire substrate layer; The sapphire substrate layer is heat treated at a temperature of 900-1200° C. for 5-10 minutes; The sapphire substrate layer after heat treatment is subjected to nitridation treatment for 3-5 minutes under the temperature condition of 1000-1100°C.
3. The method for preparing a GaN-based light-emitting diode according to claim 2, characterized in that: Growing an AlN nucleation layer on the sapphire substrate layer, comprising: An AlN nucleation layer with a thickness of 20-50 nm is grown on the nitrided sapphire substrate layer using a MOCVD process.
4. The method for preparing a GaN-based light-emitting diode according to claim 1, characterized in that: Growing a U-type GaN layer on the AlN nucleation layer, comprising: A U-type GaN layer with a thickness of 2-3 μm is grown on the AlN nucleation layer by using a MOCVD process.
5. The method for preparing a GaN-based light-emitting diode according to claim 1, characterized in that: Single layer of In x Ga 1-x The thickness of the N well layer is 2-5 nm, and the thickness of the single-layer GaN barrier layer is 9-15 nm, wherein the adjustment range of the In content x is 0.1-0.
7.
6. The method for preparing a GaN-based light-emitting diode according to claim 1, characterized in that: Etching the n-type electrode contact region to expose the first n-type GaN layer, including: The p-type GaN layer, the multi-quantum well structure, the third n-type GaN layer, the second C-doped GaN layer and a portion of the first n-type GaN layer at one end are etched away by a photolithography process to expose the remaining first n-type GaN layer.
7. A GaN-based light-emitting diode based on a C-doped current spreading layer, characterized in that: The GaN-based light-emitting diode is prepared by the method for preparing the GaN-based light-emitting diode according to any one of claims 1 to 6, wherein the GaN-based light-emitting diode comprises: Sapphire substrate layer; An AlN nucleation layer is located on the sapphire substrate layer; A U-type GaN layer, located on the AlN nucleation layer; A first n-type GaN layer is located on the U-type GaN layer, and the first n-type GaN layer has a first upper surface and a second upper surface, and the second upper surface is located below the first upper surface; A second C-doped GaN layer is located on a first upper surface of the first n-type GaN layer; A third n-type GaN layer, located on the second C-doped GaN layer; A multi-quantum well structure is located on the third n-type GaN layer, wherein the multi-quantum well structure includes a plurality of periodic quantum wells, wherein the quantum wells include In x Ga 1-x The N well layer and the In x Ga 1-x A GaN barrier layer on the N-well layer; A p-type GaN layer, located on the multi-quantum well structure; An n-type electrode is located on the second upper surface of the first n-type GaN layer; The p-type electrode is located on the p-type GaN layer.
Citation Information
Patent Citations
GaN-based lateral structure light emitting diode based on Fe doping and preparation method thereof
CN111987198A
Nitride semiconductor light emitting device
KR100738399B1